Collector, flotation reagent and method for flotation of nickel sulfide ore
Through the combined use of collectors a and b and the combination of auxiliary components, the problem of insufficient harvesting capacity of low-grade nickel sulfide ore is solved, significantly improving the recovery rate and selectivity of nickel sulfide ore, and improving nickel resources Utilization.
Patent Information
- Application Number
- CN202411181807.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-27
AI Technical Summary
The existing collectors have poor harvesting capacity for low-grade nickel sulfide ore, and it is difficult to adapt to its complex embedded relationship and low-grade characteristics, resulting in low utilization of nickel metal resources.
Provide a collector containing a specific structure, through the combined use of collectors a and b, enhance the capture capacity and selectivity of nickel sulfide ore, adapt to the flotation requirements of low-grade nickel sulfide ore, and in flotation Add auxiliary ingredients such as inhibitors, activators, and foaming agents to the agent to optimize the effect.
The yield and selectivity of nickel sulfide ore are significantly improved, especially under low grade conditions, which significantly improves the flotation effect of nickel and improves the utilization rate of nickel resources.
Smart Images

Figure CN118698748B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the flotation reagent technology in the field of mineral processing, and specifically relates to the flotation field of nickel sulfide ore, especially low-grade nickel sulfide ore. Background Art
[0002] Low-grade nickel ore has a high degree of corrosion, uneven particle size, difficult dissociation of fine particles, and complex interpenetration relationships between minerals. The nickel-containing minerals are easily crushed and oxidized, and their natural floatability is similar to that of iron-containing minerals. The ore properties of low-grade nickel sulfide ore are extremely unfavorable for improving nickel flotation separation indicators, and it is a difficult-to-process nickel sulfide ore. Improving the flotation index of low-grade nickel sulfide ore is a technical problem that the global nickel industry has long been in urgent need of solving.
[0003] Flotation collectors are the most direct, effective and economical way to improve the nickel flotation index of low-grade nickel sulfide ores. However, there is currently a lack of exclusive collectors for low-grade and difficult-to-treat nickel sulfide ores. Most of the currently used collectors are the same as those for nickel sulfide-rich ores or other sulfide ores, such as BS-4, C-125, PN-405, Y-89, J-622, BK-206, AS-4 and JP-16.
[0004] For example, the Chinese patent document with publication number CN115445777A discloses a method for improving the copper-nickel flotation recovery rate of low-grade copper-nickel sulfide ore, and the specific collectors recorded include sodium butyl xanthate, O-isopropyl-N-ethylthiocarbamate and dibutyl ammonium dithiophosphate. The Chinese patent document with publication number CN115318447A discloses a flotation process suitable for reducing the magnesium oxide content in nickel concentrate and improving the nickel recovery rate of low-grade copper-nickel ore, and the specific collectors disclosed include butyl xanthate and amyl xanthate. For another example, the Chinese patent document with publication number CN115301399A discloses a beneficiation method for high-magnesium low-grade copper-nickel sulfide ore, and specifically discloses a composite collector, wherein the main collector is xanthate and the auxiliary collector is black medicine.
[0005] In summary, the current lean ore flotation industry lacks efficient and highly selective collectors, and the continued use of conventional xanthate collectors can easily lead to problems such as low nickel metal resource utilization. Summary of the invention
[0006] In view of the problem that the existing collectors have unsatisfactory nickel capture capacity and are difficult to adapt to the flotation requirements of low-grade nickel sulfide ores, the present invention provides a collector for flotation of nickel sulfide ores, aiming to improve the nickel capture capacity and make it adapt to the flotation requirements of low-grade nickel sulfide ores.
[0007] The second object of the present invention is to provide a flotation reagent comprising the collector for flotation of nickel sulfide ore.
[0008] The third object of the present invention is to provide a method for flotation of nickel sulfide ore using the collector and a flotation reagent containing the collector.
[0009] High-grade nickel sulfide ores are easy to achieve high-selective flotation. However, low-grade nickel sulfide ores have low grade themselves and have a complex intergrowth relationship with a large number of gangue minerals, which increases the difficulty of flotation exponentially. In view of this problem, the present invention has been studied in depth and provides the following solutions:
[0010] A collector for flotation of nickel sulfide ore, comprising a collector a having a structure of formula 1;
[0011]
[0012] The R 1 C 1 ~C 4 of alkyl.
