A water-based carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode and its preparation method and application

By using a specific component of water-based carboxyl-terminated nitrile rubber binder in lithium-ion batteries, the problems of poor flexibility and safety hazards of the binders in lithium-ion batteries are solved, and battery performance improvements with high toughness and low cost are achieved.

CN118516071BActive Publication Date: 2024-10-29ZHEJIANG CASNOVO MATERIALS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410986345.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-29
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing water-based binders in lithium-ion batteries have shortcomings such as poor flexibility and high rigidity, making it difficult to meet the requirements of new production processes. In addition, traditional organic solvent-based binders have safety hazards and high costs.

Method used

A water-based carboxyl-terminated nitrile rubber binder is used for the lithium iron phosphate cathode, and a specific proportion of carboxyl-terminated nitrile rubber, (meth)acrylic acid, N-(3-aminopropyl)methacrylamide, acrylonitrile and non- The combination of polar monomers and other components forms a stable emulsion, increases the toughness of the binder and increases the solid content. It is prepared by reaction with additives such as catalysts and surfactants.

Benefits of technology

The toughness and bonding strength of the binder are significantly improved. The battery's capacity retention rate is still over 85% after 6,000 cycles, and it is safe, environmentally friendly and low-cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516071B_ABST
    Figure CN118516071B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of battery binders, and more specifically, to a water-based carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, and a preparation method and application thereof. In parts by weight, the raw materials for preparation include: 5-10% carboxyl-terminated nitrile rubber, 15-35% (methyl) acrylic acid, 15-35% N-(3-aminopropyl) methacrylamide, 15-40% acrylonitrile, and 5-20% non-polar monomer. The final product has no VOC residue and is an environmentally friendly, non-toxic, pure green water-based binder; the binder of the present invention has a toughness that is enhanced by more than 2 times, and exhibits better bonding strength; the prepared battery, after 6000 cycles, still has a capacity retention rate of more than 85%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery binders, and more specifically to an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrodes, and a preparation method and application thereof. Background Art

[0002] In the production process of lithium-ion batteries, the binder plays a role in bonding the various substances in the slurry and the slurry to the current collector. It can not only stabilize the pole piece structure, but also affect the internal resistance between the active material and the current collector. Therefore, the performance of the binder not only plays a key role in the mechanical properties of the pole piece, but also affects the electrochemical properties of the lithium-ion battery. At present, organic solvent polyvinylidene fluoride (PVDF) is generally used as a binder, and organic solvent N-methylpyrrolidone (NMP) is used as a dispersant. PVDF has good bonding properties, but its electronic and ionic conductivity is poor; organic solvent NMP has good dispersibility, but it is volatile, flammable, explosive, and highly toxic. The pole piece coating process using PVDF as a binder requires sealing and has high production costs. On the other hand, because PVDF contains fluorine, it is easy to react with lithium-intercalated graphite, etc., resulting in a decrease in the performance of lithium-ion batteries. Water-based binders have no solvent release, are green and environmentally friendly, low cost, non-combustible, and highly safe, and have become an urgent development direction for the current lithium-ion battery binder industry.

[0003] Wang Xinxin, Liu Jian, Gong Zhengliang, et al. Application of carboxymethyl cellulose-styrene butadiene rubber composite binder in silicon-based lithium-ion batteries. Journal of Xiamen University (Natural Science Edition), 2018, 57 (4): 471-476. A mixed system of carboxymethyl cellulose (CMC) and styrene butadiene rubber (SBR) as an aqueous negative electrode binder is disclosed, which not only requires the use of two components, but also has a high cost. At the same time, it still relies on existing petrochemical products. At present, aqueous binders used in lithium-ion batteries generally have the disadvantages of poor flexibility and high rigidity. It is urgent to propose a new solution to increase the toughness of the binder to meet the requirements of the new production process. Summary of the invention

[0004] The first aspect of the present invention provides an aqueous carboxyl-terminated nitrile rubber binder for a lithium iron phosphate positive electrode. The preparation raw materials include, by weight percentage: 5-10% carboxyl-terminated nitrile rubber, 15-35% (methyl) acrylic acid, 15-35% N-(3-aminopropyl) methacrylamide, 15-40% acrylonitrile and 5-20% non-polar monomer.

