A wear-resistant and peel-resistant aluminum-plated film and a preparation method thereof
By using the primer layer prepared by using polyurethane acrylate and other materials in the aluminum-plated film, a nitrogen-containing sulfide structure is formed, which solves the problem of insufficient adhesion of the aluminum foil layer of the aluminum-plated film, and realizes the wear resistance and resistance of the aluminum-plated film. The peeling performance is significantly improved and is suitable for the food and pharmaceutical industries.
Patent Information
- Application Number
- CN202411198786.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The aluminum foil layer of the existing aluminum-plated film materials is insufficiently adhesion, which is prone to wear and fall off, affects the performance and poses safety risks, especially in the food and pharmaceutical industries.
The primer layer is composed of polyurethane acrylate, monofunctional acrylate, adhesion strengthening agent and diluent. The nitrogen-containing sulfide structure is formed through click reaction, which enhances the adhesion of the aluminum-plating layer and is also used to plating the aluminum-plating process. A stable film layer is formed in it to improve the wear resistance and adhesion of the aluminum-plated layer.
It significantly improves the wear resistance and adhesion of the aluminum-plated layer, reduces the peeling of aluminum-plated particles, and shows excellent wear resistance and peeling resistance. It is suitable for non-polar film materials without corona treatment, improving the stability of the film materials. Sex and safety.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite film materials, and in particular relates to a wear-resistant and peel-resistant aluminum-plated film and a preparation method thereof. Background Art
[0002] Aluminum-coated film is a composite flexible packaging material formed by coating an extremely thin layer of metal aluminum on the surface of a plastic film using a special process. The most commonly used processing method is vacuum aluminizing, which is to melt and evaporate metal aluminum at high temperature under a high vacuum state, so that the aluminum vapor precipitates and accumulates on the surface of the plastic film, thereby giving the surface of the plastic film a metallic luster. It has the advantages of light protection, moisture resistance, anti-static, and anti-magnetic field, and is widely used in food, electronics, pharmaceuticals and other industries.
[0003] At present, most aluminized films use PET and BOPP as substrates, among which PET is a polar film material that can be directly evaporated, while BOPP is a non-polar film material that generally requires surface pretreatment, such as corona and plasma treatment, which makes the aluminizing process complicated, and the coating equipment and production lines diverse, which is not conducive to industrialized production. In addition, the aluminum foil layer of the existing aluminized film material has insufficient adhesion and is prone to wear and fall off during use, affecting the performance of the film material. In some fields, such as food and medicine, the detached aluminum poses a safety hazard. In high-precision equipment, the detached aluminum affects the stability of the product. Therefore, the present application aims to disclose a wear-resistant and peeling-resistant aluminized film. Summary of the invention
[0004] In order to solve the technical problems mentioned in the background technology, the purpose of the present invention is to provide a wear-resistant and peel-resistant aluminum-plated film and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A wear-resistant and peel-resistant aluminum-plated film comprises a base film, a primer layer coated on the surface of the base film, and an aluminum-plated layer on the surface of the primer layer.
[0007] The primer includes the following raw materials in parts by weight:
[0008] 50-60 parts of polyurethane acrylate, 25-35 parts of monofunctional acrylate, 16-22 parts of adhesion enhancer, 1.3-1.5 parts of photoinitiator, 0.25-0.3 parts of leveling agent and 8-12 parts of diluent.
[0009] Furthermore, the adhesion enhancer is prepared by the following method:
[0010] Step A1: mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol are mixed, nitrogen is introduced for protection, the temperature is raised to 45-55°C, stirring is applied at 120-150 rpm, ultraviolet irradiation is applied and diallylamine is added intermittently, the total reaction time is controlled to be 3.5-4.5 hours, and ethanol is removed by rotary evaporation after the reaction to obtain an intermediate;
[0011] Furthermore, the dosage ratio of diallylamine, mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol is 0.1mol: 0.21-0.22mol: 15-20mg: 25-30mL. Under the promotion of dimethylphenylphosphine and ultraviolet radiation, the active thiol in mercaptoethanol and the double bond of diallylamine click reaction to form a nitrogen-containing sulfide compound, wherein the nitrogen and sulfur structures can form a stable six-ring chelate structure with the metal.
