Graphene oxide-based calcium phosphate composite materials and their applications

By combining the graphene-based calcium phosphate composite material GO-TAPP@CaP with chitosan, a bone repair scaffold that simulates the cellular microenvironment is prepared, which solves the problems of loss of pluripotency and insufficient mechanical strength of existing materials in vitro. Effective osteogenic differentiation and repair of bone defects are achieved.

CN118557784BActive Publication Date: 2024-10-15WEIFANG MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048009.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-15
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

Existing bone repair materials lose their pluripotency during the in vitro expansion process, making it difficult to repair bone defects in situ. Moreover, the materials have insufficient mechanical strength, small pore size, and low connectivity rate, which hinders cell penetration and body fluid exchange, leading to cell apoptosis. Difficulty connecting dead and new bones.

Method used

The graphene oxide-based calcium phosphate composite material GO-TAPP@CaP is modified in two steps to generate a three-dimensional topological structure. It is combined with chitosan to prepare a bone repair scaffold, which simulates the natural three-dimensional microenvironment of cells, enhances stem cell attachment and osteogenic differentiation, and through Microporous and mesoporous structures promote extracellular matrix adsorption and osseointegration.

Benefits of technology

It improves the biocompatibility and osteogenic differentiation ability of bone repair materials, achieves effective repair of bone defects, enhances the mechanical strength and cell permeability of the material, promotes the synergy of inorganic components of bone, and reduces preparation costs and Difficulty.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118557784B_ABST
    Figure CN118557784B_ABST
Patent Text Reader

Abstract

The invention discloses graphene oxide-based calcium phosphate composite material and its application, and belongs to the field of biomedical technology. 5,10,15,20-tetrakis (4-ethynylphenyl)-porphyrin and graphene oxide are reacted to obtain a black solid, and a graphene oxide-porphyrin three-dimensional porous material is obtained after washing and drying; the graphene oxide-porphyrin three-dimensional porous material is mixed with calcium chloride, and then disodium hydrogen phosphate is added to react to obtain an off-white powder, and a graphene oxide-based calcium phosphate composite material is obtained after drying. The material has good biocompatibility, can effectively simulate the natural three-dimensional microenvironment of cells, enhance the attachment of stem cells, which is not only conducive to the proliferation of stem cells, but also conducive to osteogenic differentiation. The graphene oxide-based calcium phosphate composite material reacts with chitosan to obtain a bone repair scaffold, which can be directly applied to the bone defect without post-processing, thereby improving its application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of biomedicine technology, and in particular to a graphene oxide-based calcium phosphate composite material and applications thereof. Background Art

[0002] Bone injury remains a major clinical problem. The reason is due to the complexity of the bone tissue microenvironment in the body. Although bones have the ability to regenerate and repair themselves, some situations cannot heal themselves, such as tumors, bone diseases, etc. In past studies, many strategies for treating bone injuries have been proposed. The most conventional method is fixation to allow the injured area to self-repair. In addition, there are bone transplants combined with appropriate physical therapy, such as ultrasound, hypoxic environment and other methods. The materials for repairing bone injuries in bone transplants include synthetic bone materials, xenografts, allografts and autografts. Among them, autografts are considered to be the "gold standard" for bone repair materials. However, autologous transplants are limited by bone sources and may also introduce new trauma and complications. The use of allografts and xenografts may trigger immune rejection reactions. Therefore, synthetic bone materials with higher biocompatibility are a better choice for bone transplants.

[0003] Calcium phosphate, as a matrix for bone regeneration, can promote the process of bone regeneration. However, calcium phosphate is not easy to target to bone damage, so it is necessary to use some carriers that can target bone damage to fix calcium phosphate to bone damage, such as gel or composite hydroxyapatite. At the microscopic level, graphene is a densely packed two-dimensional honeycomb lattice of carbon atoms. It also has electrical, thermal and optical properties and is widely used in various fields of social production, including energy production, polymer science and biomedical technology. Graphene-based materials can induce stem cells to differentiate into functional cells such as bone, cartilage and nerves. Among them, graphene-based materials can promote the proliferation, migration and transfer of cell mediators of stem cells by using their large specific surface area and pores and different pore size distributions, thereby promoting their osteogenic differentiation. Stem cell therapy, as one of the most promising means to repair diseased tissues, has great potential to differentiate into mature specialized cells and has been rapidly developed. However, the clinical application of stem cell-dominated regenerative medicine is severely hindered by the loss of pluripotency during long-term in vitro expansion. In addition to the composition of the material, it is also related to the microstructure of the material. The patent application number CN201510932435.4 discloses a method for preparing a bone repair material with multidimensional channels, wherein the bone repair material is composed of at least two layered matrix structures, and the matrix structure has through holes and grooves. However, the molecular bonding of the bone repair material is weak, there is not enough mechanical strength, the degradation metabolism is fast, and it cannot meet the needs of osteogenesis; the pore size of the material is small and the connectivity rate is low, making it difficult for cells to penetrate into the scaffold, hindering the exchange of body fluids inside the scaffold, and ultimately leading to apoptosis of cells inside the scaffold material, making it impossible for new bones to connect to each other, and lacking continuity and integration, affecting the reconstruction of large defect areas. Therefore, a highly biocompatible and degradable scaffold of calcium-based graphene is needed, which can both induce cell differentiation and achieve the repair of bone defects. Summary of the invention

[0004] In view of the above-mentioned prior art, the purpose of the present invention is to provide a graphene oxide-based calcium phosphate composite material and its application. The graphene oxide-based calcium phosphate composite material GO-TAPP@CaP prepared by the present invention generates a graphene-based biomaterial with a three-dimensional topological structure by performing two-step modification on two-dimensional graphene. The material has good biocompatibility and can effectively simulate the natural three-dimensional microenvironment of cells and enhance the attachment of stem cells, which is not only beneficial to the proliferation of stem cells, but also to osteogenic differentiation. GO-TAPP@CaP is compounded with chitosan to make a bone repair scaffold GO-TAPP@CaP / CS, which can be directly placed on the bone defect without post-processing, thereby improving its application prospects.

[0005] To achieve the above object, the present invention adopts the following technical solutions:

[0006] In a first aspect of the present invention, a graphene oxide-based calcium phosphate composite material is provided. The graphene oxide-based calcium phosphate composite material is a graphene oxide-porphyrin three-dimensional porous material loaded with calcium phosphate.

[0007] Preferably, the graphene oxide-based calcium phosphate composite material is prepared by the following method:

[0008] (1) Add 5,10,15,20-tetrakis(4-ethynylphenyl)-porphyrin, bis(triphenylphosphine)palladium chloride and cuprous iodide to tetrahydrofuran and mix them evenly in the dark, then add graphene oxide and triethylamine, mix them in the dark, and then let them stand to react to obtain a black solid, which is then washed and dried to obtain a graphene oxide-porphyrin three-dimensional porous material;

[0009] (2) The graphene oxide-porphyrin three-dimensional porous material is mixed with calcium chloride, and then disodium hydrogen phosphate is added to react to obtain a graphene oxide-based calcium phosphate composite material.

[0010] Preferably, in step (1), the ratio of the added amounts of 5,10,15,20-tetrakis(4-ethynylphenyl)-porphyrin, graphene oxide, bis(triphenylphosphine)palladium chloride, cuprous iodide, triethylamine and tetrahydrofuran is 31 mg: 31 mg: 2.8 mg: 0.8 mg: 34 μL: 2 mL.

