Method for separating and purifying lead-containing slag as a resource
Through the process of pickling and pH adjustment of lead-containing slag, high-grade lead ore and medium-grade rare earth ore were successfully separated, and high-purity lead oxide was obtained through roasting, which solved the problems of resource waste and environmental pollution and realized the development of lead resources. Closed-loop recycling and efficient extraction of rare earths.
Patent Information
- Application Number
- CN202411069139.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing technology has problems of resource waste and environmental pollution when processing lead-containing slag. In particular, the sulfur dioxide/sulfur trioxide waste gas generated during the roasting process causes acid rain, and the rare earth resources are not completely recovered, which increases the processing cost.
By adding water to the lead-containing slag, adding hydrochloric acid for solid-liquid separation, adjusting the pH value to separate high-grade lead ore and medium-grade rare earth ore, and then roasting to obtain high-purity lead oxide, achieving closed-loop recovery of lead resources and high efficiency of rare earths. extract.
It achieves zero-emission lead resource recovery, increases the rare earth recovery rate, reduces processing costs, and converts lead resources into high-purity lead oxide, reducing the amount of solid waste treatment.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of recycling and reusing lead-containing slag, and in particular relates to a method for separating and purifying the lead-containing slag as a resource. Background Art
[0002] During the wet smelting process of rare earth concentrate, there are two steps in the rare earth chloride impurity removal stage. The first step is to adjust the pH to remove fluorine and phosphorus, and the second step is to remove lead by adding alkali sulfide. The second step of lead removal will produce a large amount of lead-containing slag. The main component of the lead-containing slag is lead sulfide, which is mixed with a small amount of rare earth sulfide, trace amounts of rare earth sulfate, and calcium salt precipitates (calcium fluoride, calcium phosphate, calcium sulfate).
[0003] At present, the conventional treatment method for lead-containing slag is to extract rare earth resources through acid washing, and then sell the remaining lead-containing slag to related industries for treatment as solid hazardous waste. This treatment method will cause a large amount of lead resources in lead-containing slag to be wasted, and at the same time impose a serious burden on the cost of rare earth extraction.
[0004] Lead is a corrosion-resistant heavy nonferrous metal material. Due to its low melting point, corrosion resistance, plasticity, and radiation isolation properties, it is widely used in chemical, cable, battery, radioactive protection and other industrial sectors, and has great application value. The smelting raw material of lead is lead ore mainly composed of lead oxide. The higher the grade of the lead ore, the higher its value.
[0005] CN103572064A discloses a method for enriching lead and recovering rare earth from rare earth lead slag, comprising the following steps: roasting rare earth lead slag obtained by precipitating rare earth with sodium sulfide at 750-850°C; adding sulfuric acid to the roasted rare earth lead slag, leaching at 80-90°C; separating the treated product into solid and liquid, extracting rare earth from the supernatant after alkali conversion and acid dissolution; washing the solid to obtain a lead enrichment, which greatly reduces the difficulty and cost of treating lead-containing wastes, and can extract 40% of the rare earth contained in the lead slag. However, in the process of roasting rare earth lead slag obtained by precipitating rare earth with sodium sulfide, due to the shortcomings of the sulfide itself, the method will produce a large amount of sulfur dioxide / sulfur trioxide waste gas during roasting and heating, polluting the atmosphere and causing acid rain. It is difficult for conventional absorption tower spraying to achieve pollution-free emission of flue gas, so a large amount of lime is required for adsorption, and a large amount of solid waste will be generated accordingly.
[0006] CN115058608A discloses a method for recovering rare earth from rare earth lead-zinc sulfide slag, wherein the rare earth lead-zinc sulfide slag is beaten with clean water, hydrochloric acid is added and the temperature is raised for washing, and weak acid washing is performed to recover the rare earth, and the pH of the rare earth lead-zinc sulfide slag is controlled at a certain temperature, while the rare earth hydroxide is dissolved, the generation of hydrogen sulfide is reduced, and the impurity lead and zinc are avoided from being dissolved, and finally the rare earth attached to the lead-zinc sulfide slag is recovered using weak acid washing water, and more than 90% of the rare earth can be recovered. This recovery method has good controllability, low cost, and high resource utilization rate, but the disadvantage of this process is that the slag still contains 10% of the remaining rare earth resources after hydrochloric acid weak acid washing, and there is an incomplete recovery of rare earth resources, and due to the presence of rare earth, the remaining rare earth-containing lead slag is an irrecoverable hazardous waste, and the lead resources cannot be recovered, there is a waste of resources, and the processing cost and production cost of the enterprise are greatly increased. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for separating and purifying lead-containing slag for resource utilization, thereby obtaining three types of products, namely high-purity lead oxide, high-grade lead ore and medium-grade rare earth, and achieving the goal of zero heavy metal lead solid waste emission.