[0013] The present invention shows that the compound of formula 1 has excellent specific capture ability for nickel sulfide ore, and using it as a collector for nickel sulfide ore can effectively improve the capture rate and selectivity of nickel sulfide ore. In addition, the study shows that the formula 1 is also particularly suitable for the flotation requirements of low-grade nickel sulfide ore, and can improve the capture ability of low-grade nickel sulfide ore.
[0014] The collector for flotation of nickel sulfide ore of the present invention further comprises a collector b, wherein the collector b comprises at least one compound having a structure of Formula 2 or a structure of Formula 3;
[0015]
[0016]
[0017] The R 2 C 1 ~C 4 The alkyl group;
[0018] The R 3 C 8 ~C 16 wherein M is Na, K or NH 4 .
[0019] In the present invention, the collector a and the collector b are innovatively combined to further achieve synergy, and can enhance the capture capacity and selectivity of nickel sulfide ores, and in particular, can further enhance the capture capacity and selectivity of low-grade nickel ores.
[0020] Preferably, the collector b contains a compound of formula 2 and a compound of formula 3. The present invention also shows that when the collector b contains formula 2 and formula 3, and further forms a ternary collection system with the collector a, the synergy between the components can be further achieved, and the nickel collection effect can be further enhanced, especially the collection capacity of low-grade nickel ore can be enhanced.
[0021] Further preferably, in the collector b, the weight ratio of the compound of formula 2 to the compound of formula 3 is 1:0.1-10, and can further be 1:0.5-2.
[0022] In the present invention, the content of the collector a for flotation of nickel sulfide ore is 10wt.% or more, and can be 10-90wt.%, preferably 20-80wt.%, and more preferably 25-50wt.%. The content of the collector b can be 10-90wt.%, and can be 75-50wt.%.
[0023] The present invention also provides a flotation agent for flotation of nickel sulfide ore, which comprises the collector of the present invention and at least one flotation aid selected from the group consisting of an inhibitor, an activator, a frother and a pH regulator.
[0024] The flotation reagent of the present invention, in addition to the collector of the present invention, other components and dosages thereof can be adjusted based on conventional principles and means.
[0025] For example, the inhibitor may be conventional, such as may include at least one of sodium hexametaphosphate, water glass, carboxymethyl cellulose, dextrin, guar gum, lignin, causticized starch, and citric acid.
[0026] The activator may be conventional, for example, may include at least one of copper sulfate, calcium chloride, calcium oxide, oxalic acid, and sodium sulfide.
[0027] The pH regulator may be conventional, for example, may include at least one of ammonium sulfate, sodium carbonate, sodium hydroxide, and sulfuric acid.
[0028] The foaming agent may be conventional, for example, may include at least one of methyl isobutyl carbinol (MIBC), terpineol, cresol oil, and polyethylene glycol ether.
[0029] In the present invention, the components of the flotation reagent exist independently of each other before use, or exist in the form of partial mixing or complete mixing. In addition, the dosage of each component can also be reasonably adjusted according to the flotation needs and efficiency.
[0030] The present invention also provides a method for flotation of nickel sulfide ore, which adopts the collector of the present invention to flotate the ore to be selected containing nickel sulfide ore to obtain nickel sulfide ore concentrate.
[0031] Furthermore, the method for flotation of nickel sulfide ore can use the flotation reagent of the present invention to float the nickel-containing sulfide ore to be selected to obtain the nickel-containing sulfide ore concentrate.
[0032] In the present invention, in the flotation stage, except for the use of the collector of the present invention, other components and operations can be conventional.
[0033] In the present invention, the flotation method can be applied to any nickel grade of the selected minerals, but in order to maximize the flotation value, the selected minerals are particularly selected from low-grade nickel sulfide ores with a nickel content of less than 1 wt.% (for example, 0.1-0.9 wt.%, and further 0.3-0.8 wt.%).
[0034] In the present invention, the dosage of the reagent in the flotation stage can be reasonably regulated based on conventional principles. For example, considering the effect and cost, the dosage of the collector in the flotation stage can be 50-200 g / t, further 60-180 g / t.
[0035] For another example, the flotation aids in the flotation stage include an inhibitor and an activator, wherein the inhibitor is used in an amount of 80-200 g / t, and may further be 100-180 g / t, and the activator is used in an amount of 100-1200 g / t, and may further be 150-300 g / t.
[0036] For another example, there is no special requirement for the pH value in the flotation stage, and it can be, for example, 6 to 9.