[0011] Preferably, in step (1), the temperature of the static reaction is 25° C. and the time of the static reaction is 48 h.

[0012] Preferably, in step (2), the mass ratio of the graphene oxide-porphyrin three-dimensional porous material to the calcium phosphate contained in the graphene oxide-based calcium phosphate composite material is 1:1-5; the mass ratio of the calcium chloride to disodium hydrogen phosphate is 55.5:61.0.

[0013] Preferably, in step (2), the reaction temperature is 37° C. and the reaction time is 12 h.

[0014] The second aspect of the present invention provides the use of graphene oxide-based calcium phosphate composite materials in the preparation of drugs for promoting osteogenic differentiation of stem cells or in the preparation of bone repair scaffolds.

[0015] In a third aspect of the present invention, a bone repair scaffold prepared using a graphene oxide-based calcium phosphate composite material is provided, wherein the bone repair scaffold is prepared by the following method:

[0016] Deacetylated chitosan was dissolved in acetic acid solution to obtain chitosan solution, graphene oxide-based calcium phosphate composite material was added and mixed, and then freeze-dried to obtain graphene oxide porphyrin-loaded calcium phosphate chitosan composite scaffold GO-TAPP@CaP / CS.

[0017] Preferably, the concentration of the chitosan solution is 0.02 g / mL; and the mass concentration of the acetic acid solution is 1%.

[0018] Preferably, the mass ratio of the deacetylated chitosan to the graphene oxide-based calcium phosphate composite material is 1000:6.0.

[0019] Beneficial effects of the present invention:

[0020] (1) The graphene oxide-based calcium phosphate composite material GO-TAPP@CaP prepared by the present invention is a graphene-based biomaterial with a three-dimensional topological structure generated by two-dimensional graphene modification in two steps. The material has good biocompatibility and can effectively simulate the natural three-dimensional microenvironment of cells and enhance the attachment of stem cells, which is not only beneficial to the proliferation of stem cells, but also to osteogenic differentiation. GO-TAPP@CaP has high biocompatibility, with a hemolysis rate of red blood cells less than 2% and an inhibition rate of hucMSCs less than 5%. It can promote the osteogenic differentiation of hucMSCs and the repair of bone defects, which is beneficial to its clinical application.

[0021] (2) The present invention combines GO-TAPP@CaP with chitosan to prepare a bone repair scaffold GO-TAPP@CaP / CS. The preparation method of the bone repair scaffold is simple. Its precursors GO-TAPP and GO-TAPP@CaP can be obtained by reaction at room temperature, which reduces the preparation cost and difficulty. GO-TAPP@CaP / CS can be directly applied to the bone defect without post-processing, which improves its application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 :(A) FTIR spectra of GO-TAPP, CaP and GO-TAPP@CaP;(B) UV-visible spectra of GO-TAPP, CaP and GO-TAPP@CaP;(C) 13 C NMR; (D) Thermogravimetric curve of GO-TAPP;

[0023] Figure 2 :(A)Particle size distribution curves of GO-TAPP and GO-TAPP@CaP;(B)Zeta potential of GO-TAPP, CaP and GO-TAPP@CaP;(C)Low-temperature N2 absorption isotherms of GO-TAPP and GO-TAPP@CaP at 77 K;(D)Pore size distribution curves of GO-TAPP and GO-TAPP@CaP;

[0024] Figure 3:(A)X-ray diffraction patterns of GO-TAPP and GO-TAPP@CaP;(B)Phosphate release curves of GO-TAPP@CaP with different ratios;(C)UV absorption standard curve of phosphate at 630 nm wavelength;

[0025] Figure 4 :(A)SEM of GO;(B)SEM of GO-TAPP;(C)SEM of GO-TAPP@CaP;(D)TEM of GO;(E)TEM of GO-TAPP;(F)TEM of GO-TAPP@CaP;

[0026] Figure 5 :(A)Element distribution map of GO-TAPP@CaP, including the distribution of C, N, O, P, and Ca elements in GO-TAPP@CaP;(B)EDX map of GO-TAPP@CaP;

[0027] Figure 6 :(A)Effect of GO-TAPP@CaP on hucMSCs cell viability;(B)Effect of GO-TAPP on hucMSCs cell viability;(C)Effect of CaP on hucMSCs cell viability;(D)Comparison of the effects of each treatment group on hucMSCs cell survival rate (%), data are expressed as mean ± standard error (n = 3);

[0028] Figure 7 :(A) GO-TAPP@CaP hemolysis rate of erythrocytes;(B) GO-TAPP hemolysis rate of erythrocytes;(C) CaP hemolysis rate of erythrocytes;(D) GO-TAPP@CaP, GO-TAPP and CaP hemolysis rate of erythrocytes, data are expressed as mean ± standard error (n = 3);

[0029] Figure 8 :(A) Results of Alizarin Red S (ARS staining) of GO-TAPP@CaP with different concentrations (scale bar = 200 μm);(B) Results of alkaline phosphatase staining (ALP staining) of GO-TAPP@CaP with different concentrations (scale bar = 200 μm);(C) Quantitative analysis of ARS staining results of GO-TAPP@CaP with different concentrations;(D) Quantitative analysis of ALP staining results of GO-TAPP@CaP with different concentrations, data are expressed as mean ± standard error (n = 3); # p < 0.05, ## p < 0.01, ### p < 0.001;

[0030] Fig. 9 :(A) Results of ARS staining in each group (scale bar = 200 μm);(B) Quantitative analysis of ARS staining in each group;(C) Results of ALP staining in each group (scale bar = 200 μm);(D) Quantitative analysis of ALP staining in each group, data are expressed as mean ± standard error (n = 3); ** / ## p < 0.01, *** / ### p <0.001, **** / #### p < 0.0001;

[0031] Fig.10 :(A) Volcano map of mRNA changes before and after GO-TAPP@CaP treatment of stem cells for 14 days, red indicates up-regulated proteins, blue indicates down-regulated proteins;(B) Heat map cluster of mRNA changes before and after GO-TAPP@CaP treatment of hucMSCs for 14 days, the bar graph from blue to red indicates the expression level of DEGs from low to high;(C) Gene ontology (GO) analysis of genes that changed after GO-TAPP@CaP treatment of stem cells for 14 days;(D) KEGG pathway analysis of all DEGs;

[0032] Fig.11 :(A) The expression levels of EGF and SPP1 proteins were determined by Western blot analysis;(B) Schematic diagram of GO-TAPP@CaP promoting osteogenic differentiation of stem cells;(C) EGF relative protein expression results;(D) SPP1 relative protein expression results, data are expressed as mean ± standard error (n = 3); ** p < 0.01, **** p < 0.0001;

[0033] Fig.12 :(A) Three-dimensional reconstructed digital images of skull defect model analyzed by micro-CT;(B) Quantitative analysis of BMD percentage of bone-related parameters in each group;(C) Quantitative analysis of BV / TV percentage of bone-related parameters in each group, data are expressed as mean ± standard error (n = 3); * / # p < 0.05, ** / ## p < 0.01, *** / ### p < 0.001, **** / #### p < 0.0001;

[0034] Fig.13:The weight changes of rats in different groups at different times;

