A preparation method of thermal underwear fabric
By combining the modified polyacrylonitrile fiber and viscose fiber with hollow polyester fiber and modal fiber, the problem of insufficient antibacterial, hygroscopic and warm-keeping performance of underwear fabrics is solved, and more efficient moisture absorption and sweating and warming effects are achieved. .
Patent Information
- Application Number
- CN202411204822.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-08-30
AI Technical Summary
The existing underwear fabrics have shortcomings in antibacterial, hygroscopic and warmth, and it is difficult to meet the needs of multifunctional improvement.
By preparing modified polyacrylonitrile fibers and modified viscose fibers and blending them with hollow polyester fibers and modal fibers, a specific chemical modification and weaving process enhances the antibacterial, hygroscopic and warmth properties of the fabric.
It significantly improves the antibacterial, moisture absorption and warmth performance of the fabric, achieving better moisture absorption and sweating effect and antibacterial and anti-fouling functions.
Smart Images

Figure SMS_4 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of fabrics, in particular to a method for preparing thermal underwear fabrics. Background Art
[0002] With the improvement of living standards, people have higher and higher requirements for underwear. In addition to the comfort of underwear fabrics, they also have higher and higher requirements for other functions of underwear fabrics, such as antibacterial properties, moisture absorption, etc. Therefore, it is urgent to improve the multifunctionality of underwear fabrics.
[0003] Viscose fiber is a regenerated cellulose fiber with excellent moisture absorption and air permeability. It is widely used in textile and clothing fabrics and decorative fabrics. Polyacrylonitrile fiber, commonly known as acrylic, is a synthetic fiber made from acrylonitrile copolymer. It has excellent mildew resistance, light resistance, radiation resistance and other properties. It is widely used in various fields. Modal fiber is a cellulose fiber with the characteristics of being comfortable to wear, not easy to fade or yellow, and is widely used in various fabric fields. Hollow polyester fiber has a hollow structure and contains a lot of static air inside, which can form a unique thermal insulation structure. Applying it to fabrics can significantly increase the thermal insulation performance of the fabrics.
[0004] For example, the patent with application publication number CN 116439443 A discloses a skin-friendly antibacterial underwear fabric and its preparation process. The fabric prepared with cotton fiber, modal fiber and polyacrylonitrile fiber as raw materials has excellent antibacterial properties, but does not improve the moisture absorption and warmth retention properties of the fabric. Summary of the invention
[0005] The present invention provides a method for preparing thermal underwear fabrics, by preparing modified polyacrylonitrile fiber and modified viscose fiber, and then blending them to enhance the thermal insulation performance, antibacterial performance and moisture absorption performance of the fabrics, so as to solve the above-mentioned existing problems.
[0006] In order to achieve the above object, the present invention provides a method for preparing a thermal underwear fabric, and the preparation method is as follows:
[0007] Step (1), adding polyacrylonitrile fiber to deionized water, stirring and dispersing, then adding intermediate 3 thereto, using 30% by mass sodium hydroxide solution to control the pH to 7-9, reacting at 120-130° C. for 4-8 hours, after the reaction is completed, washing with deionized water, and drying to obtain modified polyacrylonitrile fiber.
[0008] Step (2), adding viscose fiber to deionized water, stirring and mixing evenly, then adding olefin-modified nano titanium dioxide and ammonium cerium nitrate thereto, controlling the concentration of the ammonium cerium nitrate aqueous solution to be 80-100 mmol / L, reacting at 50-65° C. for 4-10 hours, filtering after the reaction, washing with deionized water, and drying to obtain modified viscose fiber.
[0009] Step (3), blending 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber to form warp threads, blending 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber to form weft threads, placing the warp threads and the weft threads in a weaving machine for weaving, and obtaining thermal underwear fabric.
[0010] Preferably, in step (1), the mass ratio of polyacrylonitrile fiber to intermediate 3 is 100:50-100.
[0011] Preferably, in step (2), the mass ratio of viscose fiber to olefin-modified nano titanium dioxide is 100:50-100.
[0012] Preferably, in step (1), the preparation method of intermediate 3 is:
[0013] S1. Add 3-bromo-5-cyanobenzoic acid and 1,6-hexanediamine to ethanol solvent, stir and disperse, heat to 75-85°C, react for 36-72h, and after the reaction, distill under reduced pressure, wash with ether, and dry to obtain intermediate 1, whose reaction formula is: .
