Metal bipolar plate coating and preparation method thereof

The multi-layer TiO gradient layer and C-doped TiOx layer were prepared by multi-target magnetron sputtering technology, which solved the problem of the passivation layer formation of PEMFC metal bipolar plates in acidic and high potential environments, and achieved high stability and conductivity The coating improves fuel cell performance.

CN118639207BActive Publication Date: 2024-11-15ARISON SURFACE TECH SUZHOU
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411113523.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-15
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The existing PEMFC metal bipolar plates are prone to form passivation layers in acidic and high potential environments, reducing conductivity and increasing interface contact resistance, affecting fuel cell performance. Moreover, TiO2, as an n-type semiconductor material, has poor conductivity and is difficult to prepare low TiO2-based coating of interface contact resistance.

Method used

Multi-layer TiO gradient layer and C-doped TiOx layer were prepared by multi-target magnetron sputtering technology, controlling O2 flow rate and temperature and bias parameters applied to the metal substrate, forming a Ti4+ wrapped Ti3+ structure to slow down the oxidation of Ti3+, and The stability and conductivity of the coating are improved by the multi-layer film structure.

Benefits of technology

It realizes the stability and conductivity of coatings in a long-term corrosion environment with high potential, reduces surface contact resistance, and improves the stability and service life of metal bipolar plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639207B_ABST
    Figure CN118639207B_ABST
Patent Text Reader

Abstract

The present invention relates to a metal bipolar plate coating and a preparation method thereof, wherein a composite structure of a multi-layer TiO gradient layer and a C-doped TiOx layer is formed by controlling the O2 flow rate and the temperature and bias voltage parameters applied to the metal substrate. This structural coating realizes Ti 4+ PackageTi 3+ , avoiding Ti 3+ The oxidation of Ti in the coating is further slowed down by the combined structure of multi-layer TiO graded layer and C-doped TiOx layer. 3+ It can resist corrosion, making it stable during long-term corrosion at high potential, and its conductivity is still excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of surface protection of metal bipolar plates for batteries, and in particular to a metal bipolar plate coating and a preparation method thereof. Background Art

[0002] Existing PEMFC metal bipolar plate materials, such as stainless steel, have good mechanical stability and electrical conductivity, but are prone to forming a passivation layer in the acidic, high-potential working environment of the fuel cell. The formation of the passivation layer not only reduces the conductivity of the bipolar plate, but also increases the interfacial contact resistance (ICR) with the gas diffusion layer (GDL), which in turn affects the power output and efficiency of the fuel cell. In addition, the metal ions under the passivation layer may be released and migrate to the membrane electrode assembly (MEA), causing damage to the catalyst and further reducing the performance of the fuel cell.

[0003] In order to solve the above problems, researchers have developed a variety of metal bipolar plate surface modification coating technologies, such as Au, amorphous carbon, metal nitrides, metal carbides, etc. Among them, although the Au coating has excellent conductivity and durability, its high cost limits its popularity in commercial applications. Although the amorphous carbon coating has a low cost, it is easy to dissolve or detach in a long-term high-potential corrosion environment, and cannot meet the needs of long-term stable operation.

[0004] As a material that can withstand long-term, high-potential acidic corrosion conditions, TiO2 shows good application potential in the field of fuel cells. However, as an n-type semiconductor material, TiO2 has relatively poor conductivity. Direct use as a bipolar plate coating will increase the interfacial contact resistance and affect the performance of the fuel cell. Therefore, how to prepare a TiO2-based coating with low ICR and apply it to the surface modification of PEMFC metal bipolar plates has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides a method for preparing a metal bipolar plate coating.

[0006] To achieve the above objectives, this application is implemented through the following technical solutions:

[0007] The present application provides a method for preparing a metal bipolar plate coating, comprising the following steps:

[0008] S1. Cleaning the metal substrate;

[0009] S2, placing the metal substrate into a multi-target magnetron sputtering chamber, wherein a Ti target and a C target are pre-set in the multi-target magnetron sputtering chamber;

[0010] S3, turning on the Ti target, setting the bias voltage applied to the metal substrate to a preset bias voltage, the preset bias voltage is -60V to -250V, setting the temperature applied to the metal substrate to 200°C to 650°C, linearly increasing the current applied to the Ti target until a first preset current value is reached, maintaining the first preset current value unchanged to deposit a Ti base layer, the first preset current value being 10A to 15A;