[0035] Fig.14 : H&E staining and Masson staining of each group after 4, 8, and 12 weeks of implantation of GO-TAPP@CaP / CS, GO-TAPP / CS, and CaP / CS (blue and yellow arrows indicate newly formed mature bones, and the left side of each group is the blank control), the scale bar of the black scale is 2000 μm, and the scale bar of the red scale is 200 μm;

[0036] Fig.15 : Hematoxylin and eosin (H&E) staining of the main organs (heart, liver, spleen, lung and kidney) of rats after different treatments (scale bar is 200 μm);

[0037] Fig.16 : The blood routine test results of the corresponding groups (week 12), including (A) WBC test results; (B) RBC test results; (C) HGB test results; (D) HCT test results; (E) MCV test results; (F) MCH test results; (G) MCHC test results; (H) PLT test results; (I) RDW-SD test results; (J) RDW test results; (K) MPV test results; (L) PCT test results, data are expressed as mean ± standard error (n = 3);

[0038] Fig.17 :Synthesis route of GO-TAPP@CaP / CS and schematic diagram of bone repair. DETAILED DESCRIPTION

[0039] Although calcium phosphate is a commonly used bone regeneration material, and graphene-based materials are commonly used materials to promote stem cell proliferation, migration, cell media delivery and osteogenic differentiation, the clinical application of stem cell-based regenerative medicine is severely hampered by the loss of pluripotency during long-term in vitro expansion. Even if osteogenic differentiation of stem cells can be achieved in vivo, it is difficult to achieve in situ repair of bone defects.

[0040] Based on this, the purpose of the present invention is to provide a graphene oxide-based calcium phosphate composite material and its application. The present invention first prepares a three-dimensional topological structure of a graphene oxide-based calcium phosphate composite material GO-TAPP@CaP by two-step modification of two-dimensional graphene. GO-TAPP@CaP uses graphene oxide as a structural unit and uses methods such as oxidative coupling to prepare a composite three-dimensional (3D) graphene-based biomaterial with a hierarchical pore structure (micropores to macropores). It can effectively simulate the natural three-dimensional microenvironment of cells and enhance the attachment of stem cells, which is not only beneficial to the proliferation of stem cells, but also to osteogenic differentiation. Then, GO-TAPP@CaP is reacted with chitosan to prepare a bone repair scaffold GO-TAPP@CaP / CS.

[0041] like Fig.17 As shown, the present invention uses graphene oxide as a template to coat graphene oxide with several porphyrin structures to form a structure of porphyrin-coated graphene oxide, and then uses a double decomposition reaction to load and coat CaP in GO-TAPP to form a GO-TAPP@CaP microporous composite material, that is, the micropores of GO-TAPP are loaded with CaP, and the surface of GO-TAPP is also coated with CaP. Finally, GO-TAPP@CaP is dispersed in deacetylated chitosan and freeze-dried to form GO-TAPP@CaP / CS. GO-TAPP@CaP has the ability to induce human umbilical cord mesenchymal stem cells (hucMSCs) to differentiate into osteoblasts. GO-TAPP@CaP / CS has a wide range of interconnected macropores, which are conducive to bone growth, capillary formation and the transportation of nutrients. In addition, the micropores and mesopores coexisting in the graphene oxide-based calcium phosphate composite material can also significantly promote the adsorption of extracellular matrix (ECM), thereby promoting cell attachment and achieving multi-scale bone integration. Both in vitro and in vivo experiments have shown that bone growth, capillary formation, and nutrient transport cooperate with nanoscale calcium phosphate (CaP), which is similar to the inorganic components of bone, to provide abundant adhesion sites, fully induce osteogenic differentiation in the absence of any soluble growth factors, and enhance its ability to repair bone in vivo.

[0042] In order to enable those skilled in the art to more clearly understand the technical solution of the present application, the technical solution of the present application will be described in detail below in conjunction with specific embodiments.

[0043] Note: The graphene oxide (GO) used in the present invention was purchased from Shanghai Dingfen Chemical Technology Co., Ltd.

[0044] Deacetylated chitosan was purchased from Anaiji Chemical Co., Ltd.

[0045] The test materials used in the examples of the present invention are all conventional test materials in the art and can be purchased through commercial channels.

[0046] Example 1: Preparation of GO-TAPP@CaP (mass ratio of GO-TAPP to CaP 1:3)

[0047] (1) Preparation of GO-TAPP: Weighed 5,10,15,20-tetrakis(4-(ethynylphenyl)-porphyrin (31 mg, 0.04 mM), bis(triphenylphosphine)palladium chloride (2.8 mg, 0.004 mM) and cuprous iodide (0.8 mg, 0.004 mM) were added to a 5 mL brown vial, and then dry tetrahydrofuran (2 mL) was added. The reaction system was sonicated for 5 min, and then graphene oxide (31 mg) and triethylamine (34 μL, 0.25 mM) were added. The reaction system was sonicated again for 5 min, and then the reaction was started at room temperature (25 °C) for 48 h. The reaction was completed to obtain a black powder, which was soaked in tetrahydrofuran (2 mL) for 24 h. After 24 h, the solvent was removed, and the eluate was washed with acetone until it was colorless, and then dried under vacuum at 60 °C for 6 h to obtain GO-TAPP.

[0048] (2) Preparation of GO-TAPP@CaP: Weigh GO-TAPP and CaP at a mass ratio of 1:3, that is, take 20.1 mg GO-TAPP and 55.5 mg CaCl2 into a 250 mL round bottle, add 50 mL distilled water, and stir at 37 °C for 3 h. Put 61 mg Na2HPO4 into a 100 mL beaker and fully dissolve it with 50 mL distilled water to obtain Na2HPO4 solution, then slowly add the Na2HPO4 solution into the round bottle at a rate of 1 drop / s, stir at 37 °C (100 rpm / min) and react for 12 h. After the reaction is completed, remove the supernatant, collect the gray precipitate, and dry it to obtain the GO-TAPP@CaP composite material.

[0049] Example 2: Preparation of GO-TAPP@CaP (mass ratio of GO-TAPP to CaP 1:1)

[0050] The difference from Example 1 is that in step (2), GO-TAPP and CaP are weighed in a mass ratio of 1:1, that is, 60.2 mg GO-TAPP and 55.5 mg CaCl2 are put into a 250 mL round bottle. Finally, a GO-TAPP@CaP composite material is prepared.

[0051] Example 3: Preparation of GO-TAPP@CaP (mass ratio of GO-TAPP to CaP 1:5)

[0052] The difference from Example 1 is that in step (2), GO-TAPP and CaP are weighed at a mass ratio of 1:5, that is, 12.1 mg GO-TAPP and 55.5 mg CaCl2 are put into a 250 mL round bottle. Finally, a GO-TAPP@CaP composite material is prepared.

[0053] Example 4: Preparation of GO-TAPP@CaP / CS (mass ratio of GO-TAPP to CaP 1:3) bone repair scaffold

[0054] 1.0 g of deacetylated chitosan powder was dissolved in 50 mL of 1.0% acetic acid solution to obtain a chitosan solution. Then 6.0 mg of GO-TAPP@CaP prepared in Example 1 was added to the chitosan solution and stirred thoroughly. The solution was added to a 96-well plate and freeze-dried (-40 °C, 24 h) to obtain a bone repair scaffold GO-TAPP@CaP / CS composite material.