[0005] Preferably, the raw materials include, by weight percentage: 5-10% carboxyl-terminated nitrile rubber, 25-35% (methyl) acrylic acid, 20-35% N-(3-aminopropyl) methacrylamide, 25-40% acrylonitrile and 5-10% non-polar monomer.

[0006] Further preferably, the raw materials for preparation include, by weight percentage: 5-10% carboxyl-terminated nitrile rubber, 30-35% (methyl) acrylic acid, 25-30% N-(3-aminopropyl) methacrylamide, 25-30% acrylonitrile and 5-10% non-polar monomer.

[0007] The raw materials for preparing the binder also include: a catalyst, a non-ionic surfactant, an initiator, an alkali solution and deionized water.

[0008] The non-polar monomer includes at least one of butyl acrylate, isooctyl acrylate, styrene and vinyl acetate.

[0009] The carboxyl-terminated nitrile rubber has a weight average molecular weight of 80,000-150,000, an average viscosity of 8,000-12,000 mPa·s at 40° C., a carboxyl content of 1-5wt%, and an acrylonitrile content of 25-40wt%.

[0010] Preferably, the molecular weight of the carboxyl-terminated nitrile rubber is 80,000-120,000, the average viscosity at 40° C. is 9,000-11,000 mPa·s, the carboxyl content is 1-3wt%, and the acrylonitrile content is 30-34wt%.

[0011] The catalyst comprises one of 1,8-diazabicyclo[5.4.0]undec-7-ene, tetramethyldipropylenetriamine and 4-dimethylaminopyridine.

[0012] Preferably, the catalyst comprises 4-dimethylaminopyridine.

[0013] Preferably, the added amount of the catalyst is 0.1-3% of the mass fraction of the carboxyl-terminated nitrile rubber.

[0014] Preferably, the added amount of the catalyst is 0.5-2% of the mass fraction of the carboxyl-terminated nitrile rubber.

[0015] The nonionic surfactant includes at least one of TX series, NP series and OP series surfactants.

[0016] Preferably, the nonionic surfactant includes NP series surfactants.

[0017] Preferably, the addition amount of the nonionic surfactant is 1-5% of the mass fraction of the carboxyl-terminated nitrile rubber.

[0018] The present application found that the molecular weight of the carboxyl-terminated nitrile rubber is 80,000-150,000, the average viscosity at 40°C is 8,000-12,000 mPa·s, the carboxyl content is 1-5wt%, and the acrylonitrile content is 25-40wt%. A stable emulsion can be formed in a multiphase. In addition, the longer soft organic side chain is conducive to improving the flexibility of the composite macromolecule and providing the core structure corresponding to the functional polymer core-shell structure model ( Figure 2 ). Further research has found that controlling the mass proportion of the carboxyl-terminated nitrile rubber (CTBN) in the water-based binder system to 5%-10% can further increase the number of initial nuclei in the seed emulsion while ensuring good water solubility of the water-based binder, provide sufficient sites for polymerization reaction, further improve the conversion rate of synthesis, and increase the solid content of the water-based binder.

[0019] The second aspect of the present invention provides a method for preparing an aqueous carboxyl-terminated nitrile rubber binder for a lithium iron phosphate positive electrode, comprising the following steps:

[0020] S1, mixing carboxyl-terminated nitrile rubber, N-(3-aminopropyl) methacrylamide, acrylonitrile, a catalyst and a nonionic surfactant in water to obtain a seed emulsion;

[0021] S2, adding alkali solution to (meth)acrylic acid to obtain a (meth)acrylate solution;

[0022] S3, adding the (meth)acrylate solution and the non-polar monomer to the seed emulsion in sequence, and stirring evenly to obtain an emulsion for reaction;

[0023] S4, under an inert gas atmosphere, dripping the initiator into the reaction emulsion for reaction, cooling, sequentially removing the monomer, adding water to dilute, filtering, and obtaining.