[0012] Step A2: The intermediate, triethylamine and tetrahydrofuran are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at 0-15° C. in an ice-water bath, and stirring is performed at 240-360 rpm. Methacryloyl chloride is slowly added, and the total reaction time is controlled to be 1.5-2 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, and the substrate is washed with water, and the aqueous phase is removed and vacuum dried to obtain an adhesion enhancer;
[0013] Furthermore, the usage ratio of the intermediate, methacryloyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.2 mol: 5-8 mL: 40-55 mL, and triethylamine is an acid binding agent to promote the esterification of methacryloyl chloride with the terminal hydroxyl groups of the intermediate molecule and introduce terminal acrylate structure modification.
[0014] Furthermore, the monofunctional acrylate is polyethylene glycol methyl ether acrylate.
[0015] Furthermore, the photoinitiator is photoinitiator 1173.
[0016] Furthermore, the diluent is ethyl acetate.
[0017] The method for preparing the wear-resistant and peel-resistant aluminum-plated film comprises the following steps:
[0018] Step S1: premixing polyurethane acrylate, monofunctional acrylate, adhesion enhancer and diluent at high speed, adding photoinitiator and leveling agent, mixing at low speed, and vacuum degassing to obtain a primer;
[0019] Step S2: Take the base film, scrape the primer on the surface, place it in an oven, control the temperature to 45±2°C, and bake for 5-8 minutes to obtain a primer film;
[0020] Furthermore, the scraping thickness of the primer is 20-30 μm.
[0021] Step S3: Send the primer film into the UV vacuum aluminum coating machine for aluminum coating, control the temperature to 35±5℃, and the UV irradiation intensity to 150-200W / m 2 , the primer is cured, and at the same time an aluminum-plated layer is formed on the surface of the primer layer to obtain an aluminum-plated film.
[0022] Furthermore, the thickness of the aluminum plating layer is not greater than 0.08 μm.
[0023] Beneficial effects of the present invention:
[0024] The invention discloses an aluminum-plated film which is a composite film material. The surface of the base film is treated with a primer to improve the wear resistance and adhesion of the aluminum-plated layer. The primer is an acrylate composition, and an adhesion enhancer is added as a functional monomer. The primer is prepared by click addition of mercaptoethanol and diallylamine to form a nitrogen-containing thioether compound, i.e., an intermediate. Then, methacryloyl chloride is esterified with the terminal hydroxyl group of the intermediate molecule to introduce a terminal acrylate structure for modification, i.e., to obtain the adhesion enhancer. During UV vacuum aluminum plating, the nitrogen-containing thioether structure in the adhesion enhancer produces a chelating effect to capture deposited aluminum particles. At the same time, the nitrogen-containing thioether structure in the adhesion enhancer copolymerizes with an acrylate substrate to improve cohesive force, thereby forming a stable film layer on the surface of the base film and strongly adhering the aluminum-plated layer to the surface of the base film. Compared with the traditional aluminum plating process, the invention has no requirements on the properties of the film material, and the non-polar film material does not need corona treatment. The aluminum-plated particles have high bonding strength with the primer layer and are not easy to peel off. They are not easy to fall off during wear, and show excellent wear resistance and peeling resistance in tests. DETAILED DESCRIPTION
[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] 1. Preparation of primer
[0028] 1.1. Take mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol and mix them, introduce nitrogen protection, heat to 55°C, stir at 150rpm, use UVA light source with 300W / m 2 Irradiation, take equal amounts of diallylamine and divide them into three portions, add them intermittently for 30 minutes, continue to irradiate and stir the reaction at a constant temperature after complete addition, and control the total reaction time of diallylamine addition to be 3.5 hours, wherein the dosage ratio of diallylamine, mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.22 mol: 15 mg: 30 mL. After the reaction is completed, remove ethanol by rotary evaporation to obtain an intermediate.
[0029] 1.2. Take the intermediate, triethylamine and tetrahydrofuran, mix them, introduce dry nitrogen for protection, control the temperature at 15°C in an ice-water bath, apply stirring at 360rpm, slowly add methacryloyl chloride within 1 hour, continue to stir at a constant temperature after complete addition, and control the total reaction time of methacryloyl chloride to be 1.5 hours. The amount ratio of the intermediate, methacryloyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.2 mol: 5 mL: 55 mL. After the reaction is completed, remove tetrahydrofuran by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry it in vacuo to obtain an adhesion enhancer.