[0055] Comparative Example 1: Preparation of GO-TAPP bone repair scaffold

[0056] 1.0 g of deacetylated chitosan powder was dissolved in 50 mL of 1.0% acetic acid solution to obtain a chitosan solution. Then 1.5 mg of GO-TAPP prepared in step (1) of Example 1 was added to the chitosan solution and stirred thoroughly. The solution was added to a 96-well plate and freeze-dried (-40 °C, 24 h) to obtain a bone repair scaffold GO-TAPP / CS composite material.

[0057] Comparative Example 2: Preparation of CaP bone repair scaffold

[0058] (1) Weigh 55.5 mg of CaCl2 into a 250 mL round bottle, add 50 mL of distilled water, and stir at 37°C for 3 h. In addition, weigh 61 mg of Na2HPO4 into a 100 mL beaker, fully dissolve it with 50 mL of distilled water, and then slowly add it to the CaCl2 aqueous solution that has been stirred for 3 h, and react for another 12 h (37°C, 100 rpm / min), then remove the supernatant and collect the white precipitate, which is CaP.

[0059] (2) Dissolve 1.0 g of deacetylated chitosan powder in 50 mL of 1.0% acetic acid solution to obtain a chitosan solution. Then, add 4.5 mg of CaP to the chitosan solution and stir thoroughly to mix. Add the solution to a 96-well plate and freeze-dry (-40 °C, 24 h) to obtain a bone repair scaffold CaP / CS composite material.

[0060] Characterization:

[0061] Unless otherwise specified, the GO-TAPP@CaP used for characterization was prepared in Example 1, GO-TAPP was prepared in step (1) of Example 1, and CaP was prepared in step (1) of Comparative Example 2.

[0062] (1) FT-IR was used to verify the construction of GO-TAPP@CaP. Figure 1 (A) is the FT-IR of GO-TAPP@CaP, GO-TAPP and CaP. It can be seen that GO-TAPP@CaP has the characteristics of both GO-TAPP and CaP. The characteristic absorption peaks of GO-TAPP are located at 1600 and 1725 cm -1 The characteristic absorption peak of CaP is located at 1058 cm -1 , which belongs to phosphate. The characteristic peaks of -C=C-, -C=O and phosphate in GO-TAPP@CaP indicate that CaP is successfully loaded into GO-TAPP.

[0063] (2) The successful construction of GO-TAPP@CaP was verified by UV-visible light. Figure 1 (B) is the UV spectrum of GO-TAPP before and after CaP loading. GO-TAPP@CaP, GO-TAPP and CaP all have certain UV absorption at wavelengths of 200-800 nm. Among them, GO-TAPP has strong UV absorption at 230-240 nm, which is caused by the π → π* transition of its own CC skeleton. In GO-TAPP@CaP, the absorption peak intensity of the CC skeleton is reduced, indicating that the shell formed by the loaded CaP shields the UV absorption of the carbon skeleton in GO-TAPP.

[0064] (3) Through solid state 13 C-NMR further confirmed the carbon skeleton structure of GO-TAPP and GO-TAPP@CaP. Figure 1 (C) Solid-state GO-TAPP before and after CaP loading 13 C CP / MAS NMR spectra show that GO-TAPP before and after CaP loading has the characteristic peaks of porphyrin macrocycle of GO-TAPP (122, 130 and 140 ppm). In addition, GO-TAPP before and after CaP loading also has the characteristic peak of -C≡CC≡C- (101 ppm), indicating that the characteristics of GO-TAPP itself have not changed before and after CaP loading.

[0065] (4) The thermal stabilities of GO-TAPP and GO-TAPP@CaP were compared by thermogravimetric analysis. Figure 1(D) is the thermogravimetric analysis curve of GO-TAPP@CaP, GO-TAPP and CaP. It can be seen that GO-TAPP@CaP has the characteristics of both GO-TAPP and CaP. Compared with GO-TAPP, the loaded CaP has higher thermal stability. Among them, GO-TAPP@CaP degrades rapidly in the range of 181-196 ℃, which is due to the continuous decomposition of oxygen-containing functional groups in GO-TAPP and CaP. Subsequently, GO-TAPP@CaP began to degrade slowly, and still maintained 73.93% of its initial weight at 800 ℃.

[0066] (5) Particle size analysis and zeta potential determination: GO-TAPP@CaP (120 μg mL -1 ) and GO-TAPP (30 μg mL -1 ) solution. 500 μL of each group was placed in a test dish, and the particle size distribution of GO-TAPP@CaP and GO-TAPP was measured by dynamic light scattering (DLS) using a Zeta potential instrument. Each experiment was performed in parallel three times. In addition, GO-TAPP@CaP (120 μg mL -1 )、GO-TAPP(30 μg·mL -1 ) and CaP (90 μg mL -1 ) solution, and then 500 μL of each group was added to the potential cell, and the potential of each group was measured with a Zeta potentiometer and quantitatively analyzed. Each experiment was carried out in parallel three times.

[0067] Dynamic light scattering (DLS) further confirmed the successful loading of CaP. The hydrodynamic diameters of GO-TAPP@CaP and GO-TAPP in water were determined. Figure 2 (A) It can be seen that after GO-TAPP was loaded with CaP, the average size of GO-TAPP@CaP increased significantly from 3091 nm to 4145 nm. Figure 2 (B) shows the Zeta potential of GO-TAPP@CaP, GO-TAPP, and CaP in distilled water solution. It can be seen that after loading CaP, the potential of GO-TAPP increased from -26.97 to -13.27 mV, indicating that CaP was successfully coated by GO-TAPP to form a GO-TAPP@CaP composite material.

[0068] (6) Figure 2 (C) shows the low-temperature N2 adsorption / desorption isotherms of GO-TAPP before and after CaP loading. The surface areas of GO-TAPP@CaP and GO-TAPP were calculated using BET (24.42 m 2 g -1 , 14.73 m2 g -1 ) and total pore volume (0.19 cm 3 g -1 , 0.0529 cm 3 g -1 ). In addition, the PSD of GO-TAPP@CaP and GO-TAPP obtained by NLDFT method further revealed typical type II and type IV isotherms, according to Figure 2 (D) It can be seen that GO-TAPP@CaP and GO-TAPP are mesoporous structures with average pore sizes of 23.14 nm and 12.31 nm, respectively. It is worth noting that compared with GO-TAPP, the specific surface area and pore size of GO-TAPP@CaP are relatively larger, indicating that after loading, CaP is not only loaded into the original pores of GO-TAPP, but also forms a CaP shell with more pores, making GO-TAPP@CaP have a larger specific surface area and pore volume.

[0069] (7) Figure 3 (A) is the XRD test results of GO-TAPP@CaP, GO-TAPP and CaP. It can be seen that GO-TAPP@CaP combines the characteristic peaks of GO-TAPP and CaP (0 2 0, 1 2 -1, 1 4 -1, 2 1 -1, 2 0 0), indicating that CaP is successfully coated on GO-TAPP.

