Concrete and preparation method thereof, 3D printing material
By using solid waste-based mineral admixtures and composite fibers in 3D printed concrete, combined with manganese ions doping calcite-type nano-calcium carbonate, the problems of poor interlayer bonding and insufficient durability of existing 3D printed concrete are solved, achieving High-performance and environmentally friendly concrete materials.
Patent Information
- Application Number
- CN202411086572.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing 3D printed concrete has problems such as poor bonding between layers, insufficient strength and durability, and being unfriendly to the environment.
Solid waste-based mineral admixture, Portland cement, sulfoaluminate cement, quartz sand, expansion agent, early strength agent and silica fume are used as concrete base materials, and manganese ion-doped calcite type nano-calcium carbonate and composite are added. fiber, optimizing the composition and preparation methods of concrete to improve its structural stability and environmental protection.
It significantly improves the tensile strength, toughness and inter-layer bonding force of concrete, improves the strength and durability of 3D printed concrete, is suitable for construction and decoration fields, and achieves the dual goals of environmental benefits and resource utilization.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete materials, and in particular to concrete and a preparation method thereof, and 3D printing materials. Background Art
[0002] The concrete material used in the 3D printing concrete process is called 3D printed concrete or additively manufactured concrete. The 3D printing concrete process refers to the use of a 3D printer to print concrete materials so that the concrete materials are stacked layer by layer to accurately construct the desired shape and structure according to the electronic model.
[0003] 3D printing concrete technology can significantly reduce construction waste, improve material efficiency, shorten construction cycles, and achieve design diversity and innovation. However, the currently known 3D printing concrete still has the following problems: poor bonding between concrete layers, insufficient concrete strength and durability, and environmental unfriendliness. Summary of the invention
[0004] In view of this, the present invention provides a concrete and a preparation method thereof, and a 3D printing material. Specifically, the present invention includes the following technical solutions:
[0005] In one aspect, a concrete is provided, the concrete comprising a dry mix and water, wherein the mass ratio of the dry mix to the water is 2-5:1;
[0006] The dry mix comprises the following components in parts by weight: 10-20 parts of solid waste-based mineral admixture, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, 10-15 parts of silica fume and reinforcing additives;
[0007] The reinforcing additive comprises: at least one of 0.6-0.9 mass parts of manganese ion-doped calcite nano-calcium carbonate and 0.5-0.7 mass parts of composite fiber;
[0008] The composite fiber comprises: titanium dioxide nanofiber, PP fiber, aluminum oxide fiber and polyamide 66 fiber in a mass ratio of 1:5-10:5-10:8-15.
[0009] In some possible implementations, the solid waste-based mineral admixture includes a solid waste mixture and modified fly ash, and the mass ratio of the solid waste mixture to the modified fly ash is 2:3-10;
[0010] The solid waste mixture includes at least one of ceramic waste, slag, and autoclaved aerated concrete waste, and the particle size of the solid waste mixture is greater than or equal to 20 meshes.
[0011] In some possible implementations, the modified fly ash is prepared by mixing fly ash and an activated modifier and then ball milling, wherein the activated modifier includes sodium carbonate and sodium hydroxide in a mass ratio of 1:2-3.
[0012] In some possible implementations, the manganese ion-doped calcite-type nano-calcium carbonate is prepared by the following method:
[0013] Dissolving calcium nitrate and urea in deionized water at a molar ratio of 1:1-10, adding a manganese chloride solution while stirring to obtain a raw material solution, wherein the concentration of manganese chloride in the raw material solution is 0.1 mol / L-0.5 mol / L;
[0014] The pH value of the raw material solution is adjusted to 7-9, and transferred to a microwave digestion instrument for treatment;
[0015] After the treatment is completed, the treated product is centrifuged to obtain a precipitate, and the precipitate is washed to obtain the manganese ion-doped calcite nano-calcium carbonate.
[0016] In some possible implementations, the processing temperature of the microwave digestion instrument is 180° C.-250° C., and the processing time of the microwave digestion instrument is 1 hour-2 hours.
[0017] In some possible implementations, the titanium dioxide nanofibers are prepared by the following method: dissolving titanium phosphide in ethanol, using acetic acid as a chelating agent, and sequentially subjecting the mixture to electrospinning and calcining to prepare the titanium dioxide nanofibers;
[0018] Wherein, the calcination temperature is 800°C-1200°C, and the calcination time is 2 hours-4 hours.
[0019] In some possible implementations, the length of the titanium dioxide nanofiber is 300 nm-500 nm, and the lengths of the PP fiber, the alumina fiber, and the polyamide 66 fiber are each independently 3 mm-8 mm.
[0020] On the other hand, a method for preparing concrete is provided, wherein the concrete is as described above;
[0021] The method for preparing the concrete comprises:
[0022] Providing or preparing various components for constituting a dry blend, and uniformly mixing the various components to prepare the dry blend;
[0023] The dry mix is mixed with water to prepare the concrete.
[0024] On the other hand, a 3D printing material is provided, wherein the 3D printing material is prepared by a 3D printing process using any of the above-mentioned concretes.