[0014] S2. Add intermediate 1 and 1,3-propanesulfonic acid lactone to methanol solvent, stir and disperse, heat to 60-70°C, react for 24-48 hours, and after the reaction, add sodium carbonate, stir for 1-3 hours, filter, distill under reduced pressure, wash with ether, and dry to obtain intermediate 2, whose reaction formula is: .
[0015] S3. Under hydrogen conditions, add intermediate 2 to ethanol solvent, stir and disperse, then add Raney nickel and sodium hydroxide, control the temperature to 70-90°C, the pressure to 2-3.5MPa, react for 1-3h, and after the reaction is completed, centrifuge, elute, distill under reduced pressure, and dry to obtain intermediate 3, whose reaction formula is: .
[0016] Preferably, in step S1, the molar ratio of 3-bromo-5-cyanobenzoic acid to 1,6-hexanediamine is 2-3.5:1.
[0017] Preferably, in step S2, the molar ratio of the intermediate 1, 1,3-propanesulfonate, and sodium carbonate is 1:2.5-3:4-4.5.
[0018] Preferably, in step S3, the molar ratio of intermediate 2, Raney nickel and sodium hydroxide is 1:1.2-1.6:1.2-1.6.
[0019] Reaction mechanism: The present invention uses 3-bromo-5-cyanobenzoic acid and 1,6-hexanediamine as raw materials, and obtains intermediate 1 through substitution reaction. Intermediate 1 is used to undergo ring-opening alkylation with 1,3-propanesulfonic acid lactone to obtain intermediate 2, which is reduced by the catalysis of Raney nickel to obtain intermediate 3, which is then grafted with polyacrylonitrile fiber to obtain modified polyacrylonitrile fiber. Viscose fiber and olefin-modified nano-titanium dioxide are used as raw materials, and ammonium cerium nitrate is used as an initiator to obtain modified viscose fiber through free radical copolymerization. Finally, the modified viscose fiber is blended with hollow polyester fiber to form a warp, and modal fiber and modified polyacrylonitrile fiber are blended to form a weft. The warp and weft are woven to obtain thermal underwear fabric.
[0020] Beneficial effects: The present invention uses nano titanium dioxide to react with viscose fiber. Nano titanium dioxide has a large specific surface area and is easy to agglomerate. The present invention organicizes it to increase its compatibility with organic matter, so that it can be more evenly dispersed on the viscose fiber. In addition, nano titanium dioxide has a photocatalytic antibacterial effect. Applying it to fabrics can increase the antibacterial properties of the fabrics.
[0021] The hollow polyester fiber used in the present invention has a continuous cavity inside the fiber and contains a large amount of static air. Air is a good heat-insulating medium. Therefore, applying it to fabrics can increase the thermal insulation performance of fabrics. The intermediate 3 prepared by the present invention through a series of reactions has a novel structure and a simple preparation method. It contains a disulfonate structure and a carboxylate structure and has strong water absorption performance. The fabric prepared by grafting and modifying it with polyacrylonitrile and further processing has a good moisture absorption effect. After absorbing the sweat produced by the human body, it can diffuse to the surface layer of the fabric and evaporate, thereby achieving a good moisture absorption and perspiration effect and a moisture absorption and quick-drying effect. The fabric prepared by the present invention has good antibacterial performance, moisture absorption performance and thermal insulation performance after experimental verification. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Preparation method of olefin-modified nano titanium dioxide: add 1 g of nano titanium dioxide to 100 mL of ethanol solvent, stir and disperse, then add 10 mL of vinyltriethoxysilane, stir and mix evenly at 40°C, then add 10 mL of ammonia water, react for 2 hours, after the reaction is completed, filter, wash with ethanol, and dry to obtain olefin-modified nano titanium dioxide.
[0024] Example 1
[0025] (1) Add 0.2 mol of 3-bromo-5-cyanobenzoic acid and 0.1 mol of 1,6-hexanediamine to 200 mL of ethanol solvent, stir and disperse, heat to 85°C, react for 48 hours, and after the reaction is completed, distill under reduced pressure, wash with ether, and dry to obtain intermediate 1.