[0070] (8) PO4 3- Determination of standard curve: CaP (10 mg) was accurately weighed and dispersed in 1 mL of distilled water, and then diluted to concentrations of 1, 2.5, 5, 10, 20, 30, 40 and 50 μg mL -1 A series of standard solutions were prepared. The absorbance of each group of samples at a wavelength of 620 nm was measured using a malachite green phosphate detection kit (purchased from Shanghai Bio-Tech Biotechnology Co., Ltd., product number S0196S, specification 500 times) and an enzyme marker. 3- The standard curve was used to deduce PO4 3- The linear regression equation was obtained. The malachite green phosphate detection kit was used to analyze the release of phosphate in GO-TAPP@CaP with different loading rates. Different concentrations of PO4 3- Solution, draw the standard curve see Figure 3 (C).

[0071] PO4 3- Determination of release amount: PO4 3- Detected by malachite green phosphate detection kit. 1 mL of GO-TAPP@CaP (120 μg mL -1) were transferred to dialysis bags (molecular weight cutoff 7 kD) and then transferred to 50 mL of distilled water. The PO4 content of the solution outside the dialysis bag was measured at different time periods. 3- The release curves were drawn and each experiment was repeated three times.

[0072] according to Figure 3 (B) Standard curve for measuring the release of PO4 from GO-TAPP@CaP prepared in Examples 1 to 3 3- The results showed that the release of phosphate increased with the increase of CaP ratio, indicating that the loading effect of CaP is related to the concentration of CaP, and as the CaP ratio increases, PO4 3- Therefore, when the mass ratio of GO-TAPP and CaP components is 1:3, GO-TAPP@CaP has a relatively slow release capacity for PO4 3- Better release ability.

[0073] (10) Determination of loading rate and encapsulation efficiency: During the preparation of GO-TAPP@CaP according to Examples 1 to 3, the content of free phosphate in the supernatant was used to indirectly determine the loading capacity and encapsulation efficiency of GO-TAPP@CaP. The GO-TAPP@CaP distilled water suspension prepared in Examples 1 to 3 was centrifuged at 8000 rpm for 10 min at room temperature, and the supernatant was taken to analyze its phosphate content. Each group of experiments was repeated three times. The calculation method of EE% and LC% is as follows:

[0074] LC% = (W1-W2) / W3× 100% (Formula 1);

[0075] EE% = (W1-W2) / W1× 100% (Formula 2);

[0076] W1 is the added PO4 3- The mass of W2 is the free PO4 in the suspension. 3- W3 is the mass of the final GO-TAPP@CaP. The drug loading and encapsulation efficiency of the GO-TAPP@CaP / CS composite scaffold materials prepared in Examples 1 to 3 are shown in Table 1.

[0077] Table 1

[0078]

[0079] According to Table 1, it can be seen that the GO-TAPP@CaP (1:3) prepared in Example 1 has the highest encapsulation efficiency and higher loading capacity (80.12 ± 0.68, 64.37 ± 0.55). Therefore, the GO-TAPP@CaP prepared in Example 1 was used in subsequent studies such as bone differentiation.

[0080] (11) The transmission electron microscopy and element distribution mapping of GO-TAPP@CaP were analyzed to observe the distribution of C, N, O, Ca, and P in GO-TAPP@CaP. In addition, an appropriate amount of GO-TAPP@CaP was taken and the contents of Ca and P in GO-TAPP@CaP were determined by inductively coupled plasma mass spectrometry (ICP-MS).

[0081] Figure 4 The microstructural changes from GO to GO-TAPP@CaP observed using SEM and TEM. From SEM, it can be seen that GO is a smooth layered structure, while GO-TAPP formed after TAPP coating on GO is a rough layered structure. GO-TAPP@CaP formed by CaP loading on GO-TAPP is a layer of irregular spheres and rods wrapped on the rough layered structure of GO-TAPP. This shows the successful synthesis of GO-TAPP@CaP. The micromorphology of GO-TAPP@CaP matches its BET results. The rough surface, high specific surface area and high pore volume of GO-TAPP@CaP make it have the potential to promote cell proliferation. Figure 5 The mapping diagram of GO-TAPP and the corresponding energy dispersive X-ray (EDX) spectrum clearly show that the required elements (i.e., C, N, and O) are uniformly distributed in GO-TAPP@CaP. The contents of Ca and P in GO-TAPP@CaP were detected by ICP-MS, which were 16.02% and 11.71%, respectively.

[0082] Test Example 1: In vitro biocompatibility evaluation

[0083] (1) Determination of cytotoxicity: The experiment was divided into four groups, using basic DMEM medium and different concentrations (0-2000 μg mL -1 ) prepared in Example 1 (denoted as GO-TAPP@CaP group), GO-TAPP prepared in step (1) of Example 1 (denoted as GO-TAPP group), CaP group prepared in step (1) of Comparative Example 2 (denoted as CaP group), and a control group without drug addition. In a 96-well plate, 5 × 10 3 Human umbilical cord mesenchymal stem cells (hucMSCs) (from the Stem Cell Laboratory of Shandong Second Medical University) were inoculated at a density of 10 cells per well, and 180 μL of cell suspension (cell suspension containing 5 × 10 3DMEM complete growth medium was purchased from Gibco, USA) and 200 µL PBS was added to the surrounding replicate wells for liquid sealing to prevent excessive evaporation of cells. After culturing for 24 h, 20 µL of the previously prepared drug was added to achieve 0-200 µg mL per well. -1 The cells were cultured together for another 72 h. After 72 h, 20 µL of MTT reagent was added to each well. After 4 h, the supernatant was removed and 150 µL of DMSO was added to dissolve the MTT-formamide crystals. After dissolving on a shaker for 10 min, the absorbance of the 96-well plate was measured at a wavelength of 570 nm using a microplate reader. Each experiment was repeated three times.

[0084] To study the adverse damage of GO-TAPP@CaP itself to stem cells, the cytotoxicity tests of GO-TAPP@CaP, GO-TAPP and CaP on hucMSCs were conducted. Figure 6 Different concentrations of GO-TAPP@CaP, GO-TAPP and CaP (0-200 μg mL -1 ) The survival rate of hucMSCs cells after 3 days of culture. It was found that the relative viability of cells did not change significantly with the increase of material concentration. -1 Within the concentration range, the cell viability of all treatment groups was higher than 95%, indicating that GO-TAPP@CaP had almost no effect on hucMSCs cells.

[0085] (2) Determination of hemolysis rate: Fresh blood was collected from SD female rats (purchased from Beijing Weitong Lihua Experimental Animal Technology Co., Ltd., 10 weeks old). Red blood cells were collected by centrifugation at 15,000 rpm for 20 min and then washed three times with PBS. Red blood cells (4% w / w) were then incubated with GO-TAPP@CaP, GO-TAPP, and CaP (0-200 µg mL -1 ) at a ratio of 1:9 (v / v) at 37 °C for 3 h and centrifuged at 12000 rpm for 20 min. Then 100 µL of supernatant from each group was placed in a 96-well plate, and the absorbance of each group was measured at a wavelength of 570 nm using an ELISA reader. Each experiment was repeated three times. Distilled water was used as a positive control and PBS as a negative control. The amount of hemolysis was calculated according to the following formula:

[0086] Hemolysis (%) = (A – An) / (Ap – An) × 100% (Formula 3);

[0087] Among them, "A" is the absorbance of the supernatant after adding GO-TAPP@CaP, GO-TAPP and CaP to erythrocytes. "An" is the absorbance of the supernatant after adding PBS (negative control) to erythrocytes. "Ap" is the absorbance of the supernatant after adding distilled water (positive control) to erythrocytes.