[0011] S4, maintaining the current applied to the Ti target unchanged, introducing O2 into the cavity of the multi-target magnetron sputtering instrument, and linearly increasing the flow rate of the introduced O2 until reaching a first preset flow rate value, to prepare a TiO gradient layer, wherein the first preset flow rate value is 20 sccm to 60 sccm;

[0012] S5, maintaining the current applied to the Ti target and the flow rate of O2 unchanged, linearly increasing the current applied to the C target until it reaches a second preset current value, maintaining the second preset current value unchanged to deposit a C-doped TiOx layer, the second preset current value is 1A to 5A;

[0013] S6. Linearly reduce the O2 flow rate and the C target current to 0 within 5 minutes, and then repeat steps S4 and S5 to prepare a TiO gradient layer and a C-doped TiOx layer in sequence.

[0014] As a further improvement of the present application, the metal substrate may be any one of a stainless steel substrate, a Ti substrate, and an Al substrate.

[0015] As a further improvement of the present application, the purity of the Ti target is 99.99%, the purity of the C target is 99.99%, and the purity of O2 is 99.99%.

[0016] As a further improvement of the present application, in step S3, the current value applied to the Ti target increases linearly at a rate of 1.0 A / min to 1.5 A / min.

[0017] As a further improvement of the present application, in step S3, the time for depositing the Ti base layer is 10 minutes to 30 minutes while maintaining the first preset current value unchanged.

[0018] As a further improvement of the present application, in step S4, the linear increase rate of the flow rate of O2 until it reaches the first preset flow value is 0.5 sccm / min to 1.5 sccm / min.

[0019] As a further improvement of the present application, in step S5, the time for depositing the C-doped TiOx layer while maintaining the second preset current value unchanged is 1 hour to 2 hours.

[0020] As a further improvement of the present application, step S6 also includes repeating the operation of step S6 once or twice.

[0021] As a further improvement of the present application, the total thickness of the TiO graded layer and the C-doped TiOx layer is 450 nm to 550 nm.

[0022] As a further improvement of the present application, in step S1, the metal substrate is sequentially subjected to ultrasonic cleaning and plasma cleaning.

[0023] As a further improvement of the present application, the specific steps of the ultrasonic cleaning are as follows: placing the metal substrate to be cleaned in an ultrasonic cleaning machine, and cleaning it in analytical pure anhydrous alcohol and acetone in turn using 15kHz to 30kHz ultrasonic waves;

[0024] The specific steps of the plasma cleaning are as follows: placing the metal substrate after ultrasonic cleaning in a vacuum chamber, evacuating the vacuum chamber to a pressure of 4×10 -3 Pa, Ar is introduced to maintain the vacuum degree at 2Pa-4Pa, and the metal substrate is bombarded with ions using a medium frequency power supply.

[0025] To achieve the above objectives, the present application also provides a metal bipolar plate coating prepared using the above-mentioned method for preparing the metal bipolar plate coating.

[0026] The beneficial effect of the present application is that the present application provides a method for preparing a metal bipolar plate coating, by controlling the O2 flow rate and the temperature and bias parameters applied to the metal substrate, a composite structure of a multi-layer TiO gradient layer and a C-doped TiOx layer is formed. This structural coating realizes Ti 4+ PackageTi 3+ , avoiding Ti 3+ The oxidation of Ti in the coating is further slowed down by the combined structure of multi-layer TiO graded layer and C-doped TiOx layer. 3+ It can resist corrosion, making it stable during long-term corrosion at high potential, and its conductivity is still excellent.

[0027] The surface contact resistance of the metal bipolar plate coating prepared in this application before corrosion is less than 3mΩ·cm 2 , under the condition of +1.6V (vs. SHE) constant potential corrosion for 10h, the surface contact resistance is less than 10mΩ·cm 2 , the constant potential polarization curve is stable. Applying it in the field of surface modification of metal bipolar plates of fuel cells can improve the stability and service life of metal bipolar plates. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1This is an XPS spectrum of the combined structure of the multi-layer TiO gradient layer and the C-doped TiOx layer of the metal bipolar plate coating of Example 2;

[0029] Figure 2 is an XRD spectrum of a combined structure of a multi-layer TiO gradient layer and a C-doped TiOx layer of the metal bipolar plate coating of Example 2;

[0030] Figure 3 It is a constant potential polarization spectrum of the combined structure of the multi-layer TiO gradient layer and the C-doped TiOx layer of the metal bipolar plate coating of Example 2 during the corrosion process (+1.6V (vs. SHE));

[0031] Figure 4 It is a surface contact resistance spectrum of the combined structure of the multi-layer TiO gradient layer and the C-doped TiOx layer of the metal bipolar plate coating of Example 2 before and after corrosion. DETAILED DESCRIPTION

[0032] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solution of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0033] In order to make the above-mentioned objects, features and advantages of the present application more obvious and easy to understand, the present application is further described in detail below in conjunction with specific implementation methods.