[0030] 1.3. Ingredients were prepared according to weight: 50 parts of polyurethane acrylate, RU-2261B raw material from Guangdong Ruisheng New Material Technology Co., Ltd. was used in the implementation process; 28 parts of monofunctional acrylate, polyethylene glycol methyl ether acrylate from Hangzhou Yuhao Chemical Technology Co., Ltd. was used in the implementation process; 16 parts of adhesion enhancer, which was prepared in this embodiment; 1.3 parts of photoinitiator, commercially available photoinitiator 1173 was used in the implementation process; 0.25 parts of leveling agent, BYK-354 from BYK Chemical was used in the implementation process; 8 parts of diluent, industrial-grade ethyl acetate was used in the implementation process;
[0031] Polyurethane acrylate, monofunctional acrylate, adhesion enhancer and diluent were added and premixed at 1000 rpm for 5 minutes, then photoinitiator and leveling agent were added and mixed at 60 rpm for 15 minutes, and vacuum degassing was performed for 10 minutes to obtain a primer.
[0032] 2. Preparation of Aluminum Film
[0033] 2.1. Take BOPP film as the base film, scrape the primer on the surface of the base film, control the scraping thickness to 20μm, place it in an oven, control the temperature to 45±2℃, bake for 5min, and obtain a primer film.
[0034] 2.2. Send the base coating film into the UV vacuum aluminum plating machine for aluminum plating. Control the temperature to 35±5℃ and the UV irradiation intensity to 150W / m 2 , the wire feeding rate is set to 800 mm / min, the winding rate is set to 4.5 m / s, the primer is cured, and at the same time, an aluminum-plated layer with a thickness of about 0.05 μm is formed on the surface of the primer layer to obtain an aluminum-plated film.
[0035] Example 2
[0036] 1. Preparation of primer
[0037] 1.1. Take mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol and mix them, introduce nitrogen protection, heat to 45°C, stir at 120rpm, use UVA light source with 250W / m2 Irradiation, take equal amounts of diallylamine and divide them into three parts, add them intermittently for 40 minutes, continue to irradiate and stir the reaction at a constant temperature after complete addition, and control the total reaction time of diallylamine addition to be 4.5 hours, wherein the dosage ratio of diallylamine, mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.21 mol: 20 mg: 25 mL. After the reaction is completed, remove ethanol by rotary evaporation to obtain an intermediate.
[0038] 1.2. Take the intermediate, triethylamine and tetrahydrofuran, mix them, introduce dry nitrogen for protection, control the temperature at 0°C in an ice-water bath, apply stirring at 360rpm, slowly add methacryloyl chloride within 1.2h, continue to stir at a constant temperature after complete addition, and control the total reaction time of methacryloyl chloride to be 2h, wherein the amount ratio of the intermediate, methacryloyl chloride, triethylamine and tetrahydrofuran is 0.1mol:0.2mol:8mL:40mL. After the reaction is completed, remove tetrahydrofuran by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry it in vacuum to obtain an adhesion enhancer.
[0039] 1.3. Ingredients were prepared according to weight: 60 parts of polyurethane acrylate, RU-2261B raw material from Guangdong Ruisheng New Material Technology Co., Ltd. was used in the implementation process; 25 parts of monofunctional acrylate, polyethylene glycol methyl ether acrylate from Hangzhou Yuhao Chemical Technology Co., Ltd. was used in the implementation process; 22 parts of adhesion enhancer, which was prepared in this embodiment; 1.5 parts of photoinitiator, commercially available photoinitiator 1173 was used in the implementation process; 0.3 parts of leveling agent, BYK-354 from BYK Chemical was used in the implementation process; 12 parts of diluent, industrial-grade ethyl acetate was used in the implementation process;
[0040] Polyurethane acrylate, monofunctional acrylate, adhesion enhancer and diluent were added and premixed at 1000 rpm for 5 minutes, then photoinitiator and leveling agent were added and mixed at 60 rpm for 15 minutes, and vacuum degassing was performed for 10 minutes to obtain a primer.
[0041] 2. Preparation of Aluminum Film
[0042] 2.1. Take BOPP film as the base film, scrape the primer on the surface of the base film, control the scraping thickness to 30μm, place it in an oven, control the temperature to 45±2℃, bake for 8min, and obtain a primer film.
[0043] 2.2. Send the base coating film into the UV vacuum aluminum coating machine for aluminum coating. Control the temperature to 35±5℃ and the UV radiation intensity to 200W / m 2 , the wire feeding rate is set to 800 mm / min, the winding rate is set to 4.5 m / s, the primer is cured, and at the same time, an aluminum-plated layer with a thickness of about 0.05 μm is formed on the surface of the primer layer to obtain an aluminum-plated film.
