Application of a MOF material in separation of tetramethylsilane and isopentane

By using porous crystal MOF materials formed by metal ions and formic acid ligands, the separation problem of tetramethylsilane and isopentane is solved, the separation selectivity and efficiency are improved, energy consumption and production costs are reduced, and the high purity tetramethylsilane is achieved. Methylsilane separation.

CN118681539BActive Publication Date: 2024-11-22KAIYANG NEW MATERIALS (ZHUHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411162502.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-22
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

It is difficult to effectively separate tetramethylsilane and isopentane in the prior art. The boiling points and molecular sizes of the two are similar, resulting in low separation selectivity and efficiency, and difficult to distinguish between traditional adsorbents.

Method used

The porous crystalline MOF material formed by coordination bonds of metal ions and formic acid ligands is used as adsorbents to achieve molecular level distinction between tetramethylsilane and isopentane through carefully designed pore sizes and structures.

Benefits of technology

It significantly improves the purity and separation selectivity of tetramethylsilane, reduces energy consumption costs, and the recycling and environmental protection of MOF materials are suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118681539B_ABST
    Figure CN118681539B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of gas adsorption separation, and discloses an application of a MOF material in separating tetramethylsilane and isopentane. The MOF material is a type of porous crystalline material formed by metal ions and formic acid ligands through coordination bonds, and the metal ions are positive divalent alkaline earth metal ions or positive divalent transition metal ions of the fourth period. The present invention uses a MOF material with porous crystals composed of metal ions and formic acid ligands as an adsorption material, and applies it to the separation of tetramethylsilane and isopentane. Through the careful design of the structure of the MOF material, it can accurately distinguish between tetramethylsilane and isopentane, two similar molecules, at the molecular level, and can greatly improve the separation selectivity and separation efficiency, and reduce the separation energy consumption; and the separated tetramethylsilane has high purity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of gas adsorption separation, and specifically relates to application of a MOF material in separation of tetramethylsilane and isopentane. Background Art

[0002] Methylsilane (TMS) is a silicon-based gas widely used in nuclear magnetic resonance references, reagents, solvents, aviation fuels and other fields. High-purity tetramethylsilane is used as an electronic gas in the semiconductor industry. Its high purity and low impurity content make it widely used in the electronics industry. With the expansion of the scale of the electronics industry, the demand for electronic gases in the semiconductor field continues to increase, and the tetramethylsilane market is also growing. At present, TMS is mainly obtained in industrial production by separating it from low-boiling residues, which often contain isopentane impurities. Since the size (5.01×6.15×7.78Å3) and boiling point (27.8℃) of isopentane molecules are similar to those of TMS molecules (size: 6.55×6.45×6.90Å3; boiling point: 26.5℃), it is very challenging to effectively separate these two substances.

[0003] Among the commonly used separation methods, distillation and adsorption are the two main options. Distillation uses the different volatilities of the components in the mixture for separation, and requires that the components to be separated have a significant difference in boiling points. For substances with a small difference in boiling points, distillation is difficult to achieve effective separation. Since tetramethylsilane and isopentane have similar boiling points, the distillation efficiency is low, and it is difficult to achieve efficient separation. The adsorption method uses porous materials as fixed bed adsorbents to selectively adsorb gases, and then desorbs them at a certain temperature and pressure to obtain the target product. The adsorption method is simple to operate, and the adsorbent can usually be recycled. It has environmental and economic advantages and has been proven to be an effective method for gas separation and purification. However, due to the similar molecular sizes of tetramethylsilane and isopentane, it is still extremely challenging to select a suitable adsorbent to distinguish between tetramethylsilane and isopentane.

[0004] Metal-organic frameworks (MOFs), also called porous coordination polymers (PCPs), are a type of porous crystalline materials with a periodic multidimensional network structure formed by self-assembly of metal ions or metal cluster units and organic ligands through coordination. As an emerging porous material, it not only has a developed pore structure and a high specific surface area, but also has structural diversity and flexibility in synthesis. Therefore, it is widely used in gas adsorption, storage and separation, optoelectronic and electromagnetic materials, catalysis and other fields. However, the current MOF materials still have much room for improvement in the separation effect of tetramethylsilane / isopentane.

