Liquid crystal frame sealing adhesive and preparation method thereof

By using components such as bisphenol A type epoxy resin and materials such as aminobisindole in liquid crystal frame sealing glue, the cross-linking network structure is solved, and the performance of existing liquid crystal frame sealing glue is poor in high temperature and high humidity environments. Problem, higher bonding strength and high temperature and high humidity resistance are achieved, and the liquid crystal display device is prevented from contamination.

CN118685142BActive Publication Date: 2024-11-05HEFEI SINOPISE MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411165243.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-05
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Existing liquid crystal frame sealing glue cannot effectively prevent the invasion of water vapor and oxygen in high temperature and high humidity environments, resulting in the possibility of degradation in performance and contamination of liquid crystal display devices.

Method used

Using a combination of bisphenol A type epoxy resin, epoxy acrylate, hydrophobic silica, aminobisindole, organic sodium salt, photoinitiator and silane coupling agent, the proportion and process parameters of each component are strictly controlled , a tight crosslinking network structure is formed to improve bonding strength and high temperature and humidity resistance.

Benefits of technology

It significantly enhances the bonding strength and high temperature and high humidity resistance of liquid crystal frame sealing adhesive, effectively blocks water vapor and oxygen, prevents liquid crystal display devices from being contaminated, and maintains the bonding performance in high temperature and high humidity environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118685142B_ABST
    Figure CN118685142B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of adhesives, and specifically discloses a liquid crystal frame sealant and a preparation method thereof. The liquid crystal frame sealant of the present invention comprises the following raw materials in parts by weight: 60-100 parts of bisphenol A epoxy resin, 40-60 parts of epoxy acrylate, 10-30 parts of hydrophobic silica, 4-10 parts of aminobisindole, 1-3 parts of organic sodium salt, 2-5 parts of photoinitiator, 8-15 parts of thermosetting agent, and 3-7 parts of silane coupling agent; the preparation method of the present invention is to mix the above raw materials; the components in the prepared liquid crystal frame sealant interact with each other, which not only significantly enhances the bonding strength, but also helps to improve the high temperature and high humidity resistance. In a high temperature and high humidity environment, the frame sealant can still effectively block water vapor and oxygen from invading a liquid crystal display, effectively ensuring that the performance of the liquid crystal display device is not affected by the environment, and can be widely used in liquid crystal displays.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and more specifically, to a liquid crystal frame sealing adhesive and a preparation method thereof. Background Art

[0002] Liquid crystal displays have become a hot topic for major electronic and electrical appliance companies to study due to their many advantages, such as thin body, space saving, power saving, no high temperature, low radiation, soft picture and no harm to the eyes. Among them, liquid crystal frame glue mainly plays a sealing role in liquid crystal display devices, bonding the upper and lower substrate materials with electrodes and orientation layers, and maintaining a certain gap to seal the liquid crystal in them; this sealing structure not only ensures that the liquid crystal will not leak, but also prevents external heat, moisture and dust from entering the liquid crystal display device, thereby ensuring the stability and reliability of the device.

[0003] At present, CN114106742 A discloses a high-viscosity liquid crystal frame sealant, which comprises the following raw materials by weight: 10-20 parts of epoxy resin, 40-60 parts of acrylic resin, 0.2-2 parts of bismaleimide resin, 0.2-2 parts of photoinitiator, 15-30 parts of organic filler, 0.2-2 parts of coupling agent, 0.2-3 parts of silicon dioxide, and 10-20 parts of thermal curing agent, wherein the thermal curing agent adopts malonic acid dihydrazide curing agent; the viscosity of the frame sealant has been greatly improved, the adhesion of the frame sealant has been improved, and the leakage of liquid crystal has been effectively prevented; however, the high temperature and high humidity resistance of the frame sealant needs to be improved. In a high temperature and high humidity environment, it is impossible to effectively avoid the invasion of water vapor and oxygen, and thus it is impossible to effectively ensure that the performance of the liquid crystal display device is not affected by the environment for a long time, and there is a possibility that the liquid crystal is contaminated.

[0004] Based on the above statements, the present invention proposes a liquid crystal frame-sealing adhesive and a preparation method thereof. Summary of the invention

[0005] In order to solve the problem that the existing liquid crystal frame sealing adhesive has poor high temperature and high humidity resistance, the present invention provides a liquid crystal frame sealing adhesive and a preparation method thereof.