[0044] Example 3
[0045] 1. Preparation of primer
[0046] 1.1. Take mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol and mix them, introduce nitrogen protection, heat to 52°C, stir at 150rpm, use UVA light source with 300W / m 2 Irradiation, take equal amounts of diallylamine and divide them into three parts, add them intermittently for 30 minutes, continue to irradiate and stir the reaction at a constant temperature after complete addition, and control the total reaction time of diallylamine addition to be 4 hours, wherein the amount ratio of diallylamine, mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.22 mol: 18 mg: 30 mL. After the reaction is completed, remove ethanol by rotary evaporation to obtain an intermediate.
[0047] 1.2. Take the intermediate, triethylamine and tetrahydrofuran, mix them, introduce dry nitrogen for protection, control the temperature at 5°C in an ice-water bath, apply stirring at 300rpm, slowly add methacryloyl chloride within 1 hour, continue to stir at a constant temperature after complete addition, and control the total reaction time of methacryloyl chloride to be 1.8 hours. The amount ratio of the intermediate, methacryloyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.2 mol: 6 mL: 50 mL. After the reaction, remove tetrahydrofuran by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry it in vacuum to obtain an adhesion enhancer.
[0048] 1.3. Ingredients were prepared according to weight: 52 parts of polyurethane acrylate, RU-2261B raw material from Guangdong Ruisheng New Material Technology Co., Ltd. was used in the implementation process; 35 parts of monofunctional acrylate, polyethylene glycol methyl ether acrylate from Hangzhou Yuhao Chemical Technology Co., Ltd. was used in the implementation process; 20 parts of adhesion enhancer, which was prepared in this embodiment; 1.4 parts of photoinitiator, commercially available photoinitiator 1173 was used in the implementation process; 0.28 parts of leveling agent, BYK-354 from BYK Chemical was used in the implementation process; 10 parts of diluent, industrial-grade ethyl acetate was used in the implementation process;
[0049] Polyurethane acrylate, monofunctional acrylate, adhesion enhancer and diluent were added and premixed at 1000 rpm for 5 minutes, then photoinitiator and leveling agent were added and mixed at 60 rpm for 15 minutes, and vacuum degassing was performed for 10 minutes to obtain a primer.
[0050] 2. Preparation of Aluminum Film
[0051] 2.1. Take BOPP film as the base film, scrape the primer on the surface of the base film, control the scraping thickness to 25μm, place it in an oven, control the temperature to 45±2℃, bake for 7min, and obtain a primer film.
[0052] 2.2. Send the base coating film into the UV vacuum aluminum plating machine for aluminum plating. Control the temperature at 35±5℃ and the UV irradiation intensity at 180W / m 2 , the wire feeding rate is set to 800 mm / min, the winding rate is set to 4.5 m / s, the primer is cured, and at the same time, an aluminum-plated layer with a thickness of about 0.05 μm is formed on the surface of the primer layer to obtain an aluminum-plated film.
[0053] Comparative Example 1
[0054] This comparative example is a control example of Example 3, using 1,6-hexanediol diacrylate to replace the adhesion enhancer, wherein the formula of the primer is:
[0055] 55 parts of polyurethane acrylate, RU-2261B raw material from Guangdong Ruisheng New Material Technology Co., Ltd. was used in the implementation process; 35 parts of monofunctional acrylate, polyethylene glycol methyl ether acrylate from Hangzhou Yuhao Chemical Technology Co., Ltd. was used in the implementation process; 18 parts of 1,6-hexanediol diacrylate was prepared in this embodiment; 1.5 parts of photoinitiator, commercially available photoinitiator 1173 was used in the implementation process; 0.25 parts of leveling agent, BYK-354 from BYK Chemical was used in the implementation process; 11 parts of diluent, industrial grade ethyl acetate was used in the implementation process; the specific film-making process is exactly the same as that in Example 3.
[0056] Comparative Example 2
[0057] This comparative example uses plasma treatment of the base film, followed by direct vacuum aluminum plating, and the specific implementation process is as follows:
[0058] Plasma treatment: Place the BOPP base film in a plasma treatment system, control the discharge voltage to 7 kV, the discharge current to 0.3 A, nitrogen flow protection, and the winding rate to 100 m / min to obtain the blank film to be plated;
[0059] Vacuum aluminum plating: the blank film to be plated is fed into a vacuum aluminum plating machine, the wire feeding rate is controlled to be 800 mm / min, and the winding rate is controlled to be 4.5 m / s, and an aluminum plating layer with a thickness of about 0.05 μm is formed on the surface of the blank film to be plated to obtain an aluminum-plated film.