[0034] The inherent characteristic of magnetron sputtering is columnar crystal growth, which will produce deeper grain boundaries, which will be the location where pitting corrosion occurs. To solve the above problem, the present application adopts a multi-layer film design to slow down the occurrence of pitting corrosion.

[0035] According to the conductivity mechanism of different titanium oxides, Ti 4+ TiO2 has no electron transition channel because Ti and O form a covalent bond. 3+ and Ti 2+ When 3+ 、Ti 2+ It will provide additional electron transfer channels, increasing the conductivity of TiO2. 3+ The generation of Ti causes lattice rearrangement, causing lattice distortion of O atoms, reducing the energy of the coating, improving the stability of the coating, and making the coating corrosion resistant. 3+ Surrounded by Ti 4+ When protecting, Ti 3+It is difficult to be oxidized, so the coating has excellent stability. In addition, element doping will bring new electron transmission points to the coating. At the same time, the lattice distortion brought by element doping may bring more electron transmission paths and improve conductivity.

[0036] Based on the above discussion, in the process of preparing the TiO gradient layer and the C-doped TiOx layer, the coating is grown into a TiO layer by adjusting the oxygen flow rate and the temperature and bias voltage of the metal substrate. 4+ PackageTi 3+ The structure avoids Ti 3+ The oxidation of TiO in the coating is further slowed down by forming a multilayer structure composed of a TiO graded layer and a C-doped TiOx layer. 3+ It can resist corrosion, making it stable during long-term corrosion at high potential, and its conductivity is still excellent.

[0037] In order to verify the technical solution of the present application, the following examples are provided as evidence.

[0038] Example 1

[0039] This embodiment provides a method for preparing a metal bipolar plate coating, comprising the following steps:

[0040] S1. Cleaning the metal substrate, which is a 316L stainless steel substrate. Specifically: First, place the metal substrate to be cleaned in an ultrasonic cleaning machine, and clean it in analytical pure anhydrous alcohol and acetone using 30kHz ultrasonic waves for 15 minutes; second, place the metal substrate after ultrasonic cleaning in a vacuum chamber, and evacuate the vacuum chamber to a pressure of 4×10 -3 Pa, Ar is introduced, the vacuum degree is maintained at 2Pa-4Pa, and the metal substrate is bombarded with ions using a medium frequency for 30 minutes.

[0041] S2, placing the metal substrate into a multi-target magnetron sputtering chamber, wherein a Ti target and a C target are pre-set in the multi-target magnetron sputtering chamber;

[0042] S3, turning on the Ti target, setting the bias voltage applied to the metal substrate to a preset bias voltage of -60 V, setting the temperature applied to the metal substrate to 550° C., linearly increasing the current applied to the Ti target at a rate of 1.2 A / min until it reaches 12 A, maintaining 12 A constant and depositing the Ti base layer for 20 min;

[0043] S4, maintaining the current applied to the Ti target unchanged, introducing O2 into the cavity of the multi-target magnetron sputtering instrument, and linearly increasing the flow rate of the introduced O2 at a rate of 1 sccm / min until it reaches 45 sccm, to prepare a TiO gradient layer;

[0044] S5, maintaining the current applied to the Ti target and the flow rate of O2 unchanged, linearly increasing the current applied to the C target until it reaches 2A, maintaining 2A unchanged for 1h to prepare a C-doped TiOx layer;

[0045] S6, linearly reducing the O2 flow rate and the C target current to 0 within 5 minutes, and then repeating steps S4 and S5 to sequentially prepare a TiO gradient layer and a C-doped TiOx layer;

[0046] Step S6 is repeated once more to obtain a coating structure composed of three TiO graded layers and a C-doped TiOx layer.