[0006] In a first aspect, the present invention provides a liquid crystal frame sealant, which adopts the following technical solution:

[0007] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 60-100 parts of bisphenol A epoxy resin, 40-60 parts of epoxy acrylate, 10-30 parts of hydrophobic silica, 4-10 parts of aminobisindole, 1-3 parts of organic sodium salt, 2-5 parts of photoinitiator, 8-15 parts of thermal curing agent, and 3-7 parts of silane coupling agent;

[0008] The structural formula of the aminobisindole is: .

[0009] Preferably, the aminobisindole is prepared by the following method:

[0010] Step A1, under nitrogen environment, add 5-nitroindole, 1,3-dichloropropane and anhydrous potassium carbonate to N-methylpyrrolidone, stir and react at 180-200° C. for 10-15 hours, cool to room temperature, and then cool in ice water for 10-30 minutes, solid precipitates, filter, wash and dry to obtain compound I;

[0011] Step A2. Under a nitrogen environment, add compound I and palladium-carbon catalyst to N,N-dimethylformamide, stir evenly, heat to 70-80°C, slowly drop hydrazine hydrate, and after the dropwise addition is completed within 4-6 minutes, stir the reaction for 20-30 hours. After the reaction is completed, filter while hot to obtain a filtrate; cool the filtrate to room temperature, then place it in ice water and cool for 10-30 minutes, precipitate a solid, filter it with suction, wash it, and dry it to obtain aminobisindole.

[0012] The reaction process of aminobisindole is as follows:

[0013] .

[0014] Preferably, in step A1, the ratio of 5-nitroindole, 1,3-dichloropropane, anhydrous potassium carbonate and N-methylpyrrolidone is 3.2-3.5 g: 1-1.1 g: 2.8 g: 30-40 mL.

[0015] Preferably, in step A2, the ratio of compound I, palladium-carbon catalyst, hydrazine hydrate and N,N-dimethylformamide is 1.8-2 g: 0.2 g: 1.9-2.2 g: 30-50 mL.

[0016] Preferably, the Pd loading in the palladium-carbon catalyst is 5%.

[0017] Preferably, the hydrophobic silica is prepared by the following method:

[0018] Step B1, dissolving suberic acid in ethyl acetate, adding nano-silicon dioxide, stirring and reacting at 40-60° C. for 3-4 hours, filtering, washing, drying and grinding to obtain SA-SiO2;

[0019] Step B2: Add SA-SiO2 and 1-adamantanol to toluene, stir and react at 50-60° C. for 4-5 hours, cool to room temperature, filter, wash, dry and grind to obtain hydrophobic silica.

[0020] Preferably, in step B1, the usage ratio of suberic acid, nano-silicon dioxide and ethyl acetate is 3-5 g:5 g:40-50 mL.

[0021] Preferably, the usage ratio of SA-SiO2, 1-adamantanol and toluene in step B2 is 5g:2-3g:40-60mL.

[0022] Preferably, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 10:3-4.

[0023] Preferably, the organic sodium salt is sodium 2,4-diaminobenzenesulfonate.

[0024] Preferably, the photoinitiator is at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2-hydroxy-2-methylpropiophenone and 2,2-dimethoxy-2-phenylacetophenone.

[0025] Preferably, the thermal curing agent is an organic acid hydrazide; the organic acid hydrazide is at least one of sebacic acid dihydrazide, isophthalic acid dihydrazide, adipic acid dihydrazide and malonic acid dihydrazide.

[0026] Preferably, the silane coupling agent is at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and N-aminoethyl-γ-aminopropyltrimethoxysilane.

[0027] In a second aspect, the present invention provides a method for preparing a liquid crystal frame sealant, which adopts the following technical solution:

[0028] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0029] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator are stirred at a speed of 100-500 r / min for 10-20 minutes, then hydrophobic silica, aminobisindole and organic sodium salt are added, and stirred at a speed of 100-500 r / min for 20-30 minutes, and finally a thermal curing agent and a silane coupling agent are added, and stirred at a speed of 100-500 r / min for 20-30 minutes to obtain a liquid crystal frame sealant.