[0060] Samples were taken from the aluminized films of the embodiments and comparative examples to test the peel strength of the aluminized layer in accordance with GB 8808-1988 standard; the abrasion resistance of the aluminized layer was tested in accordance with GB / T 1768-2006 standard, and the change rate of the light transmittance of the film before and after abrasion was measured by a 3M transmissometer and recorded as the abrasion rate of the aluminized layer. The specific test data are shown in the following table:
[0061] ;
[0062] It can be seen from the test data in the above table that the aluminum-plated film prepared in the embodiment has more excellent wear resistance and anti-peeling performance.
[0063] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0064] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A wear-resistant and peel-resistant aluminum-plated film, comprising a base film, a primer layer and an aluminum-plated layer, It is characterized in that The primer includes the following raw materials in parts by weight: 50-60 parts of polyurethane acrylate, 25-35 parts of monofunctional acrylate, 16-22 parts of adhesion enhancer, 1.3-1.5 parts of photoinitiator, 0.25-0.3 parts of leveling agent and 8-12 parts of diluent; The adhesion enhancer is prepared by the following method: Step A1: mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol are mixed, nitrogen is introduced for protection, the temperature is raised to 45-55°C, the mixture is stirred and irradiated with ultraviolet light, diallylamine is added intermittently, and the total reaction time is controlled to be 3.5-4.5h. After the reaction is completed, ethanol is removed by rotary evaporation to obtain an intermediate; Step A2: The intermediate, triethylamine and tetrahydrofuran are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at 0-15° C. in an ice-water bath. Methacryloyl chloride is slowly added with stirring. The total reaction time is controlled to be 1.5-2 h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation. The substrate is washed with water, the aqueous phase is removed, and the product is dried in vacuo to obtain an adhesion enhancer.
2. The wear-resistant and peel-resistant aluminum-plated film according to claim 1, It is characterized in that The usage ratio of diallylamine, mercaptoethanol, dimethylphenylphosphine and anhydrous ethanol is 0.1 mol: 0.21-0.22 mol: 15-20 mg: 25-30 mL.
3. The wear-resistant and peel-resistant aluminum-plated film according to claim 2, It is characterized in that The usage ratio of the intermediate, methacryloyl chloride, triethylamine and tetrahydrofuran is 0.1 mol: 0.2 mol: 5-8 mL: 40-55 mL.
4. The method for preparing the wear-resistant and peel-resistant aluminum-plated film according to claim 3, It is characterized in that The steps include: Step S1: premixing polyurethane acrylate, monofunctional acrylate, adhesion enhancer and diluent, then adding photoinitiator and leveling agent, mixing evenly, and vacuum degassing to obtain a primer; Step S2: Take the base film, scrape the primer on the surface, place it in an oven, control the temperature to 45±2°C, and bake for 5-8 minutes to obtain a primer film; Step S3: Send the primer film into the UV vacuum aluminum coating machine for aluminum coating, control the temperature to 35±5℃, and the UV irradiation intensity to 150-200W / m 2 , the primer is cured, and at the same time an aluminum-plated layer is formed on the surface of the primer layer to obtain an aluminum-plated film.
5. The method for preparing the wear-resistant and peel-resistant aluminum-plated film according to claim 4, It is characterized in that The scraping thickness of the primer is 20-30 μm.
6. The method for preparing the wear-resistant and peel-resistant aluminum-plated film according to claim 4, It is characterized in that The thickness of the aluminum plating layer is not higher than 0.08 μm.
7. The method for preparing the wear-resistant and peel-resistant aluminum-plated film according to claim 4, It is characterized in that The monofunctional acrylate is polyethylene glycol methyl ether acrylate.
8. The method for preparing a wear-resistant and peel-resistant aluminum-plated film according to claim 4, It is characterized in that The photoinitiator was photoinitiator 1173.
9. The method for preparing a wear-resistant and peel-resistant aluminum-plated film according to claim 4, It is characterized in that The diluent was ethyl acetate.
Citation Information
Patent Citations
PP mirror coating UV paint and preparation method and construction method thereof
CN117447912A
Multifunctional fireproof and explosion-proof plate and preparation method thereof
CN117774061A