[0008] The method for resource separation and purification of lead-containing slag of the present invention comprises the following steps: first, adding water to the lead-containing slag, beating the slurry, adding hydrochloric acid to the obtained slurry, performing solid-liquid separation, and obtaining high-grade lead ore and supernatant A; then, adjusting the pH of the supernatant A to 2-2.5, heating to 40°C-60°C, preferably 45°C-55°C, mixing evenly, and continuing to adjust the pH to 6.5-7, and obtaining medium-grade rare earth ore and supernatant B after separation; finally, maintaining the temperature of the supernatant B at 45°C-65°C, adjusting the pH to 10-13, washing the obtained precipitate, and then roasting to obtain high-purity lead oxide.
[0009] The lead-containing slag has a lead content of 8%-17%, a rare earth content of 20%-40%, a calcium content of 0.5%-1.5%, a sodium content of 1%-1.5%, a phosphate content of 0.1%-0.5%, and the balance is water.
[0010] The performance indicators of the high-grade lead ore are: lead content>35%, rare earth content≤0.3%, and calcium content<0.15%; the performance indicators of the medium-grade rare earth ore are: rare earth content>40%, lead content=3.5%-4.5%; the performance indicator of high-purity lead oxide is lead content≥99%.
[0011] After adding hydrochloric acid to the slurry, the residual acidity (in terms of H +concentration meter) is 0.35mol / L-1mol / L, the insulation temperature is controlled at 58℃-85℃, and stirred for 15min-45min.
[0012] After solid-liquid separation, the solid is first washed with a hydrochloric acid solution and then washed with pure water, and the pH of the hydrochloric acid solution is 0.5-1.
[0013] The number of pure water washings is 2-4 times.
[0014] The pH is adjusted to 6.5-7 and then stirred for 10-20 minutes. The regulator used is a sodium hydroxide solution or a potassium hydroxide solution with a mass concentration of 1%-10%, and a more preferred range is a sodium hydroxide solution of 3%-5%.
[0015] The pH is adjusted to 10-13 by adding 5%-10% carbonate or bicarbonate solution, preferably sodium carbonate solution, to the supernatant B at a rate of 0.25-2.25 drops / second. All soluble carbonates / bicarbonates (excluding ammonium salts in this system, which will react and reduce the lead recovery rate). 2 drops / second is equivalent to 1 mL / min.
[0016] The end point of the washing is when the conductivity of the washing liquid becomes 1-20 μs / cm.
[0017] The calcination temperature is 700° C.-900° C., and the calcination time is 4 h.-15 h.
[0018] The zero discharge of heavy metal lead solid waste described in the present invention means that: the present invention recycles lead resources, and the supernatant containing lead <1ppm finally enters the rare earth extraction stage and is used as washing water. As the rare earth production reaches the lead slag discharge stage, it will be extracted again by this process, completing the closed-loop production in sequence, and achieving zero discharge of heavy metal lead.
[0019] Specifically, the method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0020] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to slurry, add hydrochloric acid to the obtained slurry to adjust the acidity to above 0.5mol / L (acid-base titration test value), raise the temperature to 58℃-85℃, and keep stirring for 15min-45min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L-1mol / L, and the suspension is filtered with a suction filtration bottle and a Buchner funnel. The solid is washed 3-5 times, and the first time is washed with 50mL of hydrochloric acid solution with pH=0.5-1, and the next 2-4 times are washed with 100mL of pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle.