[0088] To study the hematotoxicity of GO-TAPP@CaP, the hemolytic rates of GO-TAPP@CaP, GO-TAPP, and CaP were evaluated using retinal arterial blood from SD rats ( Figure 7 The results showed that the hemolysis rate of all groups was less than 2% (concentration: 40-200 μg·mL -1 ). Among them, when the concentration is 200 μg·mL -1 When , the hemolysis rate of GO-TAPP@CaP was only 0.66 ± 0.05%, indicating that GO-TAPP@CaP has good blood compatibility.

[0089] Experimental Example 2: In vitro stem cell differentiation experiment

[0090] (1) Stem cell induction method: After hucMSCs were stably cultured in growth medium (GM) to a cell density of 70-80% (density percentage), the medium was replaced with human umbilical cord mesenchymal stem cell osteogenic differentiation medium (ODM) and grouped according to experimental needs (specifically divided into a control group without drug addition, GO-TAPP@CaP group, GO-TAPP group and CaP group; different concentrations of drugs were added for differentiation experiments each time the ODM medium was changed). Each group was cultured for a total of 14 days (ODM medium was changed every 2-3 days).

[0091] (2) Determination of ARS staining: Prepare a 24-well plate and treat hucMSCs according to the stem cell differentiation method (the experiment was divided into four groups: control group (no drug added), GO-TAPP@CaP group, GO-TAPP group and CaP group; 0-200 μg mL -1The above four groups of drugs were differentiated for 14 days). A blank control group (no drug or culture medium) was set up: 50 μL of 10% CPC solution was added to each well, and the OD value was measured at a wavelength of 570 nm. Each experiment was repeated three times. After 14 days, the ODM was removed, the cells were rinsed twice with PBS, and the cells were fixed in 300 μL of 4% paraformaldehyde for 20 min. Then the paraformaldehyde fixative was removed, the cells were rinsed three times with distilled water, and then stained with 300 μL of 1% Alizarin Red S (pH 4.2) dye at room temperature in the dark for 10-20 min. Then the cells were rinsed three times with distilled water to terminate the color reaction. Finally, the cells were dried, stored at room temperature in the dark, and photographed with an optical microscope. Each experiment was repeated three times. Take the dried 24-well plate from the ARS staining qualitative experiment above, add 250 µL of 10wt% CPC solution (chlorocetylpyridinium) to each well, and incubate at room temperature for 30-60 min to dissolve the alizarin red on the mineralized nodules (mineralized nodules are calcium nodules stained with alizarin red S). Mix the dissolved solution thoroughly, and then add 50 µL of the mixed solution to each well of the 96-well plate, with three replicate wells for each sample.

[0092] To evaluate the ability of GO-TAPP@CaP to induce stem cells to differentiate into osteoblasts in vitro, ARS staining was used to detect mineralized nodules in hucMSCs cells. The differentiation ability of GO-TAPP@CaP at different concentrations on hucMSCs cells was detected by ARS staining. Figure 8 (A) and Figure 8 (C) The results showed that compared with the control group, 120 μg mL -1 The GO-TAPP@CaP with the highest mineralized nodules can be regarded as the optimal differentiation concentration. Based on the evaluation of the effects of different concentrations of GO-TAPP@CaP on the mineralization of stem cells, the optimal differentiation concentration of GO-TAPP@CaP (120 μg·mL -1 )、GO-TAPP(30 μg·mL -1 ) and CaP (90 μg mL -1 ) on the differentiation ability of hucMSCs, see Fig. 9 (A) and Fig. 9(B). The results showed that the ARS staining color of the GO-TAPP@CaP group was the darkest, indicating that the amount of mineralized nodules was the highest. In addition, quantitative analysis of the ARS staining experiment also led to the same conclusion as the staining experiment, where the percentage of mineralized nodules in the GO-TAPP@CaP group was 566.88 ± 17.45%, while that in the GO-TAPP group or the CaP group was only 190.92 ± 8.10% and 445.19 ± 0.52%. This proves that GO-TAPP@CaP combines the ability of GO-TAPP and CaP to promote the differentiation of stem cells into osteoblasts.

[0093] (3) Determination of ALP staining: Prepare a 24-well plate and treat hucMSCs according to the stem cell differentiation method (specifically divided into a control group (no drug added), a GO-TAPP@CaP group, a GO-TAPP group, and a CaP group; add 0-200 μg mL ALP each time the ODM culture medium is replaced. -1 The cells were treated with drugs of each group and differentiated for 14 days). After 14 days, ODM was removed, the cells were rinsed twice with PBS, fixed with 300 μL of 4% paraformaldehyde for 20 min, and then rinsed three times with distilled water. The cells were then incubated with 300 μL of ALP staining reagent (10 mL ALP buffer, 33 μL BCIP solution, and 66 μL NBT solution) for 24 h, and the staining reagent was removed. Finally, the cells were washed with distilled water, dried, and stored in the dark at room temperature. The photos were taken with an optical microscope, and each experiment was repeated three times.

[0094] Prepare 24-well plates and influence hucMSCs according to the stem cell differentiation method (specifically divided into a control group without drug addition, a GO-TAPP@CaP group, a GO-TAPP group, and a CaP group; add 0-200 μg mL each time the ODM medium is replaced) -1 After 14 days, the ODM was removed, washed twice with PBS, and 0.2 mL of cell lysis buffer (RIPA lysis buffer) was added to each well for 40 min. The cell suspension (cell fragments after lysis and lysis buffer) was incubated at 1.5 × 10 4 Centrifuge at rpm for 5 min and extract the supernatant, then add p-nitrophenyl phosphate (pNPP) (colorimetric substrate) to the supernatant according to the alkaline phosphatase quantitative kit (purchased from Shanghai Biyuntian Biotechnology Co., Ltd., product number P0321S, specification 100 times) and incubate for 30 min (50 μL per well), and finally add the reaction stop solution in the kit to terminate the reaction. Three replicate wells were set for each sample, and the absorbance was measured at a wavelength of 450 nm using an enzyme reader, and each group of experiments was repeated three times.

[0095] Based on the ALP staining results, the ALP expression level in hucMSCs cells was detected by ALP staining. First, the differentiation ability of GO-TAPP@CaP at different concentrations on hucMSCs cells was detected by ALP staining kit. Figure 8 (B) and Figure 8 (D) The results showed that compared with the control group, 120 μg mL -1 GO-TAPP@CaP had the highest ALP expression, which matched the ARS staining results, indicating that 120 μg·mL -1 The optimal differentiation concentration was evaluated based on the effect of different concentrations of GO-TAPP@CaP on the ALP content of stem cells. -1 )、GO-TAPP(30 μg·mL -1 ) and CaP (90 μg mL -1 ) on the differentiation ability of hucMSCs, see Fig. 9 (C) and Fig. 9 (D). The results showed that the ALP staining color of the GO-TAPP@CaP group was the darkest, indicating that the ALP production was the highest. In addition, quantitative analysis of the ALP staining experiment also yielded the same conclusion as the staining experiment, where the percentage of ALP production in the GO-TAPP@CaP group was (243.54 ± 8.12%), while that in the GO-TAPP group and the CaP group was only (134.65 ± 7.66%) and (196.22 ± 7.59%). This also proves that GO-TAPP@CaP combines the ability of GO-TAPP and CaP to promote the differentiation of stem cells into osteoblasts.