[0026] (2) 0.1 mol of intermediate 1 and 0.28 mol of 1,3-propanesulfonic acid lactone were added to 200 mL of methanol solvent, stirred and dispersed, heated to 66°C, and reacted for 36 hours. After the reaction was completed, 0.42 mol of sodium carbonate was added, stirred for 2 hours, filtered, distilled under reduced pressure, washed with ether, and dried to obtain intermediate 2.
[0027] (3) Under hydrogen conditions, 0.1 mol of intermediate 2 was added to 200 mL of ethanol solvent and stirred for dispersion. Then, 0.15 mol of Raney nickel and 0.16 mol of sodium hydroxide were added thereto. The temperature was controlled at 80 °C and the pressure was 3.5 MPa. The reaction was carried out for 2 h. After the reaction was completed, the mixture was centrifuged, eluted, distilled under reduced pressure, and dried to obtain intermediate 3.
[0028] (4) Add 50 parts by weight of polyacrylonitrile fiber to 150 parts by weight of deionized water, stir and disperse, then add 25 parts by weight of intermediate 3, use 30% by mass sodium hydroxide solution to control the pH to 8, react at 130°C for 4 hours, and after the reaction is completed, wash with deionized water and dry to obtain modified polyacrylonitrile fiber.
[0029] (5) Add 40 parts by weight of viscose fiber to 100 parts by weight of deionized water, stir and mix evenly, then add 20 parts by weight of olefin-modified nano-titanium dioxide and ammonium cerium nitrate, control the concentration of the ammonium cerium nitrate aqueous solution to 90 mmol / L, react at 65°C for 6 hours, filter after the reaction, wash with deionized water, and dry to obtain modified viscose fiber.
[0030] (6) 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber are blended to form warp threads, 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber are blended to form weft threads, and the warp threads and weft threads are placed in a weaving machine for weaving to obtain thermal underwear fabric.
[0031] Example 2
[0032] (1) 0.25 mol of 3-bromo-5-cyanobenzoic acid and 0.1 mol of 1,6-hexanediamine were added to 200 mL of ethanol solvent, stirred and dispersed, heated to 85°C, and reacted for 72 hours. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain intermediate 1.
[0033] (2) 0.1 mol of intermediate 1 and 0.3 mol of 1,3-propanesulfonic acid lactone were added to 200 mL of methanol solvent, stirred and dispersed, heated to 65°C, and reacted for 48 hours. After the reaction was completed, 0.42 mol of sodium carbonate was added, stirred for 2 hours, filtered, distilled under reduced pressure, washed with ether, and dried to obtain intermediate 2.
[0034] (3) Under hydrogen conditions, 0.1 mol of intermediate 2 was added to 200 mL of ethanol solvent and stirred for dispersion. Then, 0.14 mol of Raney nickel and 0.16 mol of sodium hydroxide were added thereto. The temperature was controlled at 90 °C and the pressure was 2 MPa. The reaction was carried out for 2 h. After the reaction was completed, the mixture was centrifuged, eluted, distilled under reduced pressure, and dried to obtain intermediate 3.
[0035] (4) Add 50 parts by weight of polyacrylonitrile fiber to 150 parts by weight of deionized water, stir and disperse, then add 30 parts by weight of intermediate 3, use 30% by weight sodium hydroxide solution to control the pH to 8, react at 125°C for 6 hours, and after the reaction is completed, wash with deionized water and dry to obtain modified polyacrylonitrile fiber.
[0036] (5) Add 40 parts by weight of viscose fiber to 100 parts by weight of deionized water, stir and mix evenly, then add 25 parts by weight of olefin-modified nano-titanium dioxide and ammonium cerium nitrate, control the concentration of the ammonium cerium nitrate aqueous solution to 80 mmol / L, react at 50°C for 10 hours, filter after the reaction, wash with deionized water, and dry to obtain modified viscose fiber.
[0037] (6) 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber are blended to form warp threads, 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber are blended to form weft threads, and the warp threads and weft threads are placed in a weaving machine for weaving to obtain thermal underwear fabric.
[0038] Example 3
[0039] (1) 0.35 mol of 3-bromo-5-cyanobenzoic acid and 0.1 mol of 1,6-hexanediamine were added to 200 mL of ethanol solvent, stirred and dispersed, heated to 75°C, and reacted for 36 hours. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain intermediate 1.