[0021] (2) While stirring, add a 30% sodium hydroxide solution dropwise to the supernatant A, gradually adjust the acidity to pH = 2-2.5, raise the temperature to 40°C-60°C, mix evenly, and continue to use a 1%-10% sodium hydroxide solution to adjust the pH to 6.5-7, then stir for 10min-20min, during which time a white flocculent precipitate appears, and a gray precipitate appears when the pH approaches 7. During the stirring time, the pH is maintained at 6.5-7, and low-concentration hydrochloric acid or sodium hydroxide solution is used to fine-tune the pH stability. Filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B; low-concentration hydrochloric acid or sodium hydroxide solution refers to a 0.5%-10% mass concentration.
[0022] (3) The supernatant B is heated to 45°C-65°C while stirring, and a 5%-10% sodium carbonate solution is added dropwise at a rate of 0.25-2.25 drops / second (this dropping method can obtain a lead carbonate precipitate with excellent precipitation effect and easy to filter). The pH is adjusted to 10-13, and a white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, using 100 mL each time until the conductivity of the washing liquid is 1-20 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C-900°C for 4h-15h to obtain a black substance, i.e., high-purity lead oxide.
[0023] According to the method of the present invention, in the steps provided, the conditions in step (1) are explored, 500g of lead-containing slag is used as the initial reactant, after being slurried with water, the acidity is adjusted by adding hydrochloric acid at room temperature, and stirred for 5 minutes, and the rare earth content and calcium content in the filter cake (unwashed) are detected at various acidities, and the optimal residual acidity is determined by selecting the residual acidity with the lowest rare earth content in the filter cake at the lowest acidity (saving hydrochloric acid). When the residual acidity is 0.35-1.0 mol / L, the rare earth content in the filter cake before washing is 0.572%-0.592%, and the calcium content in the filter cake is 0.433%-0.457%, and the rare earth and calcium levels in the filter cake are low; when the residual acidity is below 0.34 mol / L, the rare earth content in the filter cake is 0.842%-3.34%, and the calcium content in the filter cake is 0.542%-0.847%, and the rare earth content and calcium content in the filter cake are at a relatively high level.
[0024] 500g of lead-containing slag was used as the initial reactant. After being slurried with water, hydrochloric acid was added to adjust the residual acidity to 0.35mol / L, the reaction temperature was controlled, and the mixture was stirred for 5 minutes at a constant temperature. The rare earth content and calcium content (unwashed) in the filter cake were detected at various temperatures. The optimal reaction temperature was determined by selecting the temperature when the rare earth content of the filter cake was the lowest. At 58℃-85℃, the rare earth content of the filter cake before washing was 0.356-0.399%, and the calcium content was 0.216-0.271%. When the temperature dropped to room temperature -57℃, the rare earth content of the filter cake before washing was 0.432-0.565%, and the calcium content was 0.252-0.516%.
[0025] 500 g of lead-containing slag is used as the initial reactant. After slurrying with water, hydrochloric acid is added to adjust the residual acidity to 0.35 mol / L, the reaction temperature is controlled to 60°C, the heat preservation and stirring time is controlled to 15 minutes, and the filter cake is washed twice. The washing medium (hydrochloric acid solution with a pH of 0.5-1, pure water) is controlled when the reaction is completed and filtered. The optimal washing method is determined by detecting the rare earth content and calcium content in the filter cake at each time. When hydrochloric acid is used for both washings, the rare earth content of the filter cake is 0.299%, and the calcium content is 0.195%; when pure water is used for both washings, the rare earth content of the filter cake is 0.367%, and the calcium content is 0.237%; when pure water is used first and then hydrochloric acid is used, the rare earth content of the filter cake is 0.303%, and the calcium content is 0.189%; and in the present invention, after hydrochloric acid is first used and then pure water is used for washing, the rare earth content of the filter cake is 0.281%, and the calcium content is 0.165%.