[0025] The beneficial effects of the technical solution provided by the embodiment of the present invention include at least:
[0026] The concrete provided by the embodiment of the present invention has a dry mix comprising 10-20 parts of solid waste-based mineral admixtures, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, and 10-15 parts of silica fume. By using solid waste-based mineral admixtures, silicate cement, sulphoaluminate cement, quartz sand, expansion agent, early strength agent and silica fume as concrete base materials, it is beneficial to the structural stability, sustainability and green environmental protection of concrete products, thereby constructing high-performance concrete products based on solid waste resource utilization. In particular, the dry mix also includes reinforcing additives, and the reinforcing additives include: 0.6-0.9 parts by mass of manganese ion-doped calcite-type nano-calcium carbonate, 0.5-0.7 parts by mass of at least one of the composite fibers, and the composite fibers include: titanium dioxide nanofibers, PP fibers, alumina fibers, and polyamide 66 fibers with a mass ratio of 1:5-10:5-10:8-15. This helps increase the tensile strength, toughness and interlayer bonding of concrete, and is suitable for 3D printing applications in multiple fields such as construction, infrastructure, and decoration, and can improve the strength, interlayer bonding and durability of 3D printed concrete products. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] On the one hand, an embodiment of the present invention provides a concrete comprising a dry mix and water, wherein the mass ratio of the dry mix to water is 2-5:1, for example, including but not limited to: 2:1, 3:1, 4:1, 5:1, etc.
[0029] The dry mix includes the following components in parts by weight: 10-20 parts of solid waste-based mineral admixture, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, 10-15 parts of silica fume and reinforcing additives. The reinforcing additives include at least one of 0.6-0.9 parts by weight of manganese ion-doped calcite nano-calcium carbonate and 0.5-0.7 parts by weight of composite fibers. The composite fibers include titanium dioxide nanofibers, PP fibers, alumina fibers and polyamide 66 fibers in a mass ratio of 1:5-10:5-10:8-15.
[0030] One example is that the dry mix includes the following components in parts by mass: 10-20 parts of solid waste-based mineral admixture, 0.6-0.9 parts of manganese ion-doped calcite-type nano-calcium carbonate, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, and 10-15 parts of silica fume.
[0031] Another example is that the dry mix includes the following components in parts by weight: 10-20 parts of solid waste-based mineral admixture, 0.5-0.7 parts of composite fiber, 55-75 parts of Portland cement, 5-15 parts of sulfoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, and 10-15 parts of silica fume.
[0032] Another example is that the dry mix includes the following components in parts by mass: 10-20 parts of solid waste-based mineral admixture, 0.6-0.9 parts of manganese ion-doped calcite-type nano-calcium carbonate, 0.5-0.7 parts of composite fiber, 55-75 parts of silicate cement, 5-15 parts of sulfoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, and 10-15 parts of silica fume.
[0033] For example, the mass parts of solid waste-based mineral admixtures include but are not limited to: 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0034] The mass parts of manganese ion-doped calcite-type nano-calcium carbonate include but are not limited to: 0.6 parts, 0.7 parts, 0.8 parts, 0.9 parts, etc.
[0035] The mass proportion of the composite fiber includes, but is not limited to, 0.5, 0.6, 0.7, etc.
[0036] The mass parts of Portland cement include but are not limited to: 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts, 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, etc.
[0037] The mass parts of sulphoaluminate cement include but are not limited to: 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.
[0038] The mass parts of quartz sand include but are not limited to: 70 parts, 71 parts, 72 parts, 73 parts, 74 parts, 75 parts, 76 parts, 77 parts, 78 parts, 79 parts, 80 parts, 81 parts, 82 parts, 83 parts, 84 parts, 85 parts, 86 parts, 87 parts, 88 parts, 89 parts, 90 parts, 91 parts, 92 parts, 93 parts, 94 parts, 95 parts, 96 parts, 97 parts, 98 parts, 99 parts, 100 parts, etc.
[0039] The mass parts of the expansion agent include but are not limited to: 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.
[0040] The mass parts of the early strength agent include but are not limited to: 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 parts, etc.
[0041] The mass parts of silica ash include but are not limited to: 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.
[0042] The concrete provided in the embodiment of the present invention may be 3D printing concrete, which is suitable for preparing high-quality 3D printed products through a 3D printing process.
[0043] The concrete provided by the embodiment of the present invention has a dry mix comprising 10-20 parts of solid waste-based mineral admixtures, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, and 10-15 parts of silica fume. By using solid waste-based mineral admixtures, silicate cement, sulphoaluminate cement, quartz sand, expansion agent, early strength agent and silica fume as concrete base materials, it is beneficial to the structural stability, sustainability and green environmental protection of concrete products, thereby constructing high-performance concrete products based on solid waste resource utilization. In particular, the dry mix also includes reinforcing additives, and the reinforcing additives include: 0.6-0.9 parts by mass of manganese ion-doped calcite-type nano-calcium carbonate, 0.5-0.7 parts by mass of at least one of the composite fibers, and the composite fibers include: titanium dioxide nanofibers, PP fibers, alumina fibers, and polyamide 66 fibers with a mass ratio of 1:5-10:5-10:8-15. This helps increase the tensile strength, toughness and interlayer bonding of concrete, and is suitable for 3D printing applications in multiple fields such as construction, infrastructure, and decoration, and can improve the strength, interlayer bonding and durability of 3D printed concrete products.