[0030] In summary, the present invention has the following beneficial effects:

[0031] 1. The liquid crystal frame sealant of the present invention comprises bisphenol A type epoxy resin, epoxy acrylate, hydrophobic silica, aminobisindole, organic sodium salt, photoinitiator, thermal curing agent and silane coupling agent, and the weight of each component is strictly controlled to promote the interaction between the components, which not only significantly enhances the bonding strength of the frame sealant, but also helps to improve the high temperature and high humidity resistance of the frame sealant, and can effectively prevent water vapor and oxygen from invading the liquid crystal display and causing the liquid crystal display to be contaminated.

[0032] 2. The present invention uses 5-nitroindole, 1,3-dichloropropane and hydrazine hydrate as main raw materials and strictly controls process parameters to prepare aminobisindole; during the curing process of the frame-sealing adhesive, the amino group of the aminobisindole and the epoxy group of the main resin undergo a chemical reaction to increase the cross-linking density; and in the cross-linked network structure, the indole group can form a cation-π bond interaction with the sodium ions in the organic sodium salt to construct a physical cross-linked network structure and improve the rigidity of the molecular chain; at the same time, the present invention preferably uses sodium 2,4-diaminobenzenesulfonate as the organic sodium salt, and sodium 2,4-diaminobenzenesulfonate can provide amino groups in different chemical environments, further strengthening the cross-linking effect and forming a polymer with a more complex structure, thereby improving the bonding strength and high temperature and high humidity resistance of the frame-sealing adhesive.

[0033] 3. The present invention first grafts suberic acid on the surface of nano-silica, and then utilizes the carboxyl group at the other end of suberic acid to react with the hydroxyl group of 1-adamantanol for esterification, so that a strong hydrophobic film is formed on the surface of the nano-silica, thereby reducing the moisture permeability of the frame-sealing adhesive. Moreover, due to the long carbon chain structure of suberic acid, there is sufficient physical space between the hydrophobic film layer and the nano-silica, which can accommodate more resin. During subsequent curing, the frame-sealing adhesive will be firmly embedded in the interior of the hydrophobic silica, further improving the high temperature and high humidity resistance of the frame-sealing adhesive.

[0034] 4. During the preparation process of the liquid crystal frame-sealing adhesive of the present invention, various process parameters are controlled to promote the formation of a tight network structure. The prepared frame-sealing adhesive will not lose viscosity or deform under high temperature and high humidity, and still has good bonding properties. The preparation method of the present invention has simple steps, is green and environmentally friendly, is suitable for industrial production, and has positive significance for sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] The present invention will be further described below in conjunction with the accompanying drawings.

[0036] Figure 1 This is a picture of a liquid crystal box;

[0037] Figure 2 This is a picture of a liquid crystal box made of the frame-sealing adhesive obtained in Example 1 after being treated with high temperature and high humidity and observed under a polarizing film;

[0038] Figure 3 This is a picture of a liquid crystal box made of the frame sealing adhesive obtained in Comparative Example 4 after being treated with high temperature and high humidity and observed under a polarizing film. DETAILED DESCRIPTION

[0039] The present invention is further described in detail below with reference to the embodiments.

[0040] The materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial channels unless otherwise specified; among them, nano-silicon dioxide: CAS No. 60676-86-0, purchased from Shanghai McLean Biochemical Technology Co., Ltd. (99.5%, 50±5nm); bisphenol A epoxy resin E-44: epoxy equivalent is 210-240g / mol, purchased from Baling Petrochemical; bisphenol A epoxy resin E-51: epoxy equivalent is 184-194g / mol, purchased from Baling Petrochemical; epoxy acrylate: CAS No. 71281-65-7, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd. (99%); sodium 2,4-diaminobenzenesulfonate: CAS No. 3177-22-8, purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd. (≥98.0%).

[0041] Preparation Examples 1-3 provide methods for preparing aminobisindole.

[0042] Preparation Example 1

[0043] Aminobisindole is prepared by the following method:

[0044] Step A1, under nitrogen environment, add 3.2 g of 5-nitroindole, 1 g of 1,3-dichloropropane, and 2.8 g of anhydrous potassium carbonate to 30 mL of N-methylpyrrolidone, stir and react at 180°C for 10 h, cool to room temperature, and then cool in ice water at -10°C for 10 min. Solid precipitates, and is filtered off by suction. The filter residue is washed with ethanol three times, and then dried in a vacuum drying oven at 60°C for 1 h to obtain compound I;

[0045] Step A2. Under a nitrogen environment, add 1.8 g of compound I and 0.2 g of palladium carbon catalyst (Pd loading is 5%) to 30 mL of N,N-dimethylformamide, stir evenly, heat to 70°C, slowly drop 1.9 g of hydrazine hydrate, and after the addition is completed within 4 min, stir the reaction for 20 h. After the reaction is completed, filter while hot to obtain a filtrate; cool the filtrate to room temperature, place it in ice water at -10°C and cool it for 10 min, precipitate the solid, filter it by suction, wash the filter residue with distilled water 3 times, and dry it in a vacuum drying oven at 40°C for 1 h to obtain aminobisindole.