[0026] The supernatant A obtained after the first separation of the present invention has the following contents: rare earth content: 40-75g / L; lead content: 1600-3400ppm. The determined supernatant A has a rare earth content of 47g / L and a lead content of 1674ppm. Take the supernatant A after extracting high-grade lead ore as the raw material, take 5L, add 30% sodium hydroxide solution, adjust the pH to 2-2.5, and continue to add 30% sodium hydroxide solution at room temperature. By controlling the endpoint pH, the rare earth ion and lead ion content in the supernatant at each gradient endpoint pH, as well as the lead content and rare earth content of the filter cake are detected. The optimum precipitation pH is selected when the rare earth ion content in the supernatant is the lowest and the lead content is the highest, and the rare earth content and lead content in the filter cake are the highest. If both cannot be taken into account at the same time, the supernatant result is used as the main optimal condition indicator. When the endpoint pH is 6.5, the rare earth ion content in the supernatant is the highest and the lead content in the filter cake is the lowest. The rare earth content in the supernatant was 0.0007 g / L and the lead content was 1290 ppm. When the endpoint pH was 7, the rare earth content in the supernatant was 0.004 g / L and the lead content was 1176 ppm. The rare earth and lead contents in the medium-grade rare earth ore finally obtained in the above two ranges both met the performance indicators. When the endpoint pH was 7.5, the rare earth content in the supernatant was 0.001 g / L and the lead content was 720 ppm. The lead content in the medium-grade rare earth ore finally obtained was unqualified. When the endpoint pH was 6, the rare earth content in the supernatant was 2.4 g / L and the lead content was 1580 ppm. The rare earth and lead contents in the medium-grade rare earth ore finally obtained did not meet the performance indicators.
[0027] The supernatant B after extracting the medium-grade rare earth ore: the lead content is 1000-1500ppm. The supernatant B in this experiment: the lead content is 1165ppm. The mass concentration of sodium carbonate is above 10%, which makes the Tsinghua mine difficult to filtrate. It is relatively difficult at 15%, and it is difficult to extract after reaching 20%. The supernatant after extracting the medium-grade rare earth ore is used as the raw material for extracting high-purity lead oxide. Take 20L of the supernatant, 10% sodium carbonate solution as the precipitant, under stirring, by controlling the reaction temperature as a gradient, the end point pH=10, and determine the optimal reaction temperature according to the lead content in the supernatant and the difficulty of filtration of the filter cake. Under the precipitation of sodium carbonate, the lead content of the supernatant will show a trend of first decreasing and then increasing as the temperature rises. Therefore, the optimal condition should be the lowest temperature range of the supernatant, that is, 45℃-65℃. The washed filter cake to be calcined is used as the raw material, the temperature gradient is controlled, the insulation time is 15 hours, and the purity of the obtained high-purity lead oxide is detected to select the optimal calcination temperature. When the calcination temperature is 700°C-900°C, the purity of the calcined lead oxide can reach more than 99.0%, and when the calcination temperature is 650°C, the purity of the calcined lead oxide is 98.4%. As the temperature decreases, the purity continues to decrease. When the calcination temperature is 1000°C, the purity of the recovered lead oxide after calcination is 97.86%, which is relatively low.
[0028] The lead-containing slag treated by the present invention is mainly a mixture of lead sulfide, rare earth sulfide, lead sulfate and other trace impurities of miscellaneous salts, wherein under certain acidity conditions, rare earth sulfide and trace impurity salts can be dissolved in a solution, and the corresponding lead sulfide is affected by concentration and only slightly dissolved, and most of it is solid crystallized, so that high-grade lead ore (lead sulfide / galena) can be separated; the supernatant after extracting the high-grade lead ore (lead sulfide / galena) contains lead ions, rare earth ions, sulfur ions and hydrogen ions, and different precipitant ions are selected according to their different precipitation pH values to achieve the separation of medium-grade rare earth ore and high-purity lead oxide; the pH value of all rare earth precipitation is 6.5, lead begins to precipitate at pH=7, and the precipitation amount is the largest at pH=10 (the precipitation degree is best at pH=8-9), lead sulfide dissolves when acid is added, and as the acidity increases and the solubility approaches saturation, it no longer dissolves; the precipitation pH difference between lead and rare earth is used to separate and extract rare earth ions and fluorine and phosphorus ions, so as to purify the lead source.