[0044] In an embodiment of the present invention, the solid waste-based mineral admixture includes a solid waste mixture and modified fly ash, and the mass ratio of the solid waste mixture to the modified fly ash is 2:3-10, which includes but is not limited to: 2:3, 2:4, 2:5, 2:6, 2:7, 2:8, 2:9, 2:10, etc.
[0045] The solid waste mixture includes at least one of ceramic waste, slag, and autoclaved aerated concrete waste, and the particle size of the solid waste mixture is greater than or equal to 20 meshes.
[0046] In some examples, the solid waste-based mineral admixture is prepared by the following method: the solid waste mixture is washed to make its surface clean to remove impurities and harmful substances. Then, the washed solid waste is coarsely crushed by a crusher to break it into smaller blocks, and then the crushed waste is sent to a ball mill and finely ground by adding a grinding aid. The ground material is screened by a screening device to remove large particle size materials that do not meet the fineness requirements, thereby obtaining a solid waste mixture with a particle size greater than or equal to 20 mesh. The solid waste mixture is evenly mixed with fly ash in a mass ratio of 2: (3-10) to prepare a solid waste-based mineral admixture.
[0047] In some examples, the grinding aid is a mixture of sodium hexametaphosphate and sodium stearate in a mass ratio of 1:1 to obtain a better grinding effect.
[0048] In some examples, the modified fly ash is prepared by mixing fly ash and an activated modifier and then ball milling, wherein the activated modifier includes sodium carbonate and sodium hydroxide in a mass ratio of 1:2-3, for example, the mass ratio of sodium carbonate to sodium hydroxide can be 1:2. The modified fly ash is more beneficial for improving the compressive strength, tensile strength and tensile bond strength of concrete.
[0049] The fly ash used can be fly ash coarse ash from coal-fired power plants, the doping concentration of the activated modifier used can be 0.5%-3%, and the ball mill used can be a (φ2*9)m closed-circuit ball mill.
[0050] In some examples, the modified fly ash has a specific surface area of 500-1000m 2 / g.
[0051] In the embodiment of the present invention, by using manganese ions to dope calcite-type nano-calcium carbonate, it is beneficial to enhance the compressive properties and tensile bond strength (also known as tensile bond strength) of concrete. This is because manganese ions doped calcite-type nano-calcium carbonate generally have higher activity and specific surface area, so when it reacts with the hydration product of cement, it can form a denser gel structure, thereby enhancing the durability of concrete and interlayer bonding strength.
[0052] Exemplarily, manganese ion-doped calcite nano-calcium carbonate is prepared by the following method: calcium nitrate and urea are dissolved in deionized water at a molar ratio of 1:1-10, and a manganese chloride solution is added while stirring to obtain a raw material solution, wherein the concentration of manganese chloride in the raw material solution is 0.1mol / L-0.5mol / L. The pH value of the raw material solution is adjusted to 7-9, and transferred to a microwave digestion instrument for treatment. After the treatment is completed, the treated product is centrifuged to obtain a precipitate, and the precipitate is washed to obtain manganese ion-doped calcite nano-calcium carbonate.
[0053] The molar ratio of calcium nitrate to urea includes, but is not limited to, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc. In some examples, the molar ratio of calcium nitrate to urea is 1:1-5.
[0054] Exemplarily, calcium nitrate and urea are dissolved in deionized water at a molar ratio of 1:1-10, stirred for 10-30 minutes, and manganese chloride solution is added while stirring to obtain a raw material solution, wherein the concentration of manganese chloride in the raw material solution is 0.1mol / L-0.5mol / L. The pH value of the raw material solution is adjusted to 7-9 using acetic acid, and transferred to a microwave digestion instrument for treatment. After the treatment is completed, it is cooled to room temperature, the treated product is taken out, the treated product is centrifuged to obtain a precipitate, and the precipitate is washed with deionized water and ethanol to remove unreacted substances and impurities on the surface to obtain manganese ion-doped calcite nano-calcium carbonate.
[0055] The concentration of manganese chloride in the raw material solution includes but is not limited to: 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, etc.
[0056] In some examples, the particle size of manganese ion-doped calcite nano-calcium carbonate is 300nm-500nm to optimize the performance of concrete.
[0057] In some examples, the processing temperature of the microwave digestion instrument is 180°C-250°C, including but not limited to 180°C, 190°C, and 200°C, and the processing time of the microwave digestion instrument is 1 hour-2 hours, so that the reaction of calcium nitrate, urea, and manganese chloride is more complete.
[0058] The manganese ion-doped calcite nano-calcium carbonate prepared by the above method is more beneficial for improving the compressive strength, tensile strength and tensile bond strength of concrete.
[0059] In the embodiment of the present invention, composite fibers are used, which is beneficial to enhancing the compressive and flexural properties of concrete. In the embodiment of the present invention, the composite fibers include: titanium dioxide nanofibers, PP fibers, alumina fibers, and polyamide 66 fibers in a mass ratio of 1:5-10:5-10:8-15. Among them, for alumina fibers, the fiber material contains aluminum oxide and silicon dioxide. For example, the mass ratio of aluminum oxide to silicon dioxide can be 2-3:1, for example, the mass percentage of aluminum oxide is 72%, and the mass percentage of silicon dioxide is 28%.