[0037] Beneficial Effects
[0038] The research of the present invention shows that the compound of the formula 1 has excellent specific capture ability for nickel sulfide ore. Using it as a collector for nickel sulfide ore can effectively improve the capture rate and selectivity of nickel sulfide ore. In addition, further combining it with collector b can further achieve intermolecular joint synergy, further enhance the flotation ability of nickel, and especially improve the flotation effect of low-grade nickel sulfide ore. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is the flotation flow chart of Example 1. DETAILED DESCRIPTION
[0040] In the present invention, the compound of formula 1 is typically exemplified by formula 1-A, and its specific structure is:
[0041]
[0042] The compound of formula 2 is typically exemplified by formula 2-A, and its specific structure is:
[0043]
[0044] The compound of formula 3 is exemplified by formula 3-A, and its specific structure is:
[0045]
[0046] Comparative structural compounds, the specific structure is:
[0047]
[0048] The mineral to be selected described in the present invention can be a nickel sulfide mineral of any grade, but in order to further verify the capture ability of the collector of the present invention, the present invention particularly selects low-grade nickel sulfide ore. For example, as an optional scheme, the low-grade nickel sulfide ore selected below is the lean ore of Jinchuan No. 2 Mining Area, and its content is as shown in the following cases.
[0049] In the present invention, the collector of the present invention can be used to float the mineral based on conventional flotation means and principles. For example, as an optional embodiment, the flotation process can be as follows:
[0050] Example
[0051] The effect of the collector of the present invention was verified by using a two-stage closed-circuit flotation process. Figure 1 This is a closed circuit flotation flow chart. The steps are:
[0052] Step 1, grinding, each closed-circuit flotation, weigh 800 g of low-grade nickel sulfide ore (Ni grade is 0.67±0.08wt.%), grind until 70% of the mineral particles have a particle size of less than 0.074 mm.
[0053] Step 2: In the first stage flotation operation, the order of adding drugs is inhibitor sodium hexametaphosphate, activator copper sulfate and collector (see the following cases), and the dosage and slurry mixing time are as follows: Figure 1 After the addition of chemicals, 12 minutes of sweeping, 7 minutes of concentration and 4 minutes of concentration were carried out to obtain concentrate 1.
[0054] Step 3: In the second stage flotation operation, the first stage pulp is re-grinded to make 85% of the mineral particles less than 0.074 mm in size, and then the drugs are added. The order of adding drugs is inhibitor sodium hexametaphosphate, activator copper sulfate and collector. The dosage and slurry mixing time are as follows: Figure 1 As shown. After the addition of chemicals, concentrate 2 is obtained through 6 minutes of concentration and 3 minutes of concentration; tailings are obtained through 6 minutes of scavenging and 4 minutes of scavenging. The closed-circuit flotation produces three products: concentrate 1, concentrate 2 and tailings.
[0055] Step 4, results and analysis. Each group of closed-circuit flotation cycles reaches equilibrium after 2 cycles. The results of the embodiment are the average values of the various items obtained after 3-5 cycles. Two groups of flotation closed-circuit experiments were conducted in each implementation case, using collectors respectively, and other conditions were completely the same. The nickel grade / recovery rate of concentrate 1 and concentrate 2 obtained in the two groups of experiments was used to compare the collection effect of the collector of the present invention.
[0056] In the above Figure 1 Based on the flotation of the samples, the collectors and conditions of each case were adjusted. The steps and results were as follows:
[0057] Example 1 - Single Collector Solution
[0058] The collector is a single collector, and the experimental groups are:
[0059] Group A: The collector is of formula 1-A;
[0060] Comparative group a: the collector is formula 2-A;
[0061] Comparative group b: the collector is formula 3-A;
[0062] Comparative group c: the collector is formula 4-A;
[0063] Comparative group d: the collector is sodium ethyl xanthate;
[0064] The results of each group are shown in Table 1:
[0065]
[0066] It can be seen from Example 1 that the use of Formula 1 described in the present invention as a collector can adapt to the characteristics of low-grade nickel sulfide ore and obtain a more ideal collection effect.
[0067] Example 2 - Binary Collector Solution
[0068] The collector is a binary composite collector, and the experimental groups are:
[0069] Group A: The collectors are Formula 1-A and Formula 2-A in a weight ratio of 1:1;
[0070] Group B: The collectors are Formula 1-A and Formula 2-A in a weight ratio of 1:2;
[0071] Group C: The collectors are Formula 1-A and Formula 3-A in a weight ratio of 1:1;
[0072] Comparative group a: the collectors are Formula 2-A and Formula 3-A in a weight ratio of 1:1;
[0073] The results of each group are shown in Table 2:
[0074]
[0075] It can be seen from Examples 1 and 2 that combining Formula 1 with Formula 2 or Formula 3 can further enhance the synergy, adapt to the characteristics of low-grade nickel sulfide ore, and obtain a more ideal capture effect.