[0029] The invention adopts a step-by-step treatment process to sequentially carry out pickling of lead-containing slag to extract a high-grade lead ore intermediate, alkali precipitation to extract a mixture of rare earth and impurity calcium salt, precipitation to extract and recover a high-purity lead oxide intermediate, and roasting to prepare high-grade lead ore and high-purity lead oxide, thereby producing three products of high-grade lead ore, high-purity lead oxide and medium-grade rare earth ore.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] (1) Compared with the conventional chemical precipitation method for treating solid waste, the method for separating and purifying lead-containing slag of the present invention can recycle the lead resources of lead-containing ore for the purpose of resource recovery, and at the same time recover rare earth elements, taking rare earth recovery into consideration.
[0032] (2) The method for separating and purifying lead-containing slag as a resource of the present invention uses hydrochloric acid, liquid alkali and sodium carbonate as raw materials, and has a low treatment cost compared to solid waste treatment processes.
[0033] (3) The method for separating and purifying lead-containing slag as a resource of the present invention, wherein the alkaline wastewater after the purified material enters the rare earth washing process for washing operation, achieves zero discharge, does not cause environmental pollution, and the process is environmentally friendly. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with specific embodiments.
[0035] The raw materials and reagents used in the following examples and comparative examples are all normal commercially available products. The % content described below is all mass content. Normal room temperature refers to 20°C-25°C, and the room temperature in the present invention is within this range. The values for adjusting pH in the embodiments do not need to be recorded one by one, only a range needs to be controlled, and after the final regulator is added, it is within the required range. Therefore, except for specific instructions, all others are controlled within the range.
[0036] The performance of the three products recovered in the embodiment meets the following indicators: the performance indicators of high-grade lead ore are: lead content>35%, rare earth content≤0.3%, calcium content<0.15%; the performance indicators of medium-grade rare earth ore are: rare earth content>40%, lead content=3.5%-4.5%; the performance indicator of high-purity lead oxide is lead content≥99%.
[0037] Example 1
[0038] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance is water.
[0039] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0040] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0041] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 50°C, mix evenly, continue to adjust the pH to 6.5-7 with 3% sodium hydroxide solution, stir for 10 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, and filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0042] (3) The supernatant B is heated to 50°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 0.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 10 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 10 hours to obtain a black substance, i.e., high-purity lead oxide.
[0043] Example 2
[0044] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance is water.
[0045] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0046] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 65℃, and keep stirring for 25min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.5mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0047] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 60°C, mix evenly, continue to adjust the pH to 6.5-7 with 5% sodium hydroxide solution, stir for 15 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0048] (3) The supernatant B is heated to 55°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 0.5 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 5 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 800°C for 6 hours to obtain a black substance, i.e., high-purity lead oxide.
[0049] Example 3
[0050] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance is water.
[0051] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0052] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 58℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.7mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid 4 times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next 3 times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0053] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 60°C, mix evenly, continue to use 8% sodium hydroxide solution to adjust the pH to 6.5-7, and stir for 20 minutes. During this period, white flocculent precipitate appears. When the pH is close to 7, gray precipitate appears. During the stirring time, the pH is maintained at 6.5-7. Filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0054] (3) The supernatant B is heated to 45°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 1.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 1 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 900°C for 4 hours to obtain a black substance, i.e., high-purity lead oxide.
[0055] Example 4
[0056] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance is water.
[0057] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0058] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 85℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 1mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0059] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 40°C, mix evenly, continue to adjust the pH to 6.5-7 with 1% sodium hydroxide solution, stir for 10 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0060] (3) The supernatant B is heated to 65°C while stirring, and a 6% sodium carbonate solution is added dropwise at a rate of 1.75 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 15 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 15 hours to obtain a black substance, i.e., high-purity lead oxide.
[0061] Example 5
[0062] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance is water.
[0063] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0064] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 58℃, and keep stirring for 45min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H +concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid 5 times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next 4 times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0065] (2) Add 30 wt% of liquid sodium hydroxide dropwise to the supernatant A under stirring, gradually adjust the acidity to pH = 2-2.5, raise the temperature to 55°C, mix evenly, continue to use 10% potassium hydroxide solution to adjust the pH to 6.5-7, and stir for 10 minutes. During this period, a white flocculent precipitate appears. When the pH is close to 7, a gray precipitate appears. During the stirring time, the pH is maintained at 6.5-7. Filter the suspension to obtain a solid filter cake, i.e., a medium-grade rare earth ore, and the supernatant B;
[0066] (3) The supernatant B is heated to 60°C while stirring, and 10% sodium carbonate solution is added dropwise at a rate of 2 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 20 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 15 hours to obtain a black substance, i.e., high-purity lead oxide.