[0024] The inert gas includes one of nitrogen, helium, neon, argon, krypton, and xenon.

[0025] The reaction time in step S1 is 2-6 hours, and the reaction temperature is 40-80°C.

[0026] Preferably, the reaction time in step S1 is 2-4 hours, and the reaction temperature is 40-60°C.

[0027] The reaction time in step S4 is 6-12 hours, and the reaction temperature is 60-90°C.

[0028] Preferably, the reaction time in step S4 is 8-12 hours, and the reaction temperature is 70-90°C.

[0029] The third aspect of the present invention provides an application of an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which is applied to the positive electrode plate of a lithium iron phosphate battery.

[0030] Preferably, the amount of the binder added to the positive electrode plate is 1-5wt%.

[0031] Preferably, the amount of the binder added to the positive electrode plate is 2-3wt%.

[0032] Beneficial effects:

[0033] 1. The molecular weight of the carboxyl-terminated nitrile rubber is 80,000-150,000, the average viscosity at 40°C is 8,000-12,000 mPa·s, the carboxyl content is 1-5wt%, and the acrylonitrile content is 25-40wt%. A stable emulsion can be formed in multiple phases, which is conducive to the formation of seed emulsion.

[0034] 2. The mass proportion of the carboxyl-terminated nitrile rubber (CTBN) in the aqueous binder system is controlled to be 5%-10%. This can further increase the number of initial nuclei in the seed emulsion while ensuring good water solubility of the aqueous binder, provide sufficient sites for polymerization reactions, further improve the conversion rate of the synthesis, and increase the solid content of the aqueous binder.

[0035] 3. The 4-dimethylaminopyridine is an effective catalyst for the acrylation reaction between the amino group in N-(3-aminopropyl)methacrylamide and the carboxyl group in the carboxyl-terminated nitrile rubber. The feed amount is limited to 0.1-3% of the weight of the hydroxy-terminated nitrile rubber, which can effectively improve the reaction efficiency between the amino group in N-(3-aminopropyl)methacrylamide and the carboxyl group in the carboxyl-terminated nitrile rubber, thereby improving the mechanical properties of the adhesive.

[0036] 4. Utilizing the water / oil biphasic solubility of acrylonitrile monomer, it has good bidirectional solubility for oily monomers and polar monomers, and has the dual functions of reactant and solvent, and can form a stable emulsion in the water phase, thereby carrying out water phase emulsion polymerization.

[0037] 5. The reaction time in step S4 is 6-12 hours, the reaction temperature is 60-90°C, and the aqueous binder has a viscosity within the range of 11.0-18.0 Pa•s at 40°C, a solid content of 10.0wt% and a pH value of 6.0-8.0.

[0038] 6. Compared with the binder, the toughness of the adhesive prepared in the present application is more than 2 times stronger and exhibits better bonding strength. After 6000 cycles, the capacity retention rate of the prepared battery is still above 85%. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1This is the synthetic chemical formula of the binder of Example 1.

[0040] Figure 2 Schematic diagram of a core-shell structured polymer composite water-based binder system.

[0041] Figure 3 This is a scanning electron microscope (SEM) image of the binder of Example 8.

[0042] Figure 4 This is the battery cycle performance test of Example 8 and Comparative Example 1, wherein the blue fitting line corresponds to Comparative Example 1, and the black fitting line corresponds to Example 8.