[0076] Example 3-Ternary Collector Solution
[0077] The collector is a ternary composite collector, and the experimental groups are:
[0078] Group A: Collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 1:1:1;
[0079] Group B: Collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 2:1:1;
[0080] Group C: Collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 1:2:1;
[0081] Group D: Collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 1:1:2;
[0082] The results of each group are shown in Table 3:
[0083]
[0084] It can be seen from Examples 1 to 3 that the combination of Formula 1, Formula 2 and Formula 3 can further enhance the synergy and further improve the capture effect of low-grade nickel sulfide ore.
[0085] Example 4
[0086] The collector is a ternary composite collector (with different dosages), and the experimental groups are:
[0087] Group A: The collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 2:1:1. The dosage of the collectors in the first and second roughing operations is 60 g / t and 80 g / t respectively.
[0088] Group B: The collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 2:1:1, and the dosage of the collectors in the first and second roughing is 80 g / t and 80 g / t respectively;
[0089] Group C: The collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 2:1:1, and the dosage of the collectors in the first and second roughing is 100 g / t and 80 g / t respectively;
[0090] Group D: The collectors are Formula 1-A, Formula 2-A and Formula 3-A in a weight ratio of 2:1:1, and the dosage of the collectors in the first and second roughing is 120 g / t and 80 g / t respectively;
[0091] The results of each group are shown in Table 4:
[0092]
[0093] It can be seen from Examples 3 and 4 that the combination of Formula 1, Formula 2 and Formula 3 still has an excellent collection effect on low-grade nickel sulfide ores even at a lower collector dosage.
Claims
1. A collector for flotation of nickel sulfide ore, characterized in that: Containing a collector a having a structure of Formula 1; Formula 1; The R1 is a C1~C4 alkyl group.
2. The collector for flotation of nickel sulfide ore according to claim 1, characterized in that: It also comprises a collector b, wherein the collector b comprises at least one compound having a structure of Formula 2 or a structure of Formula 3; Formula 2; Formula 3; The R2 is a C1~C4 alkyl group; The R3 is C8~C 16 The alkyl group is an alkyl group, wherein M is Na, K or NH4.
3. The collector for flotation of nickel sulfide ore according to claim 2, characterized in that: The collector b comprises a compound of formula 2 and a compound of formula 3.
4. The collector for flotation of nickel sulfide ore according to claim 3, characterized in that: In the collector b, the weight ratio of the compound of formula 2 to the compound of formula 3 is 1:0.1-10.
5. The collector for flotation of nickel sulfide ore according to any one of claims 2 to 4, characterized in that: In the collector, the content of the collector a is above 10 wt.%.
6. A flotation agent for flotation of nickel sulfide ore, characterized in that: The collector comprises the collector according to any one of claims 1 to 5, and further comprises at least one flotation aid selected from the group consisting of an inhibitor, an activator, a frother, and a pH adjuster.
7. The flotation reagent for flotation of nickel sulfide ore according to claim 6, characterized in that: The inhibitor comprises at least one of sodium hexametaphosphate, water glass, carboxymethyl cellulose, dextrin, guar gum, lignin, causticized starch, and citric acid; The activator comprises at least one of copper sulfate, calcium chloride, calcium oxide, oxalic acid and sodium sulfide; The pH regulator includes at least one of ammonium sulfate, sodium carbonate, sodium hydroxide and sulfuric acid; The foaming agent comprises at least one of methyl isobutyl carbinol, terpineol, cresol oil and polyethylene glycol ether.
8. A method for flotation of nickel sulfide ore, characterized in that: The collector described in any one of claims 1 to 5 is used to flotate the ore to be selected from the nickel-containing sulfide ore to obtain the nickel-containing sulfide ore concentrate.
9. The method according to claim 8, characterized in that The flotation agent described in any one of claims 6 to 7 is used to float the ore to be selected from the nickel-containing sulfide ore to obtain the nickel-containing sulfide ore concentrate.
10. The method according to claim 9, characterized in that The mineral to be selected is a low-grade nickel sulfide ore with a nickel content of less than 1 wt.%; The dosage of collector in the flotation stage is 50~200 g / t.