[0047] After testing the surface contact resistance of the metal bipolar plate coating obtained in Example 1, it can be seen that before corrosion, the surface contact resistance of the metal bipolar plate coating is 3.56 mΩ·cm 2 ; After 10h of corrosion at +1.6V (vs. SHE) constant potential polarization, the surface contact resistance of the metal bipolar plate coating is 9.89mΩ·cm 2 , the constant potential polarization curve remains stable.

[0048] Example 2

[0049] This embodiment provides a method for preparing a metal bipolar plate coating, comprising the following steps:

[0050] S1. Cleaning a metal substrate, wherein the metal substrate is a TA1 substrate. Specifically: first, the metal substrate to be cleaned is placed in an ultrasonic cleaning machine, and cleaned in analytical pure anhydrous alcohol and acetone using 30kHz ultrasonic waves for 15 minutes; second, the metal substrate after ultrasonic cleaning is placed in a vacuum chamber, and the vacuum chamber is evacuated to a pressure of 4×10 -3 Pa, Ar is introduced, the vacuum degree is maintained at 2Pa-4Pa, and the metal substrate is bombarded with ions using a medium frequency for 30 minutes.

[0051] S2, placing the metal substrate into a multi-target magnetron sputtering chamber, wherein a Ti target and a C target are pre-set in the multi-target magnetron sputtering chamber;

[0052] S3, turning on the Ti target, setting the bias voltage applied to the metal substrate to a preset bias voltage of -250 V, setting the temperature applied to the metal substrate to 550° C., linearly increasing the current applied to the Ti target at a rate of 1.2 A / min until it reaches 12 A, maintaining 12 A constant and depositing the Ti base layer for 20 min;

[0053] S4, maintaining the current applied to the Ti target unchanged, introducing O2 into the cavity of the multi-target magnetron sputtering instrument, and linearly increasing the flow rate of the introduced O2 at a rate of 0.75 sccm / min until it reaches 30 sccm, to prepare a TiO gradient layer;

[0054] S5, maintaining the current applied to the Ti target and the flow rate of O2 unchanged, linearly increasing the current applied to the C target until it reaches 2A, maintaining 2A unchanged for 1.5h to prepare a C-doped TiOx layer;

[0055] S6, linearly reducing the O2 flow rate and the C target current to 0 within 5 minutes, and then repeating steps S4 and S5 to sequentially prepare a TiO gradient layer and a C-doped TiOx layer;

[0056] Step S6 is repeated twice to obtain a coating structure composed of four TiO gradient layers and a C-doped TiOx layer. The XPS and XRD spectra of the combined structure of the multi-layer TiO gradient layer and the C-doped TiOx layer of the metal bipolar plate coating of Example 2 are shown in FIG. Figure 1 and Figure 2 .

[0057] After testing the surface contact resistance of the metal bipolar plate coating obtained in Example 2, it can be seen that before corrosion, the surface contact resistance of the metal bipolar plate coating is 4.88 mΩ·cm 2 After 10h of constant potential polarization at +1.6V (vs. SHE), the surface contact resistance of the metal bipolar plate coating is 6.26mΩ·cm 2 , the constant potential polarization curve remains stable, and the constant potential polarization spectrum is shown in Figure 3 The surface contact resistance spectra of the metal bipolar plate coating before and after corrosion in this embodiment are as follows: Figure 4 As shown, where: ICR is the abbreviation of surface contact resistance, and O30 represents that the preset flow value of O2 is 30sccm.

[0058] In summary, the present application provides a metal bipolar plate coating and a preparation method thereof, which forms a composite structure of a multi-layer TiO gradient layer and a C-doped TiOx layer by controlling the O2 flow rate and the temperature and bias parameters applied to the metal substrate. According to the conductive mechanism of the TiO structure, Ti 3+ The charge rearrangement caused by the presence of increases the stability of the coating and at the same time increases the conductivity of the coating.

[0059] When TiO2 in the coating wraps Ti 3+ When the conductive path in the coating is wrapped by the stable structure of TiO2, Ti 3+The coating will not be damaged, which makes the coating have excellent corrosion resistance, and the material stability is maintained after long-term corrosion, and the surface contact resistance will not increase. The doping of C element further causes lattice distortion, which can build more conductive channels. The design of TiO gradient layer increases the bonding strength between C-doped TiOx layer and Ti base layer, and also increases the bonding strength between TiOx.

[0060] Another mechanism of TiO graded layer is that it is an unsaturated structure of O atoms, with Ti 3+ and Ti 2+ The conductive bonding is more, and it is not easily corroded under the protection of the C-doped TiOx layer. At the same time, it can serve as a conductive path between the C-doped TiOx layer and the Ti base layer. After part of the titanium oxide is oxidized to TiO2, the remaining TiO structure will still maintain excellent conductivity.