[0005] Therefore, there is an urgent need to provide a MOF material with high selectivity for tetramethylsilane / isopentane separation and high purity of separated tetramethylsilane. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes an application of a MOF material in separating tetramethylsilane and isopentane. The MOF material has high selectivity for tetramethylsilane / isopentane separation, and the separated tetramethylsilane has high purity, and can be widely used in the separation of tetramethylsilane and isopentane.

[0007] The invention provides application of a MOF material in separation of tetramethylsilane and isopentane.

[0008] Specifically, a MOF material is used in the separation of tetramethylsilane and isopentane. The MOF material is a type of porous crystalline material formed by metal ions and formic acid ligands through coordination bonds; the metal ions are divalent alkaline earth metal ions or divalent transition metal ions of the fourth period.

[0009] In some embodiments of the present invention, the metal ion is selected from Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ , Fe 2+ 、Co 2+ 、Ni 2+ , Pd 2+ , Pt 2+ , Cu 2+ 、Zn 2+ , Mn 2+ Preferably, the metal ion is Co 2+ 、Ni 2+ , Mn 2+ Mg 2+ , Fe 2 + , Ca 2+ or Zn 2+ .

[0010] In some embodiments of the present invention, the pore size of the MOF material is 4.0Å-8.0Å.

[0011] In some embodiments of the present invention, the preparation method of the MOF material is as follows:

[0012] The metal salt and formic acid are dissolved in a solvent, and then heated to 50-150° C., reacted for 12-48 hours, and then the filtrate is filtered to obtain a MOF material.

[0013] In some embodiments of the present invention, the molar ratio of the metal ion in the metal salt to the formic acid is 1:(1-10).

[0014] In some embodiments of the present invention, the metal salt contains Li + 、Na + , Rb + Mg 2+ , Ca 2+ , Sr 2+ , Ba 2+ Sc 2+ 、Ti 4+ 、Zr 4+ 、 3+ Cr 3+ 、Mo 3+ 、W8 + , Mn 3+ , Fe 3+ , Fe 2+ 、Ru 3+ 、Ru 2+ , Os 3+ , Os 2+ 、Co 3+ 、Co 2+ 、Ni 2+ 、Ni + , Pd 2+ , Pd + , Pt 2+ , Pt + , Cu 2+ , Cu + 、Au + 、Zn 2+ 、A1 3+ , Ga 3+ 、In 3+ 、Si 4+ 、Si 2+ ,Ge 4+ ,Ge 2+ Sn 3+ Sn 2+ 、Bi 5+ 、Bi 3+ 、Cd 2+ , Mn 2+ , Tb 3+ , Gd 3+ 、Ce 3+ ,La 3+ Cr 4+ Metal salts of one or more metal ions.

[0015] In some embodiments of the present invention, the solvent is dimethylformamide (DMF).

[0016] In some embodiments of the present invention, the temperature for separating tetramethylsilane and isopentane is 298-423 K, and the volume ratio (separation ratio) of tetramethylsilane to isopentane is 1 / 99 to 99 / 1. Preferably, the volume ratio (separation ratio) of tetramethylsilane to isopentane is 80 / 20 to 99 / 1.

[0017] In some embodiments of the present invention, the MOF material is activated before separating tetramethylsilane and isopentane. The activation process is: degassing for 8-20 hours at 373-423K and vacuum conditions.

[0018] In some embodiments of the present invention, in the process of separating tetramethylsilane and isopentane, the MOF material is used as a filler to prepare an adsorption column, and the mixed gas of tetramethylsilane and isopentane is separated and purified by passing through the adsorption column. The MOF material is used as a filler to prepare an adsorption column, and TMS / isopentane vapor is passed through the adsorption column to separate isopentane from TMS. Compared with the traditional liquid static adsorption separation method, the separation method provided by the present invention is not only more suitable for industrial use scenarios, simplifies operation, but also can improve separation efficiency.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention uses a porous crystal MOF material composed of metal ions and formic acid ligands as an adsorption material and applies it to the separation of tetramethylsilane and isopentane. Through the careful design of the MOF material structure, it can accurately distinguish between tetramethylsilane and isopentane, two similar molecules, at the molecular level, and can effectively improve the separation selectivity and separation efficiency, and reduce the separation energy consumption; and the separated tetramethylsilane has high purity.