[0046] Preparation Example 2

[0047] Aminobisindole is prepared by the following method:

[0048] Step A1, under nitrogen environment, add 3.35 g of 5-nitroindole, 1.05 g of 1,3-dichloropropane, and 2.8 g of anhydrous potassium carbonate to 35 mL of N-methylpyrrolidone, stir and react at 190°C for 13 h, cool to room temperature, place in -10°C ice water for 25 min, solid precipitates, filter, wash the residue with ethanol 3 times, and dry in a vacuum drying oven at 60°C for 1 h to obtain compound I;

[0049] Step A2. Under a nitrogen environment, add 1.9 g of compound I and 0.2 g of palladium carbon catalyst (Pd loading is 5%) to 40 mL of N,N-dimethylformamide, stir evenly, heat to 75°C, slowly drop 2 g of hydrazine hydrate, and after the dropwise addition is completed within 5 min, stir the reaction for 25 h. After the reaction is completed, filter while hot to obtain a filtrate; cool the filtrate to room temperature, place it in ice water at -10°C and cool it for 25 min, precipitate a solid, filter it by suction, wash the filter residue with distilled water 3 times, and dry it in a vacuum drying oven at 40°C for 1 h to obtain aminobisindole.

[0050] Preparation Example 3

[0051] Aminobisindole is prepared by the following method:

[0052] Step A1, under nitrogen environment, add 3.5 g of 5-nitroindole, 1.1 g of 1,3-dichloropropane, and 2.8 g of anhydrous potassium carbonate to 40 mL of N-methylpyrrolidone, stir and react at 200°C for 15 h, cool to room temperature, place in -10°C ice water for 30 min, solid precipitates, filter, wash the residue with ethanol 3 times, and dry in a vacuum drying oven at 60°C for 1 h to obtain compound I;

[0053] Step A2. Under a nitrogen environment, add 2 g of compound I and 0.2 g of palladium carbon catalyst (Pd loading is 5%) to 50 mL of N,N-dimethylformamide, stir evenly, heat to 80°C, slowly drop 2.2 g of hydrazine hydrate, and after the addition is completed within 6 min, stir the reaction for 30 h. After the reaction is completed, filter while hot to obtain a filtrate; cool the filtrate to room temperature, place it in ice water at -10°C and cool it for 30 min, precipitate a solid, filter it by suction, wash the filter residue with distilled water 3 times, and dry it in a vacuum drying oven at 40°C for 1 h to obtain aminobisindole.

[0054] Preparation Examples 4-6 provide methods for preparing hydrophobic silica.

[0055] Preparation Example 4

[0056] Hydrophobic silica, prepared by the following method:

[0057] Step B1, dissolve 3 g of suberic acid in 40 mL of ethyl acetate, add nano-silica 5g, stirred at 400r / min for 3h at 40℃, centrifuged at 8000r / min, washed with ethanol 3 times, dried at 60℃ and ground to obtain SA-SiO2;

[0058] Step B2: Add 5 g of SA-SiO2 and 2 g of 1-adamantanol to 40 mL of toluene, stir and react at 55 °C at a speed of 400 r / min for 4 h, cool to room temperature, filter, wash with ethanol three times, dry at 60 °C and grind to obtain hydrophobic silica.

[0059] Preparation Example 5

[0060] Hydrophobic silica, prepared by the following method:

[0061] Step B1, dissolve 4 g of suberic acid in 45 mL of ethyl acetate, add nano-silica 5g, stirred at 50°C at a speed of 400r / min for 3.5h, centrifuged at a speed of 9000r / min, washed with ethanol three times, dried at 65°C and ground to obtain SA-SiO2;

[0062] Step B2: Add 5 g of SA-SiO2 and 2.5 g of 1-adamantanol to 50 mL of toluene, stir and react at 60°C at a speed of 400 r / min for 4.5 h, cool to room temperature, filter, wash three times with ethanol, dry at 60°C and grind to obtain hydrophobic silica.