[0060] Among them, polyamide fiber and PP fiber are beneficial to enhancing the toughness of concrete, while titanium dioxide nanofiber and alumina fiber are beneficial to reinforcing and improving the wear resistance and high temperature resistance of concrete.
[0061] Exemplarily, the composite fiber can be prepared by the following method: titanium dioxide nanofibers, PP fibers, alumina fibers, and polyamide 66 fibers are mixed in a set mass ratio and placed in an ultrasonic cleaner for dispersion and cleaning for at least 24 hours, for example, 30 hours. After cleaning, the fibers are placed in a double-cone mixer for uniform mixing, and naturally dried to prepare the desired composite fiber.
[0062] In some examples, titanium dioxide nanofibers are prepared by the following method: dissolving titanium phosphide in ethanol, using acetic acid as a chelating agent, and sequentially subjecting the mixture to electrospinning and calcining to prepare titanium dioxide nanofibers, wherein the calcining temperature is 800°C-1200°C, and the calcining time is 2 hours-4 hours.
[0063] For example, during the electrospinning process, the rotation speed of the spinning machine may be 50 r / min-100 r / min, and the humidity of the electrospinning environment may be 45% and the temperature may be 25°C.
[0064] In some examples, the length of the titanium dioxide nanofibers is 300 nm-500 nm, and the lengths of the PP fibers, the alumina fibers, and the polyamide 66 fibers are each independently 3 mm-8 mm.
[0065] The composite fiber prepared by the above method is more beneficial for improving the compressive strength, flexural resistance and tensile bonding strength of concrete.
[0066] The expansion agent may be any expansion agent commonly used in the concrete field. In some examples, the expansion agent is selected from at least one of calcium sulfoaluminate-calcium oxide expansion agent and magnesium oxide expansion agent.
[0067] The early strength agent can be any early strength agent commonly used in the concrete field. In some examples, the early strength agent can be selected from calcium chloride early strength agent, sodium chloride early strength agent, gypsum early strength agent, sodium aluminate early strength agent, sodium carbonate early strength agent, calcium carbonate early strength agent, etc.
[0068] In summary, the concrete provided by the embodiment of the present invention may be 3D printed concrete, which has at least the following advantages:
[0069] (1) Significant environmental benefits: Using industrial solid waste, such as ceramic waste, fly ash, slag and autoclaved aerated concrete waste, as admixtures not only utilizes waste resources, reduces environmental pollution and land occupation, but also reduces dependence on raw materials.
[0070] (2) Improved mechanical properties and durability: The use of composite fibers enhances the crack resistance and impact resistance of concrete. Specifically, polyamide fibers and PP fibers provide good toughness, allowing concrete to better absorb energy when subjected to stress, thereby reducing the formation of cracks. This toughness helps to improve the tensile strength of concrete. In addition, PP fibers can also resist chemical corrosion, further improving the durability of concrete in chemical environments. Titanium dioxide nanofibers and chopped alumina fibers enhance wear resistance and high temperature resistance. These properties make concrete more suitable for complex and harsh use environments, such as high temperature, high strength and high wear environments, extending the service life of concrete products. In addition, the uniform distribution of the above-mentioned composite fibers in the concrete material also helps to control the extension of micro cracks in concrete, thereby improving the crack resistance of concrete products.
[0071] (3) Optimizing microstructure and improving density: By doping calcite nano-calcium carbonate with manganese ions, not only does the particle size of calcite nano-calcium carbonate become smaller, but the addition of manganese ions doped with calcite nano-calcium carbonate can effectively fill the micropores in the concrete, improve the material density, and reduce the porosity. In addition, manganese ions doped with calcite nano-calcium carbonate can also increase its specific surface area. A higher specific surface area means that more surfaces can contact with cement hydration products, thereby enhancing its bonding with the cement matrix in the concrete. Therefore, manganese ions doped with calcite nano-calcium carbonate can optimize its own microstructure and improve the density of concrete materials, which is beneficial to enhancing the strength (especially flexural strength), durability, water resistance and chemical corrosion resistance of concrete, and extending the service life of concrete structures.
[0072] (4) Promote cement hydration reaction: Manganese ions replace calcium ions in the calcium carbonate lattice, which can cause the distortion of the crystal structure, affect the growth and arrangement of the crystals, and ultimately increase the activity of nano-calcium carbonate. As a result, manganese ion-doped calcite nano-calcium carbonate exhibits higher reaction activity, adsorption activity and interfacial activity. The increase in reaction activity is conducive to the reaction of manganese ion-doped calcite nano-calcium carbonate with cement hydration products in concrete to form a more stable composite structure. The increase in adsorption activity is conducive to the manganese ion-doped calcite nano-calcium carbonate to adsorb more water or other reactants, which helps to improve the mixing and hardening process of concrete. The increase in interfacial activity is conducive to the manganese ion-doped calcite nano-calcium carbonate to better combine with other components in concrete. It can be seen that manganese ion-doped calcite nano-calcium carbonate has high activity, which can not only promote the hydration reaction of cement and improve the early strength of concrete (especially flexural strength), but also help improve the hardening of concrete and the combination of its components, thereby improving the interlayer bonding during 3D printing and ensuring the overall stability and bearing capacity of the 3D printed structure.