[0040] (2) 0.1 mol of intermediate 1 and 0.25 mol of 1,3-propanesulfonic acid lactone were added to 200 mL of methanol solvent, stirred and dispersed, heated to 70°C, and reacted for 48 hours. After the reaction was completed, 0.4 mol of sodium carbonate was added, stirred for 2 hours, filtered, distilled under reduced pressure, washed with ether, and dried to obtain intermediate 2.
[0041] (3) Under hydrogen conditions, 0.1 mol of intermediate 2 was added to 200 mL of ethanol solvent and stirred for dispersion. Then, 0.16 mol of Raney nickel and 0.12 mol of sodium hydroxide were added thereto. The temperature was controlled at 90 °C and the pressure was 2 MPa. The reaction was carried out for 1 h. After the reaction was completed, the mixture was centrifuged, eluted, distilled under reduced pressure, and dried to obtain intermediate 3.
[0042] (4) Add 50 parts by weight of polyacrylonitrile fiber to 150 parts by weight of deionized water, stir and disperse, then add 35 parts by weight of intermediate 3, use 30% by weight sodium hydroxide solution to control the pH to 9, react at 120°C for 8 hours, and after the reaction is completed, wash with deionized water and dry to obtain modified polyacrylonitrile fiber.
[0043] (5) Add 40 parts by weight of viscose fiber to 100 parts by weight of deionized water, stir and mix evenly, then add 30 parts by weight of olefin-modified nano-titanium dioxide and ammonium cerium nitrate, control the concentration of the ammonium cerium nitrate aqueous solution to 100 mmol / L, react at 55°C for 4 hours, filter after the reaction, wash with deionized water, and dry to obtain modified viscose fiber.
[0044] (6) 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber are blended to form warp threads, 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber are blended to form weft threads, and the warp threads and weft threads are placed in a weaving machine for weaving to obtain thermal underwear fabric.
[0045] Example 4
[0046] (1) 0.3 mol of 3-bromo-5-cyanobenzoic acid and 0.1 mol of 1,6-hexanediamine were added to 200 mL of ethanol solvent, stirred and dispersed, heated to 80°C, and reacted for 72 hours. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain intermediate 1.
[0047] (2) 0.1 mol of intermediate 1 and 0.3 mol of 1,3-propanesulfonic acid lactone were added to 200 mL of methanol solvent, stirred and dispersed, heated to 60°C, and reacted for 24 hours. After the reaction was completed, 0.45 mol of sodium carbonate was added, stirred for 1 hour, filtered, distilled under reduced pressure, washed with ether, and dried to obtain intermediate 2.
[0048] (3) Under hydrogen conditions, 0.1 mol of intermediate 2 was added to 200 mL of ethanol solvent and stirred for dispersion. Then, 0.15 mol of Raney nickel and 0.16 mol of sodium hydroxide were added thereto. The temperature was controlled at 80 °C and the pressure was 2.5 MPa. The reaction was carried out for 3 h. After the reaction was completed, the mixture was centrifuged, eluted, distilled under reduced pressure, and dried to obtain intermediate 3.
[0049] (4) Add 50 parts by weight of polyacrylonitrile fiber to 150 parts by weight of deionized water, stir and disperse, then add 40 parts by weight of intermediate 3, use 30% by weight sodium hydroxide solution to control the pH to 9, react at 30°C for 4 hours, and after the reaction is completed, wash with deionized water and dry to obtain modified polyacrylonitrile fiber.
[0050] (5) Add 40 parts by weight of viscose fiber to 100 parts by weight of deionized water, stir and mix evenly, then add 35 parts by weight of olefin-modified nano-titanium dioxide and ammonium cerium nitrate, control the concentration of the ammonium cerium nitrate aqueous solution to 90 mmol / L, react at 60°C for 8 hours, filter after the reaction, wash with deionized water, and dry to obtain modified viscose fiber.
[0051] (6) 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber are blended to form warp threads, 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber are blended to form weft threads, and the warp threads and weft threads are placed in a weaving machine for weaving to obtain thermal underwear fabric.
[0052] Example 5
[0053] (1) 0.25 mol of 3-bromo-5-cyanobenzoic acid and 0.1 mol of 1,6-hexanediamine were added to 200 mL of ethanol solvent, stirred and dispersed, heated to 80°C, and reacted for 72 hours. After the reaction was completed, the mixture was distilled under reduced pressure, washed with ether, and dried to obtain intermediate 1.