[0063] Preparation Example 6

[0064] Hydrophobic silica, prepared by the following method:

[0065] Step B1, dissolve 5 g of suberic acid in 50 mL of ethyl acetate, add nano-silica 5g, stirred at 60°C at a speed of 400r / min for 4h, centrifuged at a speed of 10000r / min, washed with ethanol three times, dried at 70°C and ground to obtain SA-SiO2;

[0066] Step B2: Add 5 g of SA-SiO2 and 3 g of 1-adamantanol to 60 mL of toluene, stir and react at 65 °C at a speed of 400 r / min for 5 h, cool to room temperature, filter, wash with ethanol three times, dry at 70 °C and grind to obtain hydrophobic silica.

[0067] Embodiment 1-5 provides a liquid crystal frame-sealing adhesive and a preparation method thereof.

[0068] Example 1

[0069] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 60 parts of bisphenol A epoxy resin, 40 parts of epoxy acrylate, 10 parts of hydrophobic silica, 4 parts of aminobisindole, 1 part of organic sodium salt, 2 parts of photoinitiator, 8 parts of thermal curing agent, and 3 parts of silane coupling agent;

[0070] Among them, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 10:3; aminobisindole is prepared by Preparation Example 1; the organic sodium salt is sodium 2,4-diaminobenzenesulfonate; the hydrophobic silica is prepared by Preparation Example 4; the photoinitiator is 2-hydroxy-2-methylpropiophenone; the thermal curing agent is adipic acid dihydrazide; and the silane coupling agent is N-aminoethyl-γ-aminopropyltrimethoxysilane.

[0071] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0072] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator were stirred at a speed of 100 r / min for 20 minutes, and then hydrophobic silica, aminobisindole and organic sodium salt were added, and stirred at a speed of 100 r / min for 30 minutes. Finally, a thermal curing agent and a silane coupling agent were added, and stirred at a speed of 100 r / min for 30 minutes to obtain a liquid crystal frame sealant.

[0073] Example 2

[0074] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 70 parts of bisphenol A epoxy resin, 45 parts of epoxy acrylate, 15 parts of hydrophobic silica, 6 parts of aminobisindole, 1.5 parts of organic sodium salt, 3 parts of photoinitiator, 10 parts of thermal curing agent, and 4 parts of silane coupling agent;

[0075] Among them, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 10:3; aminobisindole is prepared by Preparation Example 2; the organic sodium salt is sodium 2,4-diaminobenzenesulfonate; the hydrophobic silica is prepared by Preparation Example 5; the photoinitiator is diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide; the thermal curing agent is sebacic acid dihydrazide; and the silane coupling agent is γ-glycidyloxypropyl trimethoxysilane.

[0076] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0077] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator were stirred at a speed of 200 r / min for 15 minutes, and then hydrophobic silica, aminobisindole and organic sodium salt were added, and stirred at a speed of 200 r / min for 25 minutes. Finally, a thermal curing agent and a silane coupling agent were added, and stirred at a speed of 200 r / min for 25 minutes to obtain a liquid crystal frame sealant.

[0078] Example 3

[0079] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 80 parts of bisphenol A epoxy resin, 50 parts of epoxy acrylate, 20 parts of hydrophobic silica, 7 parts of aminobisindole, 2 parts of organic sodium salt, 4 parts of photoinitiator, 11 parts of thermal curing agent, and 5 parts of silane coupling agent;

[0080] Among them, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 5:2; aminobisindole is prepared by Preparation Example 3; the organic sodium salt is sodium 2,4-diaminobenzenesulfonate; the hydrophobic silica is prepared by Preparation Example 6; the photoinitiator is 2,2-dimethoxy-2-phenylacetophenone; the thermal curing agent is adipic acid dihydrazide; and the silane coupling agent is a mixture of N-aminoethyl-γ-aminopropyltrimethoxysilane and γ-aminopropyltriethoxysilane in a mass ratio of 1:1.

[0081] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0082] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator were stirred at a speed of 300 r / min for 15 minutes, and then hydrophobic silica, aminobisindole and organic sodium salt were added, and stirred at a speed of 300 r / min for 25 minutes. Finally, a thermal curing agent and a silane coupling agent were added, and stirred at a speed of 300 r / min for 25 minutes to obtain a liquid crystal frame sealant.