[0043] Figure 5 The low-temperature discharge performance of the batteries of Example 8 and Comparative Example 1, wherein the red fitting line corresponds to Comparative Example 1, and the black fitting line corresponds to Example 8. DETAILED DESCRIPTION

[0044] Example 1

[0045] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass ratio: 5% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 15% N-(3-aminopropyl) methacrylamide; 40% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0046] The present embodiment provides a method for preparing a polymer composite aqueous binder system having a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN), such as Figure 1As shown, the following steps are as follows: carboxyl-terminated nitrile rubber (5% of the total mass fraction), N-(3-aminopropyl)methacrylamide (15% of the total mass fraction), acrylonitrile (40% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of carboxyl-terminated nitrile rubber) are mixed in water, stirred vigorously (300 rpm) for 30 minutes, and then heated to 50°C to allow the amino groups in N-(3-aminopropyl)methacrylamide and the carboxyl groups in the carboxyl-terminated nitrile rubber to fully react for 3 hours to prepare a partially acryloyl-terminated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature; an aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 12.2Pa•s (adjusting the solid content by diluting with water).

[0047] Example 2

[0048] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass ratio: 5% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 20% N-(3-aminopropyl) methacrylamide; 35% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0049] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (5% of the total mass fraction), N-(3-aminopropyl) methacrylamide (20% of the total mass fraction), acrylonitrile (35% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; helium was introduced for 30 minutes to remove oxygen in the reaction system, the stirring speed was reduced (100 rpm), and after the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, the temperature was controlled at 70°C, and the mixture was stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 13.3Pa•s (solid content was adjusted by diluting with water).

[0050] Example 3

[0051] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass percentage: 5% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 25% N-(3-aminopropyl) methacrylamide; 30% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0052] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (5% of the total mass fraction), N-(3-aminopropyl) methacrylamide (25% of the total mass fraction), acrylonitrile (30% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 80°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 14.1Pa•s (adjusting the solid content by diluting with water).

[0053] Example 4

[0054] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass percentage: 5% carboxyl-terminated nitrile rubber; 30% (methyl) acrylic acid; 30% N-(3-aminopropyl) methacrylamide; 30% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0055] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (5% of the total mass fraction), N-(3-aminopropyl) methacrylamide (30% of the total mass fraction), acrylonitrile (30% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acryloyl-terminated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, and cool to room temperature; add an aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) to (meth)acrylic acid (30% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through acid-base neutralization reaction, and cool to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; argon was introduced for 30 minutes to remove oxygen in the reaction system, the stirring speed was reduced (100 rpm), and after the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, the temperature was controlled at 90°C, and the mixture was stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 14.1Pa•s (adjusting the solid content by diluting with water).

[0056] Example 5

[0057] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass ratio: 5% carboxyl-terminated nitrile rubber; 25% (methyl) acrylic acid; 35% N-(3-aminopropyl) methacrylamide; 30% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0058] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (5% of the total mass fraction), N-(3-aminopropyl) methacrylamide (35% of the total mass fraction), acrylonitrile (30% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acryloyl-terminated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, and cool to room temperature; add an aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) to (meth)acrylic acid (25% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through acid-base neutralization reaction, and cool to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 14.7Pa•s (adjusting the solid content by diluting with water).

[0059] Example 6

[0060] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass ratio: 10% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 15% N-(3-aminopropyl) methacrylamide; 35% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0061] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (10% of the total mass fraction), N-(3-aminopropyl) methacrylamide (15% of the total mass fraction), acrylonitrile (35% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 15.5Pa•s (adjusting the solid content by diluting with water).

[0062] Example 7

[0063] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass percentage: 10% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 20% N-(3-aminopropyl) methacrylamide; 30% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0064] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (10% of the total mass fraction), N-(3-aminopropyl) methacrylamide (20% of the total mass fraction), acrylonitrile (30% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 16.1Pa•s (adjusting the solid content by diluting with water).

[0065] Example 8

[0066] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass ratio: 10% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 25% N-(3-aminopropyl) methacrylamide; 25% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0067] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (10% of the total mass fraction), N-(3-aminopropyl) methacrylamide (25% of the total mass fraction), acrylonitrile (25% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (methyl) acrylic acid solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, viscosity of 17.1Pa•s (solid content was adjusted by diluting with water), and the scanning electron microscope image of the binder is shown in the figure below. Figure 3 shown.