[0054] (2) 0.1 mol of intermediate 1 and 0.25 mol of 1,3-propanesulfonic acid lactone were added to 200 mL of methanol solvent, stirred and dispersed, heated to 65°C, and reacted for 48 hours. After the reaction was completed, 0.4 mol of sodium carbonate was added, stirred for 3 hours, filtered, distilled under reduced pressure, washed with ether, and dried to obtain intermediate 2.
[0055] (3) Under hydrogen conditions, 0.1 mol of intermediate 2 was added to 200 mL of ethanol solvent and stirred for dispersion. Then, 0.16 mol of Raney nickel and 0.14 mol of sodium hydroxide were added thereto. The temperature was controlled at 70 °C and the pressure was 3.5 MPa. The reaction was carried out for 2 h. After the reaction was completed, the mixture was centrifuged, eluted, distilled under reduced pressure, and dried to obtain intermediate 3.
[0056] (4) Add 50 parts by weight of polyacrylonitrile fiber to 150 parts by weight of deionized water, stir and disperse, then add 50 parts by weight of intermediate 3, use 30% by mass sodium hydroxide solution to control the pH to 7, react at 125°C for 5 hours, and after the reaction is completed, wash with deionized water and dry to obtain modified polyacrylonitrile fiber.
[0057] (5) Add 40 parts by weight of viscose fiber to 100 parts by weight of deionized water, stir and mix evenly, then add 40 parts by weight of olefin-modified nano-titanium dioxide and ammonium cerium nitrate, control the concentration of the aqueous solution of ammonium cerium nitrate to 100 mmol / L, react at 55°C for 8 hours, filter after the reaction, wash with deionized water, and dry to obtain modified viscose fiber.
[0058] (6) 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber are blended to form warp threads, 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber are blended to form weft threads, and the warp threads and weft threads are placed in a weaving machine for weaving to obtain thermal underwear fabric.
[0059] Comparative Example 1
[0060] The difference between this comparative example and Example 1 is that in step (6), viscose fiber is used instead of modified viscose fiber.
[0061] Comparative Example 2
[0062] The difference between this comparative example and Example 1 is that in step (6), polyacrylonitrile fiber is used instead of modified polyacrylonitrile fiber.
[0063] Comparative Example 3
[0064] The difference between this comparative example and Example 1 is that in step (6), polyester fiber is used instead of hollow polyester fiber.
[0065] Refer to GB / T21655.1-2023 to test the hygroscopicity of fabrics.
[0066] Table 1: Hygroscopicity test results of various embodiments and comparative examples
[0067] Water absorption / % Water drop diffusion time / s Wicking height / mm Example 1 109 8.0 89 Example 2 120 6.9 93 Example 3 134 4.8 104 Example 4 151 3.2 110 Example 5 169 2.5 119 Comparative Example 2 98 11.3 72
[0068] The higher the water absorption rate, the shorter the drip diffusion time, the higher the wicking height, and the better the hygroscopicity. As can be seen from the table, the fabric prepared by the present invention has good hygroscopicity.
[0069] Refer to GB / T35762-2017 to test the warmth retention of fabrics.
[0070] Table 2: Test results of thermal insulation performance of various embodiments and comparative examples
[0071] Warmth rate / % Example 1 33.16 Comparative Example 3 23.94
[0072] It can be seen from the table that the fabric prepared by the present invention has a good warmth-keeping effect.
[0073] The fabric was cut into small discs with a diameter of 6 mm, sterilized by ultraviolet light and placed in a sterile container. Staphylococcus aureus and Escherichia coli were inoculated into nutrient broth and cultured at 37 °C for 12 h. The bacterial solution was diluted to 5 × 10 5 cfu / mL bacterial suspension, spread it evenly on a common nutrient agar plate, then place the small disc of fabric on the plate, culture it at 37℃ for 24h, and measure the diameter of the inhibition zone with a vernier caliper.
[0074] Table 3: Antibacterial performance test results of each embodiment and comparative example
[0075]
[0076] It can be seen from the table that the fabric prepared by the present invention has good antibacterial properties.
[0077] The basic principles and main features of the present invention and the advantages of the present invention are shown and described above. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the appended claims rather than the above description, and it is intended that all changes within the meaning and scope of the equivalent elements of the claims are included in the present invention.