[0083] Example 4

[0084] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 90 parts of bisphenol A epoxy resin, 55 parts of epoxy acrylate, 25 parts of hydrophobic silica, 8 parts of aminobisindole, 2.5 parts of organic sodium salt, 4 parts of photoinitiator, 13 parts of thermal curing agent, and 6 parts of silane coupling agent;

[0085] Among them, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 20:7; aminobisindole is prepared by Preparation Example 1; the organic sodium salt is sodium 2,4-diaminobenzenesulfonate; the hydrophobic silica is prepared by Preparation Example 4; the photoinitiator is 2-hydroxy-2-methylpropiophenone; the thermal curing agent is adipic acid dihydrazide; and the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.

[0086] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0087] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator were stirred at a speed of 400 r / min for 20 minutes, and then hydrophobic silica, aminobisindole and organic sodium salt were added, and stirred at a speed of 400 r / min for 30 minutes. Finally, a thermal curing agent and a silane coupling agent were added, and stirred at a speed of 400 r / min for 30 minutes to obtain a liquid crystal frame sealant.

[0088] Example 5

[0089] A liquid crystal frame sealant, comprising the following raw materials in parts by weight: 100 parts of bisphenol A epoxy resin, 60 parts of epoxy acrylate, 30 parts of hydrophobic silica, 10 parts of aminobisindole, 3 parts of organic sodium salt, 5 parts of photoinitiator, 15 parts of thermal curing agent, and 7 parts of silane coupling agent;

[0090] Among them, the bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 10:3; aminobisindole is prepared by Preparation Example 1; the organic sodium salt is sodium 2,4-diaminobenzenesulfonate; the hydrophobic silica is prepared by Preparation Example 4; the photoinitiator is 2-hydroxy-2-methylpropiophenone; the thermal curing agent is adipic acid dihydrazide; and the silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.

[0091] A method for preparing a liquid crystal frame sealant comprises the following steps:

[0092] First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator were stirred at a speed of 500 r / min for 10 minutes, and then hydrophobic silica, aminobisindole and organic sodium salt were added, and stirred at a speed of 500 r / min for 30 minutes. Finally, a thermal curing agent and a silane coupling agent were added, and stirred at a speed of 500 r / min for 20 minutes to obtain a liquid crystal frame sealant.

[0093] In order to verify the comprehensive performance of the liquid crystal frame sealant prepared in Examples 1-5 of the present invention, comparative examples 1-7 are set, which are as follows:

[0094] Comparative Example 1

[0095] Comparative Example 1 is different from Example 1 only in that the bisphenol A epoxy resin is bisphenol A epoxy resin E-44.

[0096] Comparative Example 2

[0097] Comparative Example 2 is different from Example 1 only in that the bisphenol A epoxy resin is bisphenol A epoxy resin E-51.

[0098] Comparative Example 3

[0099] Comparative Example 3 is different from Example 1 only in that an equal mass of 6-aminoindole is used to replace the aminobisindole prepared in Preparation Example 1.

[0100] Comparative Example 4

[0101] Comparative Example 4 is different from Example 1 only in that an equal mass of ethylenediamine is used to replace the aminobisindole prepared in Preparation Example 1.

[0102] Comparative Example 5

[0103] Comparative Example 5 is different from Example 1 only in that the hydrophobic silica prepared in Preparation Example 4 is replaced by an equal mass of nano-silica.

[0104] Comparative Example 6

[0105] Comparative Example 6 is different from Example 1 only in that an equal mass of sodium tert-butoxide is used to replace sodium 2,4-diaminobenzenesulfonate.

[0106] Comparative Example 7

[0107] Comparative Example 7 is different from Example 1 only in that an equal mass of potassium tert-butoxide is used to replace sodium 2,4-diaminobenzenesulfonate.

[0108] In order to verify the comprehensive performance of the liquid crystal frame sealants prepared in Examples 1-5 and Comparative Examples 1-7 of the present invention, the following performance tests were performed respectively.

[0109] (1) Viscosity: The viscosity of the frame sealant is tested using a viscometer at 25°C.