[0073] (5) Improving printing efficiency and reducing energy consumption: Optimized concrete material formulations and improved material properties, such as improved rheology and rapid curing capabilities, can improve the speed and efficiency of 3D printing and reduce energy consumption and production costs.
[0074] It can be seen that the concrete provided by the embodiment of the present invention not only exhibits excellent environmental friendliness and resource utilization efficiency, but also has high strength, high durability and good economy. The concrete is particularly suitable for the construction of prefabricated components and complex structures.
[0075] On the other hand, an embodiment of the present invention provides a method for preparing concrete, and the concrete is as described above. The method for preparing concrete comprises:
[0076] Provide or prepare various components for forming a dry mix, mix the various components evenly to prepare a dry mix, and mix the dry mix evenly with water to prepare concrete.
[0077] Among them, some components in the dry mix can be prepared in combination with the above-mentioned concrete scheme, which will not be described in detail here.
[0078] On the other hand, an embodiment of the present invention provides a 3D printing material, which is prepared by a 3D printing process using any of the above-mentioned concretes.
[0079] The 3D printing material provided by the embodiment of the present invention has all the advantages of the concrete mentioned above, which will not be described in detail here.
[0080] Exemplary embodiments of the present invention will be described in more detail below. Although exemplary embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. In the embodiments, if specific techniques or conditions are not specified, the techniques or conditions described in the literature in this area or the product specifications are followed. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be obtained commercially. In the following embodiments, the expansion agent can be a calcium sulphoaluminate-calcium oxide expansion agent, and the early strength agent can be a calcium chloride early strength agent.
[0081] Example 1
[0082] Example 1 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.5 parts of composite fiber, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0083] The concrete is prepared by the following method:
[0084] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 3%.
[0085] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:5 to prepare a solid waste-based mineral admixture.
[0086] Preparation of composite fibers: First, prepare titanium dioxide nanofibers: titanium phosphide, ethanol and acetic acid are mixed evenly in a molar ratio of 1:3:2, and heated at a speed of 100 rmin in an environment with a humidity of 45% and a temperature of 25°C. -1 The electrospinning machine was used for spinning, and then the spinning product was calcined at a high temperature of 1000°C for 2 hours to prepare titanium dioxide nanofibers. Titanium dioxide nanofibers: PP fiber: short-cut alumina fiber: polyamide 66 fiber were mixed in a mass ratio of 1:6:6:10 and placed in an ultrasonic cleaner for dispersion and cleaning for 30 hours, then placed in a double cone mixer for uniform mixing, and finally dried naturally to obtain composite fibers.
[0087] The components of the concrete were mixed according to a proportion and added into a V-type mixer, and premixed at a high speed for 30 minutes to obtain a dry mix; water and the dry mix were mixed according to a mass ratio and stirred evenly to prepare concrete.
[0088] Example 2
[0089] Example 2 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.6 parts of composite fiber, 60 parts of silicate cement, 5 parts of sulfoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0090] The concrete is prepared by the following method:
[0091] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 2%.
[0092] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:5 to prepare a solid waste-based mineral admixture.
[0093] Preparation of composite fibers: First, prepare titanium dioxide nanofibers: titanium phosphide, ethanol and acetic acid are mixed evenly in a molar ratio of 1:3:2, and heated at a speed of 100 rmin in an environment with a humidity of 45% and a temperature of 25°C. -1 The electrospinning machine was used for spinning, and then the spinning product was calcined at a high temperature of 1000°C for 2 hours to prepare titanium dioxide nanofibers. Titanium dioxide nanofibers: PP fiber: short-cut alumina fiber: polyamide 66 fiber were mixed in a mass ratio of 1:7:8:12 and placed in an ultrasonic cleaner for dispersion and cleaning for 30 hours, then placed in a double cone mixer for uniform mixing, and finally dried naturally to obtain composite fibers.
[0094] The components of the concrete were mixed according to a proportion and added into a V-type mixer, and premixed at a high speed for 30 minutes to obtain a dry mix; water and the dry mix were mixed according to a mass ratio and stirred evenly to prepare concrete.
[0095] Example 3
[0096] Example 3 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 15 parts of solid waste-based mineral admixture, 0.7 parts of composite fiber, 60 parts of silicate cement, 5 parts of sulfoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.5 parts of early strength agent, and 12 parts of silica fume.
[0097] The concrete is prepared by the following method:
[0098] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 2.5%.
[0099] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:5 to prepare a solid waste-based mineral admixture.
[0100] Preparation of composite fibers: First, prepare titanium dioxide nanofibers: titanium phosphide, ethanol and acetic acid are mixed evenly in a molar ratio of 1:3:2, and heated at a speed of 100 rmin in an environment with a humidity of 45% and a temperature of 25°C. -1 The electrospinning machine was used for spinning, and then the spinning product was calcined at a high temperature of 1000°C for 2 hours to prepare titanium dioxide nanofibers. Titanium dioxide nanofibers: PP fiber: short-cut alumina fiber: polyamide 66 fiber were mixed in a mass ratio of 1:6:8:12 and placed in an ultrasonic cleaner for dispersion and cleaning for 30 hours, then placed in a double cone mixer for uniform mixing, and finally dried naturally to obtain composite fibers.