Claims
1. A method for preparing thermal underwear fabric, It is characterized in that The preparation method is as follows: Step (1), adding polyacrylonitrile fiber to deionized water, stirring and dispersing, and then adding intermediate 3 therein, the structural formula of which is: , using a sodium hydroxide solution with a mass fraction of 30% to control the pH to 7-9, reacting at 120-130°C for 4-8 hours, and after the reaction is completed, washing with deionized water and drying to obtain modified polyacrylonitrile fiber; Step (2), adding viscose fiber to deionized water, stirring and mixing evenly, then adding olefin-modified nano titanium dioxide and ammonium cerium nitrate thereto, controlling the concentration of the ammonium cerium nitrate aqueous solution to be 80-100 mmol / L, reacting at 50-65° C. for 4-10 hours, filtering after the reaction, washing with deionized water, and drying to obtain modified viscose fiber; Step (3), blending 23 parts by weight of modified viscose fiber and 37 parts by weight of hollow polyester fiber to form warp threads, blending 20 parts by weight of modal fiber and 20 parts by weight of modified polyacrylonitrile fiber to form weft threads, placing the warp threads and weft threads on a weaving machine for weaving, and obtaining thermal underwear fabric; the preparation method of the intermediate 3 is as follows: S1, adding 3-bromo-5-cyanobenzoic acid and 1,6-hexanediamine to ethanol solvent, stirring and dispersing, heating to 75-85°C, reacting for 36-72h, and after the reaction, distilling under reduced pressure, washing with ether, and drying to obtain intermediate 1; S2, adding intermediate 1 and 1,3-propanesulfonate to methanol solvent, stirring and dispersing, heating to 60-70°C, reacting for 24-48 hours, and after the reaction, adding sodium carbonate, stirring for 1-3 hours, filtering, distilling under reduced pressure, washing with ether, and drying to obtain intermediate 2; S3, under hydrogen conditions, adding intermediate 2 to ethanol solvent, stirring and dispersing, then adding Raney nickel and sodium hydroxide thereto, controlling the temperature to 70-90°C, the pressure to 2-3.5MPa, reacting for 1-3h, after the reaction is completed, centrifuging, eluting, distilling under reduced pressure, and drying to obtain intermediate 3; The preparation method of the alkenyl-modified nano titanium dioxide is as follows: 1 g of nano titanium dioxide is added to 100 mL of ethanol solvent, stirred and dispersed, 10 mL of vinyl triethoxysilane is added thereto, stirred and mixed evenly at 40° C., 10 mL of ammonia water is added thereto, reacted for 2 hours, and after the reaction is completed, filtered, washed with ethanol, and dried to obtain the alkenyl-modified nano titanium dioxide.
2. The method for preparing the thermal underwear fabric according to claim 1, It is characterized in that In the step (1), the mass ratio of polyacrylonitrile fiber to intermediate 3 is 100:50-100.
3. The method for preparing the thermal underwear fabric according to claim 1, It is characterized in that In the step (2), the mass ratio of viscose fiber to olefin-modified nano titanium dioxide is 100:50-100.
4. The method for preparing the thermal underwear fabric according to claim 1, It is characterized in that In the step S1, the molar ratio of 3-bromo-5-cyanobenzoic acid to 1,6-hexanediamine is 2-3.5:
1.
5. The method for preparing the thermal underwear fabric according to claim 1, It is characterized in that In the step S2, the molar ratio of the intermediate 1, 1,3-propanesulfonate, and sodium carbonate is 1:2.5-3:4-4.
5.
6. The method for preparing the thermal underwear fabric according to claim 1, It is characterized in that In the step S3, the molar ratio of the intermediate 2, Raney nickel and sodium hydroxide is 1:1.2-1.6:1.2-1.6.
Citation Information
Patent Citations
Skin-friendly antibacterial underwear fabric and preparation process thereof
CN116439443A
Preparation method of modified acrylic fiber
CN107687089A
Cellulose acetate grafted polyacrylonitrile fiber applied home textile fabric
CN110295437A
Antibacterial home textile fabric containing sesbania fibers and preparation method of antibacterial home textile fabric
CN113152082A
Self-cleaning cotton fiber and preparation method thereof
CN114438774A