[0021] 2. In the present invention, the MOF material is applied to the separation of tetramethylsilane and isopentane, which has the following advantages: (1) Improving separation purity: Due to the similarity between tetramethylsilane and isopentane, the traditional method is often accompanied by the mixing of impurities during separation, resulting in low product purity. The MOF material selected in the present invention has high selectivity and greatly improves the purity of the target product tetramethylsilane. (2) Reducing energy consumption cost: Compared with traditional high-energy consumption separation methods, such as distillation, the present invention utilizes the molecular sieving effect of MOF materials to avoid high-temperature operation and large energy consumption, thereby reducing the energy consumption cost of the separation process. (3) Feasibility of recycling: By selecting MOF materials with carefully designed structures and optimizing the separation process, the present invention can significantly improve the stability and recycling performance of MOF materials in the separation of tetramethylsilane and isopentane, reduce dependence on resources, and reduce production costs. (4) Environmental protection and sustainability: The MOF material selected in the present invention is a green material, and its synthesis process is relatively environmentally friendly; and the separation method adopted in the present invention does not rely on a large amount of organic solvents or high temperature conditions, which helps to reduce the adverse impact on the environment and conforms to the concept of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM morphology of Co3(HCOO)6 prepared in Example 1;

[0023] Figure 2 3D structure diagram of Co3(HCOO)6 prepared in Example 1;

[0024] Figure 3 The PXRD diffraction pattern of Co3(HCOO)6 prepared in Example 1;

[0025] Figure 4 77K N2 adsorption diagram of Co3(HCOO)6 prepared in Example 1;

[0026] Figure 5 This is the pore size distribution diagram of Co3(HCOO)6 prepared in Example 1;

[0027] Figure 6 298K TMS / isopentane adsorption isotherm of Co3(HCOO)6 prepared in Example 1;

[0028] Figure 7 This is the IAST selectivity calculation diagram of Co3(HCOO)6 prepared in Example 1;

[0029] Figure 8 3D structure diagram of Mn3(HCOO)6 prepared in Example 2;

[0030] Fig. 9The PXRD diffraction pattern of Mn3(HCOO)6 prepared in Example 2;

[0031] Fig.10 3D structure diagram of Ni3(HCOO)6 prepared in Example 3;

[0032] Fig.11 The PXRD diffraction pattern of Ni3(HCOO)6 prepared in Example 3;

[0033] Fig.12 3D structure diagram of Mg3(HCOO)6 prepared in Example 4;

[0034] Fig.13 The PXRD diffraction pattern of Mg3(HCOO)6 prepared in Example 4;

[0035] Fig.14 3D structure diagram of Ca3(HCOO)6 prepared in Example 5;

[0036] Fig.15 The PXRD diffraction pattern of Ca3(HCOO)6 prepared in Example 5;

[0037] Fig.16 3D structure diagram of Fe3(HCOO)6 prepared in Example 6;

[0038] Fig.17 The PXRD diffraction pattern of Fe3(HCOO)6 prepared in Example 6;

[0039] Fig.18 3D structure diagram of Zn3(HCOO)6 prepared in Example 7;

[0040] Fig.19 This is the PXRD diffraction pattern of Zn3(HCOO)6 prepared in Example 7. DETAILED DESCRIPTION

[0041] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be noted that the following embodiments do not limit the protection scope of the present invention.

[0042] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0043] Example 1: Synthesis of Co3(HCOO)6 and its application in separation of TMS and isopentane

[0044] 1. Synthesis of MOF materials

[0045] In a glass bottle, cobalt (II) nitrate hexahydrate (1.309 g, 4.4 mmol) and formic acid (1 ml, 25.7 mmol) were mixed with DMF (10 ml), heated to 100 °C for 24 hours, and then cooled to room temperature. The resulting pink powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material Co3(HCOO)6. Before the gas adsorption test, the sample was degassed at 413 K under vacuum conditions for 12 hours.

[0046] 2. Characterization of MOF Materials

[0047] The morphology of the prepared MOF material was analyzed using a cold field emission scanning electron microscope Hitachi S-4700. Figure 1 The SEM morphology shown is Figure 1 It can be seen that MOF materials are micron-sized spindle-shaped particles. Through X-ray powder diffraction phase analysis (PXRD), its diffraction peak and crystal structure ( Figure 2 ) The peak position of the simulated PXRD spectrum remains consistent ( Figure 3 ), proving that the synthesized MOF material is a Co3(HCOO)6 crystal structure. At the same time, nitrogen adsorption was measured at 77K, and its specific surface area was 415.12m 2 / g( Figure 4 ) and pore size around 6.1Å ( Figure 5 ).