[0101] The components of the concrete were mixed according to a proportion and added into a V-type mixer, and premixed at a high speed for 30 minutes to obtain a dry mix; water and the dry mix were mixed according to a mass ratio and stirred evenly to prepare concrete.
[0102] Example 4
[0103] Example 4 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.6 parts of manganese ion-doped calcite-type nano-calcium carbonate, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0104] The concrete is prepared by the following method:
[0105] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 1.8%.
[0106] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:6 to prepare a solid waste-based mineral admixture.
[0107] Preparation of manganese ion-doped calcite nano-calcium carbonate: Calcium nitrate and urea were dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and manganese chloride solution (to a concentration of 0.1 mol / L) was added while stirring. The pH value of the reaction solution was adjusted to 8 with acetic acid, and the reaction solution was transferred to a microwave digestion instrument. The reaction time was 1 hour at 200°C. After the reaction was completed, it was cooled to room temperature, and the microwave digestion instrument was opened to take out the reactants. The reactants were centrifuged to obtain a precipitate, and the precipitate was washed with deionized water and ethanol to remove the unreacted substances and impurities on the surface of the precipitate to obtain manganese ion-doped calcite nano-calcium carbonate.
[0108] The components of the concrete were mixed according to a proportion and added into a V-type mixer, and premixed at a high speed for 30 minutes to obtain a dry mix; water and the dry mix were mixed according to a mass ratio and stirred evenly to prepare concrete.
[0109] Example 5
[0110] Example 5 provides a concrete, including a dry mix and water in a mass ratio of 2:1; the dry mix includes the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.7 parts of manganese ion-doped calcite-type nano-calcium carbonate, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0111] The concrete is prepared by the following method:
[0112] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 3%.
[0113] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:6 to prepare a solid waste-based mineral admixture.
[0114] Preparation of manganese ion-doped calcite nano-calcium carbonate: Calcium nitrate and urea were dissolved in deionized water at a molar ratio of 1:3, stirred for 30 minutes, and manganese chloride solution (to a concentration of 0.1 mol / L) was added while stirring. The pH value of the reaction solution was adjusted to 8 with acetic acid, and the reaction solution was transferred to a microwave digestion instrument. The reaction time was 1 hour at 220°C. After the reaction was completed, it was cooled to room temperature, and the microwave digestion instrument was opened to take out the reactants. The reactants were centrifuged to obtain a precipitate, and the precipitate was washed with deionized water and ethanol to remove the unreacted substances and impurities on the surface of the precipitate to obtain manganese ion-doped calcite nano-calcium carbonate.
[0115] Example 6
[0116] Example 6 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.8 parts of manganese ion-doped calcite-type nano-calcium carbonate, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0117] The concrete is prepared by the following method:
[0118] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:4, and the mass percentage of the activated modifier is 3%.
[0119] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:6 to prepare a solid waste-based mineral admixture.
[0120] Preparation of manganese ion-doped calcite nano-calcium carbonate: Calcium nitrate and urea were dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and manganese chloride solution (to a concentration of 0.1 mol / L) was added while stirring. The pH value of the reaction solution was adjusted to 8 with acetic acid, and the reaction solution was transferred to a microwave digestion instrument. The reaction time was 2 hours at 210°C. After the reaction was completed, it was cooled to room temperature, and the microwave digestion instrument was opened to take out the reactants. The reactants were centrifuged to obtain a precipitate, and the precipitate was washed with deionized water and ethanol to remove the unreacted substances and impurities on the surface of the precipitate to obtain manganese ion-doped calcite nano-calcium carbonate.
[0121] Example 7
[0122] Example 7 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.9 parts of manganese ion-doped calcite-type nano-calcium carbonate, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0123] The concrete is prepared by the following method:
[0124] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 2.5%.
[0125] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:6 to prepare a solid waste-based mineral admixture.
[0126] Preparation of manganese ion-doped calcite nano-calcium carbonate: Calcium nitrate and urea were dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and manganese chloride solution (to a concentration of 0.1 mol / L) was added while stirring. The pH value of the reaction solution was adjusted to 8 with acetic acid, and the reaction solution was transferred to a microwave digestion instrument. The reaction time was 2 hours at 210°C. After the reaction was completed, it was cooled to room temperature, and the microwave digestion instrument was opened to take out the reactants. The reactants were centrifuged to obtain a precipitate, and the precipitate was washed with deionized water and ethanol to remove the unreacted substances and impurities on the surface of the precipitate to obtain manganese ion-doped calcite nano-calcium carbonate.
[0127] Example 8
[0128] Example 8 provides a concrete, including a dry mix and water in a mass ratio of 2:1; the dry mix includes the following components in mass parts: 12 parts of solid waste-based mineral admixture, 0.9 parts of manganese ion-doped calcite-type nano-calcium carbonate, 0.6 parts of composite fiber, 60 parts of silicate cement, 5 parts of sulfoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0129] The concrete is prepared by the following method:
[0130] Preparation of solid waste-based mineral admixtures: Coal-fired power plant fly ash coarse ash is mixed with an activated modifier and ground by a (φ2*9) m closed-circuit ball mill to prepare modified fly ash. The activated modifier is a mixture of sodium carbonate and sodium hydroxide in a mass ratio of 1:2, and the mass percentage of the activated modifier is 2%.