[0110] (2) Bonding strength

[0111] Apply the sealant to the center of the upper surface of glass A, and place glass B perpendicular to glass A and attach the sealant to the center. After attaching, spread the sealant and apply 100mW / cm 2 The glass A and glass B are both ITO glasses, and the surface is coated with PI, with the size of 25mm×40mm×0.7mm;

[0112] (3) High temperature and high humidity resistance

[0113] A. Prepare the bonding test piece by the same method as above, place the bonding test piece in an environment of temperature of 85°C and relative humidity of 85% for 240 hours, test its bonding strength, compare it with the original bonding strength, and calculate the bonding strength loss rate;

[0114] B. Remove the sealing glue to prepare a liquid crystal box, such as Figure 1 As shown, the liquid crystal box is placed in an environment with a temperature of 85°C and a relative humidity of 85% for 240 hours, and then the liquid crystal is observed under a polarizing film to see if it is contaminated. If there is no blue-purple halo phenomenon, it means that the liquid crystal is not contaminated; if there is a blue-purple halo phenomenon, it means that the liquid crystal is contaminated; wherein, Figure 2 This is a picture of a liquid crystal box made of the frame-sealing adhesive obtained in Example 1 after being treated with high temperature and high humidity and observed under a polarizing film; Figure 3 This is a picture of a liquid crystal box made of the frame-sealing adhesive obtained in Comparative Example 4 after being treated with high temperature and high humidity and observed under a polarizing film;

[0115] (4) Moisture permeability

[0116] The frame sealant was first applied with 100mW / cm 2 The film was irradiated with ultraviolet light for 30 seconds, heated at 120°C for 60 minutes, cooled to room temperature, and cut to obtain a film with a diameter of 55 mm and a thickness of 300 μm. The film was placed in a moisture permeability cup, and calcium chloride was added. The film was placed in an environment with a temperature of 85°C and a relative humidity of 85% for 24 hours. The water absorption of calcium chloride was divided by the film area to obtain the moisture permeability.

[0117] The performance test results are shown in Table 1 below.

[0118] Table 1:

[0119]

[0120] It can be seen from Table 1 that the liquid crystal frame sealing adhesives prepared in Examples 1-5 of the present invention have appropriate viscosity, will not cause liquid crystal leakage, have high bonding strength, and have low moisture permeability and small bonding strength loss under high temperature and high humidity environments, while still maintaining excellent bonding performance, and the liquid crystal is not contaminated, and can be widely used in liquid crystal displays.

[0121] By comparing Example 1 with Comparative Examples 1 and 2, it can be seen that the present invention selects a mixture of E-44 and E-51 as bisphenol A epoxy resin to effectively regulate the viscosity of the frame sealing adhesive. The two work synergistically to significantly improve the high temperature and high humidity resistance of the frame sealing adhesive.

[0122] By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that the aminobisindole prepared in the present invention has a special structure, which increases the crosslinking density by combining physical and chemical methods, so that the microstructure of the cured frame sealant is more compact and can still maintain excellent bonding performance under high temperature and high humidity environments; at the same time, combined with Figure 2 , 3 It can be seen that after the high temperature and high humidity treatment, the liquid crystal of the liquid crystal box of Example 1 is not contaminated, while after the high temperature and high humidity treatment, the frame sealing glue of the liquid crystal box of Comparative Example 4 cannot effectively block the entry of water vapor and oxygen, causing the liquid crystal to be contaminated.

[0123] By comparing Example 1 with Comparative Example 5, it can be seen that the hydrophobic silica prepared in the present invention greatly improves the moisture permeability and high temperature and humidity resistance of the frame sealing adhesive compared with nano-silicon dioxide.

[0124] By comparing Example 1 with Comparative Example 6, it can be seen that adding sodium 2,4-diaminobenzenesulfonate to the raw material of the frame sealing glue of the present invention is more helpful than sodium tert-butoxide in improving the high temperature and high humidity resistance of the frame sealing glue; further comparing Comparative Example 6 with Comparative Example 7, it can be seen that the cation-π bond force formed by sodium ions with smaller ionic radius than potassium ions and indole groups is more conducive to improving the rigidity of the molecular chain.

[0125] This specific embodiment is merely an explanation of the present invention and is not a limitation of the present invention. After reading this specification, those skilled in the art may make non-creative modifications to the present embodiment as needed. However, as long as they are within the scope of the claims of the present invention, they are protected by the patent law.