[0048] 3. Separation performance test of MOF materials

[0049] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, such as Figure 6 As shown, the separation selectivity under this condition is calculated by IAST to be 208, as shown in Figure 7 shown.

[0050] The separation selectivity of TMS / isopentane at different volume ratios at 298K is shown in Table 1.

[0051] Table 1

[0052]

[0053] 100 g of Co3(HCOO)6 was loaded into a stainless steel adsorption column (10 mm inner diameter × 180 mm), and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5 mL / min and the pressure was set to 1 bar. The purity of the penetrated TMS at different temperatures was tested. The results are shown in Table 2.

[0054] Table 2

[0055]

[0056] It can be seen from Table 2 that more than 99.99% TMS can be obtained at different adsorption temperatures, and the optimal separation temperature should be between 298 and 323K.

[0057] Example 2: Synthesis of Mn3(HCOO)6 and its application in separation of TMS and isopentane

[0058] 1. Synthesis of MOF materials

[0059] In a glass bottle, manganese (II) nitrate (4.4 mmol) and formic acid (1 ml) were mixed with DMF (10 ml), heated to 100 °C for 24 h, and then cooled to room temperature. The resulting pink powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 h.

[0060] 2. Characterization of MOF Materials

[0061] After analysis, the morphology of MOF material is micron-sized spindle-shaped particles. The diffraction peaks and crystal structure ( Figure 8 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig. 9 ), proving that the synthesized MOF material has a Mn3(HCOO)6 crystal structure.

[0062] 3. Separation performance test of MOF materials

[0063] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 198. 100g of Mn3(HCOO)6 was loaded into a stainless steel adsorption column (10mm inner diameter × 180mm), and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrating TMS was 99.99%.

[0064] Example 3: Synthesis of Ni3(HCOO)6 and its application in separation of TMS and isopentane

[0065] 1. Synthesis of MOF materials

[0066] In a glass bottle, nickel (II) nitrate (4.4 mmol) and formic acid (1 mL) were mixed with DMF (10 mL), heated to 100 °C for 24 h, and then cooled to room temperature. The resulting green powder was filtered, washed with DMF (10 mL) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 h.

[0067] 2. Characterization of MOF Materials

[0068] After analysis, the morphology of MOF material is micron-sized spindle-shaped particles. The diffraction peaks and crystal structure ( Fig.10 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig.11 ), proving that the synthesized MOF material is a Ni3(HCOO)6 crystal structure.

[0069] 3. Separation performance test of MOF materials

[0070] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 300. 100g Ni3(HCOO)6 was loaded into a stainless steel adsorption column (10mm inner diameter × 180mm), and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrating TMS was 99.99%.

[0071] Example 4: Synthesis of Mg3(HCOO)6 and its application in separation of TMS and isopentane

[0072] 1. Synthesis of MOF materials

[0073] In a glass bottle, magnesium (II) chloride (4.4 mmol) and formic acid (1 ml) were mixed with DMF (10 ml), heated to 100 °C for 24 hours, and then cooled to room temperature. The resulting white powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 hours.

[0074] 2. Characterization of MOF Materials

[0075] After analysis, the morphology of MOF material is micron-sized spindle-shaped particles. The diffraction peaks and crystal structure ( Fig.12 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig.13 ), proving that the synthesized MOF material has a Mg3(HCOO)6 crystal structure.

[0076] 3. Separation performance test of MOF materials

[0077] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 258. 100g Mg3(HCOO)6 was loaded into a stainless steel adsorption column (10mm inner diameter × 180mm), and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrating TMS was 99.99%.

[0078] Example 5: Synthesis of Ca3(HCOO)6 and its application in molecular sieving of TMS / isopentane

[0079] 1. Synthesis of MOF materials

[0080] In a glass bottle, calcium chloride (4.4 mmol) and formic acid (1 ml) were mixed with DMF (10 ml), heated to 100 °C for 24 hours, and then cooled to room temperature. The resulting white powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 hours.