[0061] Finally, the structures of magnetron sputtering are mostly columnar crystals, and the problem of grain boundaries will be inevitable. The design of multi-layer coating will prevent the corrosive liquid from corroding the substrate through the grain boundaries.

[0062] In addition, the preparation method of the metal bipolar plate coating of the present application has the advantages of high production efficiency, low energy consumption, and low equipment requirements in its preparation process, and is suitable for large-scale production.

[0063] Although this specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

[0064] The series of detailed descriptions listed above are only specific descriptions of feasible implementation methods of the present application. They are not intended to limit the scope of protection of the present application. Any equivalent implementation methods or changes that do not deviate from the technical spirit of the present application should be included in the scope of protection of the present application.

Claims

1. A method for preparing a metal bipolar plate coating, characterized in that: The steps include: S1. Cleaning the metal substrate; S2, placing the metal substrate into a multi-target magnetron sputtering chamber, wherein a Ti target and a C target are pre-set in the multi-target magnetron sputtering chamber; S3, turn on the Ti target, set the bias voltage applied to the metal substrate to a preset bias voltage, the preset bias voltage is set to -60V to -250V, set the temperature applied to the metal substrate to 200°C to 650°C, linearly increase the current applied to the Ti target until it reaches a first preset current value, maintain the first preset current value unchanged to deposit the Ti base layer, the current value applied to the Ti target increases linearly at a rate of 1.0A / min to 1.5A / min, the first preset current value is 10A to 15A, maintain the first preset current value unchanged to deposit the Ti base layer for 10min to 30min; S4, maintaining the current applied to the Ti target unchanged, introducing O2 into the cavity of the multi-target magnetron sputtering instrument, and linearly increasing the flow rate of the introduced O2 until it reaches a first preset flow value, to prepare a TiO gradient layer, the linear increase rate of the flow rate of the introduced O2 until it reaches the first preset flow value is 0.5 sccm / min to 1.5 sccm / min, and the first preset flow value is 20 sccm to 60 sccm; S5, maintaining the current applied to the Ti target and the flow rate of O2 unchanged, linearly increasing the current applied to the C target until it reaches a second preset current value, maintaining the second preset current value unchanged to deposit the C-doped TiOx layer, the second preset current value is 1A to 5A, maintaining the second preset current value unchanged to deposit the C-doped TiOx layer for 1h to 2h; S6, linearly reducing the O2 flow rate and the C target current to 0 within 5 minutes, and then repeating steps S4 and S5, sequentially preparing a TiO gradient layer and a C-doped TiOx layer, the total thickness of the TiO gradient layer and the C-doped TiOx layer is 450nm-550nm, and both the TiO gradient layer and the C-doped TiOx layer achieve Ti 4+ PackageTi 3+ .

2. The method for preparing a metal bipolar plate coating according to claim 1, characterized in that: After step S6, the process further includes repeating the operation of step S6 once or twice.

3. The method for preparing a metal bipolar plate coating according to claim 1, characterized in that: In step S1, the metal substrate is sequentially cleaned by ultrasonic cleaning and plasma cleaning.

4. The method for preparing a metal bipolar plate coating according to claim 3, characterized in that: The specific steps of the ultrasonic cleaning are as follows: placing the metal substrate to be cleaned in an ultrasonic cleaning machine, and cleaning it in analytical pure anhydrous alcohol and acetone in turn using 15kHz to 30kHz ultrasonic waves; The specific steps of the plasma cleaning are as follows: placing the metal substrate after ultrasonic cleaning in a vacuum chamber, evacuating the vacuum chamber to a pressure of 4×10 -3 Pa, Ar is introduced to maintain the vacuum degree at 2Pa-4Pa, and the metal substrate is bombarded with ions using a medium frequency power supply.

5. A metal bipolar plate coating prepared by the method for preparing a metal bipolar plate coating according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Preparation method for photoelectrode

    CN110512263A

  • Positive electrode active material and preparation method thereof, positive electrode and lithium ion secondary battery

    CN114512644A

  • Preparation method of metal bipolar plate coating

    CN118086854A

  • Method for in-situ doping of titanium dioxide film

    US20120237424A1

  • Metal separator for fuel cell and manufacturing method thereof

    WO2024143971A1