[0068] Example 9

[0069] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass percentage: 10% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 30% N-(3-aminopropyl) methacrylamide; 20% acrylonitrile; and 5% butyl acrylate (non-polar monomer).

[0070] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (10% of the total mass fraction), N-(3-aminopropyl) methacrylamide (30% of the total mass fraction), acrylonitrile (20% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 16.9Pa•s (adjusting the solid content by diluting with water).

[0071] Example 10

[0072] The present embodiment provides an aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, which includes the following components in terms of mass proportion: 10% carboxyl-terminated nitrile rubber; 35% (methyl) acrylic acid; 35% N-(3-aminopropyl) methacrylamide; 15% acrylonitrile; and 5% butyl acrylate.

[0073] The preparation method of the polymer composite water-based binder system with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN) provided in this embodiment comprises the following steps: carboxyl-terminated nitrile rubber (10% of the total mass fraction), N-(3-aminopropyl) methacrylamide (35% of the total mass fraction), acrylonitrile (15% of the total mass fraction), 4-dimethylaminopyridine (1% of the mass fraction of the carboxyl-terminated nitrile rubber) and a non-ionic surfactant (NP10, 2% of the mass fraction of the carboxyl-terminated nitrile rubber) are mixed in water. After mixing and vigorously stirring (300 rpm) for 30 minutes, heat to 50°C to allow the amino group in N-(3-aminopropyl)methacrylamide to fully react with the carboxyl group in the carboxyl-terminated nitrile rubber for 3 hours to prepare a partially acrylated carboxyl-terminated nitrile rubber (CTBN) seed emulsion, which is then cooled to room temperature. An aqueous solution of sodium hydroxide (46.4% of the mass fraction of methacrylic acid) is added to (meth)acrylic acid (35% of the total mass fraction) to prepare a sodium (meth)acrylic acid salt solution through an acid-base neutralization reaction, which is then cooled to room temperature for use. To the prepared acryloyl-terminated carboxyl-butadiene nitrile rubber (CTBN) seed emulsion solution, sodium (meth) acrylic acid salt solution and butyl acrylate were added in sequence, and the mixture was stirred vigorously (300 rpm) for 30 minutes to prepare an emulsion for reaction; nitrogen was introduced for 30 minutes to remove oxygen in the reaction system, and the stirring speed was reduced (100 rpm). After the temperature was raised to 60°C, an initiator (ammonium persulfate aqueous solution) was gradually added dropwise, and the temperature was controlled at 60°C and stirred for 12 hours; after cooling to room temperature, the mixture was stripped, diluted with water, and filtered to obtain a polymer composite water-based binder with a core-shell structure based on carboxyl-terminated nitrile rubber (CTBN). The specific parameters are: white latex, 10.0wt% solid content at 40°C, pH value of 7.1, and viscosity of 17.2Pa•s (adjusting the solid content by diluting with water).

[0074] Comparative Example 1

[0075] In this comparative example, methacrylic acid (45% of the total mass fraction), N-(3-aminopropyl)methacrylamide (15% of the total mass fraction), acrylonitrile (20% of the total mass fraction) and butyl acrylate (20% of the total mass fraction) were copolymerized in an aqueous phase to prepare an aqueous binder for lithium-ion batteries.