[0131] The surface of ceramic waste, slag and autoclaved aerated concrete waste is cleaned to remove impurities and harmful substances. The cleaned solid waste is roughly crushed by a crusher to smaller pieces. The crushed waste is sent to a ball mill, and abrasives (sodium hexametaphosphate and sodium stearate with a mass ratio of 1:1) are added for fine grinding. The ground powder is screened using a screening device to a particle size greater than or equal to 20 meshes, and finally mixed with a surface area of 1000m 2 / g of modified fly ash are uniformly mixed in a mass ratio of 2:6 to prepare a solid waste-based mineral admixture.
[0132] Preparation of manganese ion-doped calcite nano-calcium carbonate: Calcium nitrate and urea were dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and manganese chloride solution (to a concentration of 0.1 mol / L) was added while stirring. The pH value of the reaction solution was adjusted to 8 with acetic acid, and the reaction solution was transferred to a microwave digestion instrument. The reaction time was 2 hours at 210°C. After the reaction was completed, it was cooled to room temperature, and the microwave digestion instrument was opened to take out the reactants. The reactants were centrifuged to obtain a precipitate, and the precipitate was washed with deionized water and ethanol to remove the unreacted substances and impurities on the surface of the precipitate to obtain manganese ion-doped calcite nano-calcium carbonate.
[0133] Preparation of composite fibers: First, prepare titanium dioxide nanofibers: titanium phosphide, ethanol and acetic acid are mixed evenly in a molar ratio of 1:3:2, and heated at a speed of 100 rmin in an environment with a humidity of 45% and a temperature of 25°C. -1 The electrospinning machine was used for spinning, and then the spinning product was calcined at a high temperature of 1000°C for 2 hours to prepare titanium dioxide nanofibers. Titanium dioxide nanofibers: PP fiber: short-cut alumina fiber: polyamide 66 fiber were mixed in a mass ratio of 1:6:6:10 and placed in an ultrasonic cleaner for dispersion and cleaning for 30 hours, then placed in a double cone mixer for uniform mixing, and finally dried naturally to obtain composite fibers.
[0134] Comparative Example 1
[0135] Comparative Example 1 provides a concrete comprising a dry mix and water in a mass ratio of 2:1; the dry mix comprises the following components in mass parts: 12 parts of solid waste-based mineral admixture, 60 parts of silicate cement, 5 parts of sulphoaluminate cement, 80 parts of quartz sand, 5 parts of expansion agent, 0.4 parts of early strength agent, and 10 parts of silica fume.
[0136] The preparation method of the concrete can be found in Example 1, which will not be described in detail here.
[0137] Comparative Example 2
[0138] Comparative Example 2 provides a concrete, and its composition and preparation process can be referred to in Example 4. The difference between Comparative Example 2 and Example 4 is that a calcite-type nano-calcium carbonate without manganese ion doping is used, and the calcite-type nano-calcium carbonate is prepared by the following method: calcium nitrate (Ca(NO3)2) and urea (CH4N2O) are dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and the pH value of the reaction solution is adjusted to 8 with acetic acid, and the reaction solution is transferred to a microwave digestion instrument, and the reaction time is 1 hour at 200°C. After the reaction is completed, it is cooled to room temperature, and the microwave digestion instrument is opened to take out the reactant. The reactant is centrifuged to obtain a precipitate, and the precipitate is washed with deionized water and ethanol to remove unreacted substances and impurities on the surface of the precipitate to obtain calcite-type nano-calcium carbonate.
[0139] Comparative Example 3
[0140] Comparative Example 3 provides a concrete, and its composition and preparation process can be referred to in Example 6. The difference between Comparative Example 3 and Example 6 is that a calcite-type nano-calcium carbonate without manganese ion doping is used, and the calcite-type nano-calcium carbonate is prepared by the following method: calcium nitrate (Ca(NO3)2) and urea (CH4N2O) are dissolved in deionized water at a molar ratio of 1:2, stirred for 30 minutes, and the pH value of the reaction solution is adjusted to 8 with acetic acid, and the reaction solution is transferred to a microwave digestion instrument, and the reaction time is 1 hour at 200°C. After the reaction is completed, it is cooled to room temperature, and the microwave digestion instrument is opened to take out the reactant. The reactant is centrifuged to obtain a precipitate, and the precipitate is washed with deionized water and ethanol to remove unreacted substances and impurities on the surface of the precipitate to obtain calcite-type nano-calcium carbonate.
[0141] Test Case
[0142] The concrete prepared in each of the above embodiments was 3D printed using a 3D printer to obtain a 3D printed part, and the following properties of the 3D printed part were tested.
[0143] For the compression resistance test and flexural resistance test, the test methods respectively adopt the methods specified in GB / T50081-2019.
[0144] The tensile bond strength test was carried out according to JGJ / T70-2009 "Standard for Test Methods of Basic Properties of Building Mortar". The 3D printed parts were cut into test pieces with a size of 40mm×40mm×20mm, and then cured under standard conditions for 28 days before testing. The test results are shown in Table 1.