[0067] Example 6
[0068] The lead-containing slag of this embodiment has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.43%, and the balance is water.
[0069] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0070] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 45min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid 5 times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next 4 times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0071] (2) While stirring, add 30 wt% of liquid sodium hydroxide dropwise to the supernatant A, gradually adjust the acidity to pH = 2-2.5, raise the temperature to 55°C, mix evenly, and continue to use 5% sodium hydroxide solution to adjust the pH to 6.5-7. Stir for 10 minutes, during which white flocculent precipitate appears. When the pH approaches 7, a gray precipitate appears. The pH is maintained at 6.5-7 during the stirring time. Filter the suspension to obtain a solid filter cake, i.e., a medium-grade rare earth ore, and supernatant B.
[0072] (3) The supernatant B is heated to 60°C while stirring, and 10% sodium bicarbonate solution is added dropwise at a rate of 2.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 10 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 15 hours to obtain a black substance, i.e., high-purity lead oxide.
[0073] Example 7
[0074] The lead-containing slag of this embodiment has a lead content of 8.2%, a rare earth content of 39.4%, a calcium content of 0.52%, a sodium content of 1.2%, a phosphate content of 0.16%, and the balance is water.
[0075] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0076] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0077] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 50°C, mix evenly, continue to adjust the pH to 6.5-7 with 3% sodium hydroxide solution, stir for 10 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, and filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0078] (3) The supernatant B is heated to 50°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 0.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 10 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 10 hours to obtain a black substance, i.e., high-purity lead oxide.
[0079] Example 8
[0080] The lead-containing slag of this embodiment has a lead content of 17%, a rare earth content of 20.4%, a calcium content of 1%, a sodium content of 1.1%, a phosphate content of 0.28%, and the remainder is water.
[0081] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0082] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0083] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 50°C, mix evenly, continue to adjust the pH to 6.5-7 with 3% sodium hydroxide solution, stir for 10 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, and filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0084] (3) The supernatant B is heated to 50°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 0.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 10 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 10 hours to obtain a black substance, i.e., high-purity lead oxide.
[0085] Example 9
[0086] The lead-containing slag of this embodiment has a lead content of 8.6%, a rare earth content of 38.7%, a calcium content of 1.5%, a sodium content of 1.5%, a phosphate content of 0.39%, and the remainder is water.
[0087] The method for separating and purifying the lead-containing slag as a resource comprises the following steps:
[0088] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 15min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid three times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next two times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle;
[0089] (2) Add 30% sodium hydroxide solution dropwise to the supernatant A under stirring, gradually adjust the acidity to pH=2-2.5, raise the temperature to 50°C, mix evenly, continue to adjust the pH to 6.5-7 with 3% sodium hydroxide solution, stir for 10 minutes, during which white flocculent precipitate appears, and gray precipitate appears when the pH approaches 7. Keep the pH at 6.5-7 during the stirring time, and filter the suspension to obtain a solid filter cake, i.e., medium-grade rare earth ore, and supernatant B;
[0090] (3) The supernatant B is heated to 50°C while stirring, and a 5% sodium carbonate solution is added dropwise at a rate of 0.25 drops / second to adjust the pH to 10-13. A white precipitate appears. The solid-liquid mixture is filtered and washed with pure water, 100 mL each time, until the conductivity of the washing liquid is 10 μs / cm, to obtain a relatively pure lead carbonate filter cake. The filter cake is calcined in a muffle furnace at 700°C for 10 hours to obtain a black substance, i.e., high-purity lead oxide.
[0091] Comparative Example 1
[0092] A method for separating and purifying lead-containing slag comprises the following steps:
[0093] The lead-containing slag of this comparative example has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance being water.
[0094] (1) Pulping of lead-containing slag: Take 2L of clean water in a 5L beaker, add 500g of rare earth lead-zinc slag, stir for 1 hour, and ensure that there are no undispersed particles in the beaker, that is, stir evenly.