[0076] The preparation method is as follows: methacrylic acid (45% of the total mass fraction) and sodium hydroxide (11.6% of the mass fraction of methacrylic acid) are added to deionized water, and the neutralization reaction is completed and the solution is cooled to room temperature; then N-(3-aminopropyl) methacrylamide (15% of the total mass fraction), acrylonitrile (20% of the total mass fraction), butyl acrylate (20% of the total mass fraction) and surfactant (NP14, 2% of the mass fraction of butyl acrylate) are added in sequence, and the mixture is stirred vigorously (300 rpm) for 30 minutes to prepare a reaction emulsion; nitrogen is introduced for 30 minutes to remove oxygen in the reaction system, the stirring speed is reduced (100 rpm), and after the temperature is raised to 60°C, an initiator (ammonium persulfate aqueous solution, 0.1% of the monomer mass fraction) is gradually dripped in, the temperature is controlled at 60°C, and the mixture is stirred for 12 hours; after cooling to room temperature, the monomer is removed, water is added for dilution, and filtration is performed to obtain a novel aqueous binder for lithium-ion batteries. Its specific parameters are: white latex, 15.0% solid content at 40°C, pH value of 6.8, and viscosity of 16.1 Pa•s.

[0077] The percentages mentioned are all by mass.

[0078] Performance Testing Methods

[0079] 1. Elongation at break test

[0080] The tensile test specimens of the adhesive film were prepared according to ASTM standard D638, and 5 samples were required for each selected strain rate. The tensile test was carried out under constant temperature and humidity conditions, specifically 25°C and 40%RH. The test results are shown in Table 1.

[0081] 2. 180° peel force test

[0082] The binders of the above embodiments and comparative examples were used to prepare negative electrode sheets (formula: 93% lithium iron phosphate, 4% conductive carbon black and 3% binder), and their 180° peeling strength was measured. The positive electrode sheet adhesion test was carried out according to the ASTM~D3330 test method, equipment and tools: YISIDA mechanical tester (DS2-50N); 3M tape: (Scotch 600 / 20mm width), and the test results are shown in Table 1.

[0083] 3. Battery performance test

[0084] The battery was prepared by using the binder of the embodiment and comparative example of the present invention, and its performance was measured. The positive electrode sheet, battery assembly, electrolyte and processing flow were all completed by standard preparation methods and processes (ASTM~D3330).

[0085] Among them, the preparation of the positive electrode

[0086] The binders of the above-mentioned embodiments and comparative examples were used to prepare positive electrode sheets, and their 180° peeling force was measured. The specific method and results are as follows: a lithium iron phosphate compound (Hunan Yuneng, 93wt%) used as a positive electrode active material, carbon black (super-p, 4wt%) used as a conductive material, and a binder (3wt%) were added to deionized water to prepare a positive electrode mixture slurry. The positive electrode mixture slurry was coated on an aluminum (Al) foil collector with a thickness of 12 microns, dried, and rolled to form a positive electrode sheet with a surface density of 39mg / cm2 and a compaction density of 2.2g / cm3.

[0087] Preparation of negative electrode

[0088] Artificial graphite (a product of Shanshan Co., Ltd., 94wt%), binder (Zhejiang Zhongke Lide New Materials Co., Ltd. negative electrode binder NV-1T-N, 4wt%), and conductive carbon black (super-p, 2wt%) used as negative electrode active materials were added to deionized water in proportion, and negative electrode mixture slurry was prepared by wet process. The negative electrode mixture slurry was coated on a 6-micron thick copper (Cu) foil collector, and then dried and rolled. The surface density was 20mg / cm2 and the compaction density was 1.70g / cm3.

[0089] Battery winding and electrolyte injection

[0090] The above-prepared electrode is used to prepare a battery with a specification of 406379. The battery is made by winding the positive electrode, the separator and the negative electrode, and the battery is packaged using an aluminum-plastic composite. An electrolyte (ethylene carbonate (EC) / ethyl methyl carbonate (EMC) = 1 / 2 (volume ratio)) of lithium hexafluorophosphate (LiPF6) with a concentration of 1 mol / L is injected into the assembled battery, and vacuum sealing is performed to obtain a battery ready to enter an activated state.