[0096] (4) Determination of mRNA transcriptome sequencing: mRNA sequencing (mRNA-seq) was performed on hucMSCs. HucMSCs were affected according to the stem cell differentiation method. They were divided into a control group (no drug) and a GO-TAPP@CaP group; 120 μg·mL was added each time the ODM culture medium was replaced. -1 The cells were treated with drugs and differentiated for 14 days. After 14 days, the cells were collected and RNA was extracted using SparkZol reagent (purchased from Shandong Si Ke Jie Biotechnology Co., Ltd.) for sequencing. The mRNA expression level was determined using FPKM (fragments per kilobase per million fragments mapping exons). Differential expression analysis was performed using DESeq R software, and the threshold for differentially expressed genes (DEGs) was set to the corrected value. pThe value was 0.05, and the absolute value of log2FC (converted change) was ≥ 0.58. Cluster Profiler was used to perform GO analysis and KEGG enrichment analysis on the differentially expressed genes, and the results were visualized. Each group of experiments was repeated three times. Pathways with FDR values ​​less than 0.05 were considered significantly enriched.

[0097] To further study the mechanism by which GO-TAPP@CaP promotes hucMSCs differentiation, mRNA transcriptome sequencing experiments were performed. Fig.10 (A) is a volcano plot of stem cell gene changes after being affected by different concentrations of GO-TAPP@CaP, with 1574 genes upregulated and 1989 genes downregulated. Fig.10 (B) is a heat map cluster of mRNA changes, indicating that the effect of GO-TAPP@CaP on gene expression is not consistent. Fig.10 (C) Gene ontology (GO) functional enrichment analysis showed that processes such as bone mineralization and positive regulation of the PI3K signaling pathway were enriched. Fig.10 (D) Kyoto Encyclopedia of Genomes (KEGG) pathway enrichment analysis results showed that GO-TAPP@CaP promoted bone differentiation mainly through the PI3K-Akt signaling pathway. GO and KEGG enrichment analysis results showed that 120 μg mL -1 GO-TAPP@CaP promoted the differentiation of hucMSCs into osteoblasts by regulating the PI3K-Akt signaling pathway (genes such as EGF, SPP1, CDKN1A, ITGA6, and COL4A4 were enriched).

[0098] (5) Western blotting: The hucMSCs were treated with the stem cell differentiation method and divided into a control group (no drug) and a GO-TAPP@CaP group (120 μg mL -1 ); add 120 μg mL each time when changing ODM medium -1 The GO-TAPP@CaP group was treated with 120 μg·mL -1 In addition to this concentration, DMEM basic medium was used to prepare a 60 μg mL -1 GO-TAPP@CaP group (denoted as 60 μg·mL -1 hucMSCs were cultured in three 25T cell culture flasks, with a cell density of 5 × 10 5, and cultured with GM medium. When the cell density reached 80% (density percentage) or above, the ODM medium was replaced and GO-TAPP@CaP was used for treatment. After 14 days of GO-TAPP@CaP treatment of hucMSCs cells (the medium was changed every 2-3 days), the cells were collected and lysed with RIPA buffer containing protease inhibitors. After lysis, the supernatant was taken, part of the supernatant was used for protein content determination with BCA working solution, and the rest of the supernatant was diluted proportionally with 4× protein loading buffer. After dilution, it was heated in a 100℃ water bath for 10 minutes and stored at -20℃. The protein dilution was separated by sodium dodecyl sulfate polyacrylamide gel (SDS-PAGE) and transferred to a PVDF membrane. After blocking the PVDF membrane with 10% skim milk, the membrane was incubated with specific primary antibodies (specific primary antibodies for EGF are ab206423, specific primary antibodies for SPP1 are ab214050, both brands are abcam) at 4°C overnight, and then incubated with goat anti-rabbit antibody (catalog number EF0007, brand Sikejie) at room temperature for 1 h. Finally, enhanced chemiluminescence (ECL) was used to observe protein expression. Image J was used to quantitatively analyze the results, and each group of experiments was repeated three times.

[0099] Differentially expressed genes in the PI3K-Akt signaling pathway identified by mRNA transcriptome sequencing were verified by western blotting ( Fig.11 ). The results showed that GO-TAPP@CaP could significantly upregulate the expression of EGF and SPP1 proteins in hucMSCs cells.

[0100] Experimental Example 3: In vivo bone repair experiment

[0101] (1) Establishment of an animal model of bilateral skull defect in SD rats. Eighteen 10-week-old female SD rats (purchased from Beijing Weitong Lihua Experimental Animal Technology Co., Ltd.) were fasted for 8 h before surgery. Anesthesia was performed by intraperitoneal injection of 1% sodium pentobarbital (50 mg / kg). After the rats were anesthetized, they were placed prone on a fixed board, and the hair in the surgical area of ​​the skull was shaved with a shaver. After disinfection with iodine tincture, a sagittal incision was made from the midpoint of the line connecting the two orbits of the rat to the skull, and the periosteum was peeled off with a needle to expose the bone surface. Two bone defects with a diameter of 5 mm were made on both sides of the skull using a bone drill. During the process, attention was paid to cooling down and preventing rupture of the dura mater. Afterwards, the mice were randomly divided into three groups (6 mice in each group): one side of each group was loaded with a single chitosan scaffold as a control group, and the other side was loaded with the GO-TAPP@CaP / CS scaffold prepared in Example 4, the GO-TAPP / CS scaffold prepared in Comparative Example 1, and the CaP / CS scaffold prepared in Comparative Example 2, and then the wounds were sutured with 3-0 sutures. After suturing, each group of mice was intramuscularly injected with 80,000 units of sodium penicillin and housed in separate cages.

[0102] (2) In vivo bone repair experiment: Rats were killed and skulls were removed 4, 8, and 12 weeks after the skull defect animal model was established to analyze the skull defect repair. The skull samples of each group were scanned and reconstructed using a micro-computed tomography (micro-CT) system, and 3D digital and tomographic images were obtained using CTvox software. In addition, bone volume / total volume (BV / TV) and bone mineral density (BMD) were measured using auxiliary tissue morphometry software (CTAn). At week 12, major organs, including heart, liver, spleen, lung, and kidney, were collected from each group of SD rats and fixed with 4% paraformaldehyde together with the skull, followed by H&E staining, and then Masson staining of the skull. At week 12, 1 to 2 mL of blood samples were collected from the fundus artery of each group of SD rats. 200 μL of each blood sample was taken for routine blood analysis, including WBC (white blood cell count), RBC (red blood cell count), HGB (hemoglobin), HCT (hematocrit), MCV (mean corpuscular volume), MCH (mean hemoglobin), MCHC (mean corpuscular hemoglobin concentration), PLT (platelet count), MPV (mean platelet volume), RDW (red blood cell distribution width), PCT (procalcitonin), and RDW-SD (red blood cell distribution width standard deviation).

[0103] Fig.12 (A) Micro-CT results at 4, 8, and 12 weeks after scaffold implantation at the injury site were compared. At different time points, more new bone tissue was generated in the bone defect area of ​​the GO-TAPP@CaP / CS scaffolds compared with the other groups.