Claims

1. A liquid crystal frame sealant, characterized in that: The invention comprises the following raw materials in parts by weight: 60-100 parts of bisphenol A epoxy resin, 40-60 parts of epoxy acrylate, 10-30 parts of hydrophobic silica, 4-10 parts of aminobisindole, 1-3 parts of organic sodium salt, 2-5 parts of photoinitiator, 8-15 parts of thermal curing agent and 3-7 parts of silane coupling agent; The structural formula of the aminobisindole is: ; The hydrophobic silica is prepared by the following method: Step B1, dissolving suberic acid in ethyl acetate, adding nano-silicon dioxide, stirring and reacting at 40-60° C. for 3-4 hours, filtering, washing, drying and grinding to obtain SA-SiO2; Step B2, adding SA-SiO2 and 1-adamantanol to toluene, stirring and reacting at 55-65° C. for 4-5 hours, cooling to room temperature, filtering, washing, drying, and grinding to obtain hydrophobic silica; In the step B1, the ratio of suberic acid, nano-silicon dioxide and ethyl acetate is 3-5 g:5 g:40-50 mL; In step B2, the ratio of SA-SiO2, 1-adamantanol and toluene is 5 g: 2-3 g: 40-60 mL; The organic sodium salt is sodium 2,4-diaminobenzenesulfonate.

2. The liquid crystal frame sealant according to claim 1, characterized in that: The aminobisindole is prepared by the following method: Step A1, under nitrogen environment, add 5-nitroindole, 1,3-dichloropropane and anhydrous potassium carbonate to N-methylpyrrolidone, stir and react at 180-200° C. for 10-15 hours, cool to room temperature, and then cool in ice water for 10-30 minutes, solid precipitates, filter, wash and dry to obtain compound I; Step A2. Under a nitrogen environment, add compound I and palladium-carbon catalyst to N,N-dimethylformamide, stir evenly, heat to 70-80°C, slowly drop hydrazine hydrate, and after the dropwise addition is completed within 4-6 minutes, stir the reaction for 20-30 hours. After the reaction is completed, filter while hot to obtain a filtrate; cool the filtrate to room temperature, then place it in ice water and cool for 10-30 minutes, precipitate a solid, filter it with suction, wash it, and dry it to obtain aminobisindole.

3. The liquid crystal frame sealant according to claim 2, characterized in that: In the step A1, the ratio of 5-nitroindole, 1,3-dichloropropane, anhydrous potassium carbonate and N-methylpyrrolidone is 3.2-3.5 g: 1-1.1 g: 2.8 g: 30-40 mL; In the step A2, the ratio of compound I, palladium-carbon catalyst, hydrazine hydrate and N,N-dimethylformamide is 1.8-2 g: 0.2 g: 1.9-2.2 g: 30-50 mL; The loading amount of Pd in ​​the palladium-carbon catalyst is 5%.

4. The liquid crystal frame sealant according to claim 1, characterized in that: The bisphenol A epoxy resin is obtained by mixing bisphenol A epoxy resin E-44 and bisphenol A epoxy resin E-51 in a mass ratio of 10:3-4.

5. The liquid crystal frame sealant according to claim 1, characterized in that: The photoinitiator is at least one of diphenyl (2,4,6-trimethylbenzoyl) phosphine oxide, 2-hydroxy-2-methylpropiophenone and 2,2-dimethoxy-2-phenylacetophenone; The thermal curing agent is an organic acid hydrazide; the organic acid hydrazide is at least one of sebacic acid dihydrazide, isophthalic acid dihydrazide, adipic acid dihydrazide and malonic acid dihydrazide.

6. The liquid crystal frame sealant according to claim 1, characterized in that: The silane coupling agent is at least one of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane and N-aminoethyl-γ-aminopropyltrimethoxysilane.

7. A method for preparing a liquid crystal frame sealant according to any one of claims 1 to 6, characterized in that: The following steps are involved: First, bisphenol A epoxy resin, epoxy acrylate and photoinitiator are stirred at a speed of 100-500 r / min for 10-20 minutes, then hydrophobic silica, aminobisindole and organic sodium salt are added, and stirred at a speed of 100-500 r / min for 20-30 minutes, and finally a thermal curing agent and a silane coupling agent are added, and stirred at a speed of 100-500 r / min for 20-30 minutes to obtain a liquid crystal frame sealant.

Citation Information

Patent Citations

  • High-viscosity liquid crystal frame sealing glue

    CN114106742A

  • Low-temperature fast-curing epoxy adhesive for flat transformer

    CN113004846A

  • Epoxy resin adhesive and preparation method thereof

    CN117025151A

  • Adhesive composition and optical semiconductor device

    JP2019019286A

  • Adhesive composition and photosemiconductor device

    JP2020026475A