[0081] 2. Characterization of MOF Materials

[0082] After analysis, the morphology of MOF material is nanoparticles. The diffraction peaks and crystal structure ( Fig.14 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig.15 ), proving that the synthesized MOF material is a Ca3(HCOO)6 crystal structure.

[0083] 3. Separation performance test of MOF materials

[0084] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 168. 100g Ca3(HCOO)6 was loaded into a stainless steel adsorption column, and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrated TMS was 99.98%.

[0085] Example 6: Synthesis of Fe3(HCOO)6 and its application in molecular sieving of TMS / isopentane

[0086] 1. Synthesis of MOF materials

[0087] In a glass bottle, ferrous nitrate (4.4 mmol) and formic acid (1 ml) were mixed with DMF (10 ml), heated to 100 °C for 24 hours, and then cooled to room temperature. The resulting green powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 hours.

[0088] 2. Characterization of MOF Materials

[0089] After analysis, the morphology of MOF material is nanoparticles. The diffraction peaks and crystal structure ( Fig.16 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig.17 ), proving that the synthesized MOF material has a Fe3(HCOO)6 crystal structure.

[0090] 3. Separation performance test of MOF materials

[0091] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 110. 100g of Fe3(HCOO)6 was loaded into a stainless steel adsorption column, and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrated TMS was 99.97%.

[0092] Example 7: Synthesis of Zn3(HCOO)6 and its application in molecular sieving of TMS / isopentane

[0093] 1. Synthesis of MOF materials

[0094] In a glass bottle, zinc nitrate (4.4 mmol) and formic acid (1 ml) were mixed with DMF (10 ml), heated to 100 °C for 24 hours, and then cooled to room temperature. The resulting white powder was filtered, washed with DMF (10 ml) and dried in air to obtain the MOF material. Before the gas adsorption test, the sample was degassed at 413 K under vacuum for 12 hours.

[0095] 2. Characterization of MOF Materials

[0096] After analysis, the morphology of MOF material is nanoparticles. The diffraction peaks and crystal structure ( Fig.18 ) The peak position of the simulated PXRD spectrum remains consistent ( Fig.19 ), proving that the synthesized MOF material has a Zn3(HCOO)6 crystal structure.

[0097] 3. Separation performance test of MOF materials

[0098] The single component vapor adsorption curves of TMS and isopentane were measured at 298K, and the separation selectivity under this condition was calculated by IAST to be 145. 100g Zn3(HCOO)6 was loaded into a stainless steel adsorption column, and a gas with a volume ratio of TMS / isopentane of 95 / 5 was passed through the adsorption column. The flow rate was set to 5mL / min, the pressure was 1bar, and the temperature was 298K. The purity of the penetrated TMS was 99.98%.

[0099] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. Application of a MOF material in separation of tetramethylsilane and isopentane, characterized in that: The MOF material is a type of porous crystalline material formed by metal ions and formic acid ligands through coordination bonds; the MOF material is Co3(HCOO)6, Mn3(HCOO)6, Ni3(HCOO)6, Mg3(HCOO)6, Ca3(HCOO)6, Fe3(HCOO)6 or Zn3(HCOO)6; the pore size of the MOF material is 4.0Å-8.0Å; the MOF material is activated before separating tetramethylsilane and isopentane; the activation process is: degassing for 8-20h at 373-423K and vacuum conditions.

2. The use according to claim 1, characterized in that: The preparation method of the MOF material is as follows: The metal salt and formic acid are dissolved in a solvent, then heated to 50-150° C., reacted for 12-48 hours, and then filtered to remove the filtrate to obtain the MOF material.

3. The use according to claim 2, characterized in that: The molar ratio of the metal ion in the metal salt to the formic acid is 1:(1-10).

4. The use according to claim 1, characterized in that: The temperature for separating tetramethylsilane and isopentane is 298-423K, and the volume ratio of tetramethylsilane to isopentane is 1 / 99 to 99 / 1.

5. The use according to claim 4, characterized in that: The volume ratio of tetramethylsilane to isopentane is 80 / 20 to 99 / 1.

6. The use according to claim 4 or 5, characterized in that: In the process of separating tetramethylsilane and isopentane, an adsorption column is prepared using the MOF material as filler, and the mixed gas of tetramethylsilane and isopentane is separated and purified by passing through the adsorption column.