[0091] Battery Formation

[0092] After the above-obtained battery cell is placed in a 45°C environment and allowed to stand for 20 hours, it is shaped by hot pressing at 95°C for 1 minute. The battery cell is placed directly on the formation equipment without clamping and pressing, and the battery cell is formed in a 30±2°C environment. The formation current is 1C, the formation time is 100 minutes, and the formation cut-off potential is 4.35V. Then it is placed in a charge and discharge tester for charge / discharge / charge cycles in sequence, with a cut-off potential of 3.8V, and then the battery cell is degassed and the air bag is cut off to obtain a battery. In this process, only 8 minutes of hot and cold pressing are required, and no other clamps are required to clamp and form each battery. The entire formation time is 270 minutes.

[0093] Cycle performance

[0094] The battery was charged to 4.35V at a current rate of 1C and kept at a constant voltage of 4.35V; then the battery was discharged at a current rate of 1C, with a cut-off voltage of 3.0V, completing one cycle. The results are shown in Table 2 and Figure 4 .from Figure 4 It can be seen that the product of Example 8 of the present invention has good cycle performance.

[0095] Low temperature discharge test

[0096] At room temperature, charge the battery to 4.35V at a current rate of 0.2C and keep the voltage at 4.35V. Then place the battery at the set temperature for 16 hours and discharge at a current rate of 1.0C at the corresponding temperature. The cut-off voltage is 2.5V. For details, see Figure 5 and Table 2. It can be clearly seen from the above battery performance test results that the battery prepared by using the binder of Example 8 of the present invention has better performance.

[0097] Performance test data

[0098] Table 1

[0099]

[0100] Table 2

[0101]

Claims

1. A water-based carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode, characterized in that: The raw materials include, by weight percentage: 5-10% of carboxyl-terminated nitrile rubber, 15-35% of (methyl) acrylic acid, 15-35% of N-(3-aminopropyl) methacrylamide, 15-40% of acrylonitrile and 5-20% of at least one monomer selected from butyl acrylate and isooctyl acrylate; The raw materials for preparing the binder also include: a catalyst, a nonionic surfactant, an initiator, an alkali solution and deionized water; The preparation method is as follows: S1, mixing carboxyl-terminated nitrile rubber, N-(3-aminopropyl) methacrylamide, acrylonitrile, a catalyst and a nonionic surfactant in water to obtain a seed emulsion; S2, adding alkali solution to (meth)acrylic acid to obtain a (meth)acrylate solution; S3, adding a (meth)acrylate solution, at least one monomer selected from butyl acrylate and isooctyl acrylate to the seed emulsion in sequence, and stirring evenly to obtain an emulsion for reaction; S4, under an inert gas atmosphere, dripping the initiator into the reaction emulsion for reaction, cooling, sequentially removing the monomer, adding water to dilute, filtering, and obtaining.

2. The aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to claim 1, characterized in that: The carboxyl-terminated nitrile rubber has a weight average molecular weight of 80,000-150,000, an average viscosity of 8,000-12,000 mPa·s at 40° C., a carboxyl content of 1-5wt%, and an acrylonitrile content of 25-40wt%.

3. The aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to claim 2, characterized in that: The catalyst includes one of 1,8-diazabicyclo[5.4.0]undec-7-ene, tetramethyldipropylenetriamine and 4-dimethylaminopyridine.

4. The aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to claim 3, characterized in that: The nonionic surfactant includes at least one of TX series, NP series and OP series surfactants.

5. The aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to claim 4, characterized in that: The reaction time in step S4 is 6-12 hours, and the reaction temperature is 60-90°C.

6. An application of the aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to any one of claims 1 to 5, characterized in that: Used in positive electrode plates of lithium iron phosphate batteries.

7. The use of the aqueous carboxyl-terminated nitrile rubber binder for lithium iron phosphate positive electrode according to claim 6, characterized in that: The amount of the binder added to the positive electrode plate is 1-5wt%.

Citation Information

Patent Citations

  • Acrylate structural adhesive

    CN110819265A

  • Adhesive for lithium battery aluminum plastic film and preparation method of adhesive

    CN114058319A