[0104] Fig.12(B) and 12 (C) The bone evaluation indexes BMD and BV / TV of different experimental groups were also quantitatively analyzed to determine the specific bone tissue repair status. Among them, the BMD values ​​of GO-TAPP@CaP / CS scaffolds were 0.30 ± 0.0047, 0.43 ± 0.0027 and 0.61 ± 0.0076 at 4, 8 and 12 weeks, respectively (compared with the BMD values ​​of the single chitosan scaffold control group, which were 0.21 ± 0.0045, 0.29 ± 0.0096 and 0.36 ± 0.0103, respectively). The BMD values ​​of GO-TAPP / CS scaffolds were 0.24 ± 0.0054, 0.32 ± 0.0048 and 0.43 ± 0.0006 at 4, 8 and 12 weeks, respectively. The BMD values ​​of the CaP / CS scaffolds were 0.28 ± 0.0072, 0.36 ± 0.0075, and 0.49 ± 0.0041 at weeks 4, 8, and 12, respectively. The BV / TV percentages of the GO-TAPP@CaP / CS scaffolds were 18.52 ± 1.19%, 26.28 ± 0.39%, and 52.16 ± 1.76% at weeks 4, 8, and 12, respectively (compared to 6.55 ± 0.49%, 9.96 ± 0.07%, and 15.24 ± 0.2% for the chitosan scaffold control group, respectively). The BV / TV percentages of the GO-TAPP / CS scaffolds were 10.76 ± 0.36%, 15.73 ± 0.56%, and 27.92 ± 0.79% at weeks 4, 8, and 12, respectively. At weeks 4, 8, and 12, the BV / TV percentages of the CaP / CS scaffolds were 16.02 ± 0.81%, 20.18 ± 0.18%, and 40.88 ± 1.79%, respectively. The reason why the GO-TAPP@CaP / CS scaffold can promote bone repair well may be that GO-TAPP itself has a microporous structure, which can provide a good growth environment for osteoblasts and promote cell proliferation and migration. CaP is the most basic bone, which provides the basis for new bone formation.

[0105] Fig.13 The weight changes of rats in different groups at 4, 8 and 12 weeks. Compared with the control group, the weight of each experimental group had no significant change, indicating that each group had good in vivo biocompatibility.

[0106] (3) Histomorphological analysis:

[0107] Embedded sections: Cut tissues (including heart, liver, spleen, lungs, and kidneys) and the entire skull into 1 cm sections. 3, and fixed in paraformaldehyde for 1 day. The skull was then decalcified, and the fixed tissue and decalcified skull were dehydrated in ethanol gradient. After that, they were immersed in 60 ℃ wax liquid for 2 h, and the fixed tissue and skull were placed in a mold, and then liquid paraffin was added to it and embedded on a -28 ℃ freezing table. The embedded wax block was cut into 4 μm thick slices using a microtome, and spread on a glass slide to dry for later use.

[0108] H&E staining: After the tissue and skull sections are intermittently soaked in xylene and methanol, they are then soaked in distilled water, hematoxylin, distilled water, eosin, and distilled water in order, and finally soaked in methanol and xylene. After drying, add neutral resin, cover the slide with a coverslip, and dry the resin. After H&E staining is completed, it can be observed and photographed under a microscope.

[0109] Masson staining: Skull sections are stained with Weigert iron hematoxylin staining solution, then washed and stained with Masson blue solution, then washed and stained with Lichunhong acid fuchsin, then washed and dehydrated and transparentized with methanol and xylene. After drying, neutral resin is added, and the resin is dried after sealing with a coverslip. After Masson staining is completed, it can be observed and photographed under a microscope.

[0110] H&E and Masson staining were used to further evaluate the bone repair effect of GO-TAPP@CaP / CS scaffolds in vivo ( Fig.14 The results were consistent with those of micro-CT, that is, at the 4th week of implantation, except for the control group, all experimental groups had different degrees of new bone formation, among which the new bone formation in the GO-TAPP@CaP / CS group was the most obvious. At the 8th and 12th weeks of implantation, although all groups had different degrees of new bone formation, the degree of new bone formation in the GO-TAPP@CaP / CS group was significantly higher than that in the GO-TAPP / CS group and the CaP / CS group.

[0111] To evaluate the biosafety of GO-TAPP@CaP / CS scaffolds in vivo, organ tissue staining (H&E) and blood routine analysis ( Fig.15 and 16 ). The results showed that compared with the control group, no obvious histomorphological damage was found in the organs of each group. In addition, compared with the control group, the blood routine analysis results of different experimental groups were all within the safe range. The in vivo biocompatibility study of the GO-TAPP@CaP / CS scaffold demonstrated its good biosafety and its potential as an alternative bone transplant material.

[0112] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. Application of graphene oxide-based calcium phosphate composite materials in the preparation of drugs for promoting osteogenic differentiation of stem cells or in the preparation of bone repair scaffolds, characterized in that: The graphene oxide-based calcium phosphate composite material is a graphene oxide-porphyrin three-dimensional porous material loaded with calcium phosphate; the graphene oxide-based calcium phosphate composite material is a composite three-dimensional graphene-based biomaterial with a hierarchical pore structure, i.e., micropores to macropores; The graphene oxide-based calcium phosphate composite material is prepared by the following method: (1) Add 5,10,15,20-tetrakis(4-ethynylphenyl)-porphyrin, bis(triphenylphosphine)palladium chloride and cuprous iodide to tetrahydrofuran and mix them evenly in the dark, then add graphene oxide and triethylamine, mix them in the dark, and then let them stand to react to obtain a black solid, which is then washed and dried to obtain a graphene oxide-porphyrin three-dimensional porous material; (2) The graphene oxide-porphyrin three-dimensional porous material is mixed with calcium chloride, and then disodium hydrogen phosphate is added to react to obtain a graphene oxide-based calcium phosphate composite material.

2. The use according to claim 1, characterized in that: In step (1), the ratio of the added amounts of 5,10,15,20-tetrakis(4-ethynylphenyl)-porphyrin, graphene oxide, bis(triphenylphosphine)palladium chloride, cuprous iodide, triethylamine and tetrahydrofuran is 31 mg: 31 mg: 2.8 mg: 0.8 mg: 34 μL: 2 mL.

3. The use according to claim 1, characterized in that: In step (1), the temperature of the static reaction is 25° C. and the time of the static reaction is 48 h.

4. The use according to claim 1, characterized in that: In step (2), the mass ratio of the graphene oxide-porphyrin three-dimensional porous material to the calcium phosphate contained in the graphene oxide-based calcium phosphate composite material is 1:1-5; the mass ratio of the calcium chloride to disodium hydrogen phosphate is 55.5:61.

0.

5. The use according to claim 1, characterized in that: In step (2), the reaction temperature is 37° C. and the reaction time is 12 h.

6. A bone repair scaffold, characterized in that: The bone repair scaffold is prepared by the following method: Deacetylated chitosan is dissolved in an acetic acid solution to obtain a chitosan solution, the graphene oxide-based calcium phosphate composite material described in any one of claims 1 to 5 is added and mixed, and then freeze-dried to obtain a graphene oxide porphyrin-supported calcium phosphate chitosan composite scaffold.

7. The bone repair scaffold according to claim 6, characterized in that: The concentration of the chitosan solution is 0.02 g / mL; the mass concentration of the acetic acid solution is 1%.

8. The bone repair scaffold according to claim 6, characterized in that: The mass ratio of the deacetylated chitosan to the graphene oxide-based calcium phosphate composite material is 1000:6.0.