[0145]
[0146] From the test results of Examples 1-3 and Comparative Example 1 in Table 1, it can be seen that the addition of composite fibers significantly improves the flexural and compressive properties of concrete, especially the improvement in flexural properties is more significant. The reason is that polyamide fibers and PP fibers enhance the toughness of concrete, while titanium dioxide nanofibers and chopped alumina fibers improve the wear resistance and high temperature resistance of concrete.
[0147] From the test results of Examples 4-7 and Comparative Examples 1, 2 and 3 in Table 1, it can be seen that compared with the solution without adding any calcite nano-calcium carbonate and the solution without calcite nano-calcium carbonate doped with manganese ions, the addition of manganese ion-doped calcite nano-calcium carbonate effectively improves the compressive strength and tensile bond strength of concrete. This is because manganese ion-doped calcite nano-calcium carbonate has high activity and specific surface area, which can not only promote the reaction with the hydration products of cement, but also facilitate the formation of a denser gel structure, thereby enhancing the strength of concrete and interlayer bonding.
[0148] From the test results of Example 8 in Table 1, it can be seen that the composite fiber and manganese ion-doped calcite-type nano-calcium carbonate were added to the concrete at the same time, and the results showed that the compressive strength, flexural strength and interlayer bonding performance of the concrete were significantly improved.
[0149] The above description is only for the purpose of facilitating those skilled in the art to understand the technical solution of the present invention and is not intended to limit the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A concrete, characterized in that: The concrete comprises a dry mix and water, wherein the mass ratio of the dry mix to the water is 2-5:1; The dry mix comprises the following components in parts by weight: 10-20 parts of solid waste-based mineral admixture, 55-75 parts of silicate cement, 5-15 parts of sulphoaluminate cement, 70-100 parts of quartz sand, 5-15 parts of expansion agent, 0.4-0.8 parts of early strength agent, 10-15 parts of silica fume and reinforcing additives; The reinforcing additive comprises: 0.6-0.9 parts by mass of manganese ion-doped calcite nano-calcium carbonate, or the reinforcing additive comprises: 0.6-0.9 parts by mass of manganese ion-doped calcite nano-calcium carbonate and 0.5-0.7 parts by mass of composite fiber; The composite fiber comprises: titanium dioxide nanofiber, PP fiber, alumina fiber, and polyamide 66 fiber in a mass ratio of 1:5-10:5-10:8-15; The manganese ion-doped calcite nano-calcium carbonate is prepared by the following method: Dissolving calcium nitrate and urea in deionized water at a molar ratio of 1:1-10, adding a manganese chloride solution while stirring to obtain a raw material solution, wherein the concentration of manganese chloride in the raw material solution is 0.1 mol / L-0.5 mol / L; The pH value of the raw material solution is adjusted to 7-9, and the raw material solution is transferred to a microwave digestion apparatus for treatment; After the treatment is completed, the treated product is centrifuged to obtain a precipitate, and the precipitate is washed to obtain the manganese ion-doped calcite nano-calcium carbonate.
2. The concrete according to claim 1, characterized in that The solid waste-based mineral admixture comprises a solid waste mixture and modified fly ash, and the mass ratio of the solid waste mixture to the modified fly ash is 2:3-10; The solid waste mixture includes at least one of ceramic waste, slag, and autoclaved aerated concrete waste, and the particle size of the solid waste mixture is greater than or equal to 20 meshes.
3. The concrete according to claim 2, characterized in that: The modified fly ash is prepared by mixing fly ash and an activated modifier and then ball milling, wherein the activated modifier comprises sodium carbonate and sodium hydroxide in a mass ratio of 1:2-3.
4. The concrete according to claim 1, characterized in that The processing temperature of the microwave digestion instrument is 180° C.-250° C., and the processing time of the microwave digestion instrument is 1 hour-2 hours.
5. The concrete according to claim 1, characterized in that The titanium dioxide nanofibers are prepared by the following method: dissolving titanium phosphide in ethanol, using acetic acid as a chelating agent, and sequentially subjecting the mixture to electrospinning and calcining to prepare the titanium dioxide nanofibers; Wherein, the calcination temperature is 800°C-1200°C, and the calcination time is 2 hours-4 hours.
6. The concrete according to claim 1, characterized in that The length of the titanium dioxide nanofiber is 300nm-500nm, and the length of the PP fiber, the alumina fiber, and the polyamide 66 fiber are each independently 3mm-8mm.
7. A method for preparing concrete, characterized in that: The concrete is as described in any one of claims 1 to 6; The method for preparing the concrete comprises: Providing or preparing various components for constituting a dry blend, and uniformly mixing the various components to prepare the dry blend; The dry mix is mixed with water to prepare the concrete.
8. A 3D printing material, characterized in that: The 3D printing material is prepared by a 3D printing process using the concrete according to any one of claims 1 to 6.
Citation Information
Patent Citations
Microwave homogeneous hydrothermal synthesis method of magnesium-aluminum hydrotalcite
CN106276996A
High-flame-retardancy and aging-resistant polypropylene composite material for packaging
CN109054174A
High-strength polyvinyl alcohol fiber reinforced cement-based composite material as well as preparation method and application thereof
CN113045273A
Amorphous porous ceramic nanofiber membrane as well as preparation method and application thereof
CN113426492A
Cement-based material added with superfine fly ash and preparation process of cement-based material
CN114634340A