[0095] (2) Add hydrochloric acid and heat to wash: After stirring evenly, start adding hydrochloric acid, control the flow rate at 500 ml / h, slowly add hydrochloric acid, and control the pH of the slurry in the tank to be ≥3.0.
[0096] (3) Continue to add hydrochloric acid until the pH in the beaker reaches 3.0. After stopping, continue stirring for 20 minutes. The pH does not change.
[0097] (4) Heat to 60°C. The pH continues to rise. Add hydrochloric acid again until the end point pH = 3.0 and no longer changes.
[0098] (5) Filter the suspension to separate the solid and liquid. The solid obtained is the solid waste lead slag, and the liquid is the recovered rare earth material.
[0099] Comparative Example 2
[0100] A method for separating and purifying lead-containing slag comprises the following steps:
[0101] The lead-containing slag of this comparative example has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance being water.
[0102] (1) Pulping of lead-containing slag: Take 4L of clean water in a 5L beaker, add 500g of rare earth lead-zinc slag, and stir until there are no undispersed particles in the beaker, that is, stir evenly.
[0103] (2) Raise the temperature to 65°C, keep stirring, and keep warm for 30 minutes.
[0104] (3) Filter the suspension to separate the solid and liquid, and the obtained liquid is the rare earth recovery supernatant A.
[0105] (4) Add 2 L of water to the solid obtained by filtration and wash it twice according to step (1).
[0106] (5) The suspension is filtered to separate the solid and liquid. The solid is the solid waste residue, and the supernatant liquid B is mixed with the supernatant liquid A to be the recovered rare earth resources.
[0107] Comparative Example 3
[0108] Comparative Example 3, if the present invention is used, alkaline wastewater will be generated, but if other extraction processes are used, no alkaline wastewater will be generated. Comparative Example 1 is the current workshop treatment process, and Comparative Example 2 is the earliest treatment process, and neither of them generates alkaline wastewater. Therefore, it is proposed to use the rare earth supernatant recovered in Comparative Example 1 as an indicator of lead content.
[0109] The lead-containing slag of this comparative example has a lead content of 15.7%, a rare earth content of 34.2%, a calcium content of 0.6%, a sodium content of 1.2%, a phosphate content of 0.34%, and the balance being water.
[0110] (1) Take 500g of lead-containing slag in a 3L beaker, add 200mL of clean water to make pulp, add hydrochloric acid to the obtained pulp to adjust the acidity to above 0.5mol / L (acid-base titration test value), heat to 60℃, and keep stirring for 45min; after stirring, a solid-liquid suspension is obtained, and the supernatant is taken to test the acidity to 0.35mol / L (residual acidity H + concentration meter), filter the suspension with a suction filtration bottle and a Buchner funnel, wash the solid 5 times, the first time with 50mL, pH = 0.5-1 hydrochloric acid solution, and the next 4 times with 100mL pure water to obtain a clean solid gray-black substance, which is dried to obtain a high-grade lead ore, as well as the supernatant A in the suction filtration bottle.
[0111] (2) The obtained supernatant A is used in the low-acid washing step to achieve the precipitation of liquid rare earths, and the residual lead supernatant is discharged to the environmental protection center for wastewater treatment.
[0112] The high-grade lead ore, medium-grade rare earth ore and high-purity lead oxide recovered in the above examples were subjected to purity testing, and the test results are shown in Table 1.
[0113] Calculation of lead resource yield = 1-(lead content of discharged supernatant × total amount of discharged supernatant) / (lead content of rare earth lead-containing slag × 500g);
[0114] Calculation of rare earth resource yield = (rare earth content in medium-grade rare earth ore × rare earth content) / (rare earth content in rare earth lead-containing slag × 500g).
[0115] The above two yield calculation methods are different. The rare earth resource yield calculation is mainly based on the rare earth content of the recovered medium-grade rare earth ore divided by the rare earth content of the experimental lead-containing slag. As for the lead resource recovery yield, because the produced medium-grade rare earth contains some lead, this part of the lead is separated and recovered again with the recovered rare earth resources to produce lead-containing slag. Therefore, the lead resource yield calculation is to first calculate the lead loss rate, that is, the lead content in the supernatant (0-2ppm) after the resources are recovered is divided by the lead content of the experimental lead-containing slag, and then the total amount is 1 minus the lead loss rate, which is the yield.
[0116] Table 1 Test results
[0117]
[0118] The rare earth yield of Comparative Example 1, Comparative Example 2 and Comparative Example 3 = rare earth supernatant concentration × rare earth supernatant volume / (mass of rare earth lead-containing slag × rare earth content of lead-containing slag), and the calculation results are shown in Table 2.
[0119] Comparative Examples 1, 2 and 3 adopt conventional rare earth lead slag treatment processes and do not recover lead resources.
[0120] The lead resource loss rate of the supernatant of Comparative Example 3 = lead content of supernatant A × mass of supernatant / (mass of rare earth lead-containing slag × rare earth content of lead-containing slag), that is, (1611ppm / 1000×675g / 1000) / (500×15.7%) = 1.39%.
[0121] Table 2 Recovery and elimination of the processes of Comparative Examples 1 to 3
[0122]
[0123] It can be seen from Tables 1 and 2 above that the present invention successfully separates the lead-containing rare earth slag into three products: high-purity lead oxide, high-grade lead oxide, and medium-grade recovered rare earth by subjecting the lead-containing slag produced in the rare earth concentrate smelting process to hot pickling of the material, extraction of rare earth by the primary filtrate, recovery of lead intermediates by the secondary filtrate, and production of lead oxide by roasting, thereby achieving the resource separation and purification of the lead-containing slag and achieving the purpose of zero heavy metal lead solid waste emission, thereby saving a large amount of solid waste treatment funds while turning waste into treasure and recycling resources.
Claims
1. A method for separating and purifying lead-containing slag as a resource, characterized in that: The following steps are involved: First, water is added to the lead-containing slag for pulping. After hydrochloric acid is added to the obtained pulp, the residual acidity is maintained at 0.35 mol / L-1 mol / L, the insulation temperature is controlled at 58°C-85°C, and the mixture is stirred for 15min-45min to separate the solid and liquid to obtain a high-grade lead ore and a supernatant A. Then, the supernatant A is adjusted to a pH of 2-2.5, heated to 40°C-60°C, mixed evenly, and then a sodium hydroxide solution or potassium hydroxide solution with a mass concentration of 1%-10% is used. The solution is adjusted to a pH of 6.5-7 and stirred for 10-20 minutes, and a medium-grade rare earth ore and a supernatant B are obtained after separation; finally, the supernatant B is kept at a temperature of 45°C-65°C, and a 5%-10% carbonate or bicarbonate solution is added to the supernatant B at a dropping speed of 0.25-2.25 drops / second, and the pH is adjusted to 10-13, and the obtained precipitate is washed, and then roasted at 700°C-900°C for 4h-15h to obtain high-purity lead oxide; The lead-containing slag has a lead content of 8%-17%, a rare earth content of 20%-40%, a calcium content of 0.5%-1.5%, a sodium content of 1%-1.5%, a phosphate content of 0.1%-0.5%, and the balance is water.
2. The method for separating and purifying lead-containing slag as claimed in claim 1, characterized in that: The performance indicators of the high-grade lead ore are: lead content>35%, rare earth content≤0.3%, and calcium content<0.15%; the performance indicators of the medium-grade rare earth ore are: rare earth content>40%, lead content=3.5%-4.5%; the performance indicator of high-purity lead oxide is lead content≥99%.
3. The method for separating and purifying lead-containing slag as claimed in claim 1, characterized in that: After solid-liquid separation, the solid is first washed with a hydrochloric acid solution and then washed with pure water, and the pH of the hydrochloric acid solution is 0.5-1.
4. The method for separating and purifying lead-containing slag as claimed in claim 3, characterized in that: The number of pure water washings is 2-4 times.
5. The method for separating and purifying lead-containing slag as claimed in claim 4, characterized in that: The end point of the washing is when the conductivity of the washing liquid becomes 1-20 μs / cm.
Citation Information
Patent Citations
Method for enriching lead and recovering rare earth from rare earth lead slag
CN103572064A
Technology of removing lead and recycling rare earth from saponified wastewater generated during process of rare earth extraction
CN105087964A
Method for recovering rare earth from rare earth lead and zinc sulfide residues
CN115058608A