Nano-zinc oxide antibacterial and bactericidal surface layer material for paper diapers and preparation method of nano-zinc oxide antibacterial and bactericidal surface layer material

By combining lotus leaf fiber, coconut leaf fiber, cassava straw fiber and mountain bark fiber in the diaper surface material, and adding ferromagnesia amphibole powder and copper-aluminum-zinc alloy powder, a nano zinc oxide antibacterial and sterilizing surface layer is formed, which solves the problem of diaper surface The problem of insufficient moisture absorption and air permeability of the layer is eliminated, and the comfort and durability of diapers are improved.

CN118718062AInactive Publication Date: 2024-10-01PINGXIANG XIAORI TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410737434.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing diaper surface materials have deficiencies in hygroscopicity and breathability, leading to skin discomfort and potential allergic reactions, and their low strength and durability can easily lead to urine leakage.

Method used

Nano zinc oxide antibacterial and sterilizing surface material is used. The lotus leaf fiber, coconut leaf fiber, cassava straw fiber and mountain bark strip fiber are melted and combined with magnesia amphibole powder, copper aluminum zinc alloy powder and polyvinyl chloride fiber to form a unique The fiber bundles of the interwoven structure are sprayed on the outer layer through ultrasonic dispersed nano-zinc oxide to enhance the antibacterial and sterilizing effect.

Benefits of technology

It achieves good hygroscopicity, breathability and strength, reduces urine back seepage and skin discomfort, enhances the antibacterial and sterilizing properties of the surface layer, and improves the comfort and durability of diapers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004882205140000091
    Figure BDA0004882205140000091
  • Figure BDA0004882205140000101
    Figure BDA0004882205140000101
  • Figure BDA0004882205140000121
    Figure BDA0004882205140000121
Patent Text Reader

Abstract

The invention provides a nano-zinc oxide antibacterial and bactericidal surface layer material for paper diapers. The surface layer material is divided into an inner layer and an outer layer, and the inner layer material is prepared from the following raw materials in parts by weight: 50-70 parts of lotus leaf fibers, 30-40 parts of coconut leaf fibers, 20-30 parts of cassava stalk fibers and 20-30 parts of szechwan indigo fibers; the outer surface layer material is prepared from the following raw materials in parts by weight: 6 to 10 parts of iron magnesium amphibole powder, 10 to 20 parts of copper aluminum zinc alloy powder, 80 to 100 parts of polyvinyl chloride fiber and 2 to 4 parts of nano zinc oxide. The surface layer material is prepared through the steps of inner layer fiber preparation, outer layer fiber preparation, carding web formation, spunlace reinforcement, dehydration compaction, nano zinc oxide atomization spraying, drying and hot rolling bonding. The nano-zinc oxide antibacterial and bactericidal surface layer material for the paper diaper prepared by the invention not only has excellent hygroscopicity, reverse osmosis performance and air permeability, but also has efficient and stable antibacterial property, the bacteriostasis rate on escherichia coli is 99.5%, and the bacteriostasis rate on staphylococcus aureus is 98.3%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of antibacterial surface layer materials and preparation methods thereof, and in particular to a nano zinc oxide antibacterial and sterilization surface layer material for diapers and a preparation method thereof. Background Art

[0002] Diapers are disposable absorbent articles, usually made of absorbent materials, that absorb urine and prevent it from penetrating to the outside. People who need diapers include infants, incontinent adults, people with limited mobility, bedridden people, people who cannot go to the toilet for a long time, etc. For infants, diapers are essential items in daily care, which can help reduce the burden on parents and reduce the difficulty of cleaning; for incontinent adults and people with limited mobility, diapers can provide a convenient and comfortable use experience, while also reducing the burden on caregivers.

[0003] Diapers are a multi-layer, multi-structure, multi-material composite absorbent structure, generally composed of four parts: the surface layer, the diversion layer, the absorption layer, and the bottom layer. The surface layer is in direct contact with human skin, so it is required to be soft, breathable, and not harmful to the skin. It also needs to have good drying properties, be able to quickly guide urine into the lower diversion layer or the absorption core, and also need to prevent urine from seeping back to the surface of the diaper to a certain extent.

[0004] The surface materials of diapers on the market are mainly spunbond nonwovens, hot air nonwovens and spunlace nonwovens. Spunbond nonwovens have high strength and elasticity, can provide good absorption and quick-drying properties, and also have good tensile strength and durability. However, spunbond nonwovens have poor air permeability, which can easily make the skin feel stuffy and are not suitable for long-term use. Hot air nonwovens have good air permeability and moisture absorption properties, can quickly transfer urine and keep the skin dry and comfortable. At the same time, hot air nonwovens are also soft and warm, which can provide a better user experience. However, the strength and durability of hot air nonwovens are relatively low, and they are easy to be damaged or torn, which can easily cause urine leakage. Spunlace nonwovens have good water absorption and air permeability, can quickly absorb urine and transfer it to the next layer, and also have good softness and durability. However, the raw materials of the spunlace nonwoven materials currently used as the surface layer of diapers are generally cotton, viscose and other fibers, which have strong moisture absorption and water storage capacity, high re-permeability, and easily form a humid surface environment, which gives a poor skin experience and may cause skin problems such as skin allergies, redness and swelling. Summary of the invention

[0005] In view of this, the present invention proposes a nano zinc oxide antibacterial and sterilization surface material for diapers and a preparation method thereof to solve the above problems.

[0006] The technical solution of the present invention is achieved as follows: a nano zinc oxide antibacterial and sterilization surface layer material for diapers, the surface layer material is divided into an inner layer and an outer layer, the inner layer material comprises 50-70 parts of lotus leaf fiber, 30-40 parts of coconut leaf fiber, 20-30 parts of cassava stalk fiber, 20-30 parts of mountain bark fiber, and the outer layer material comprises 6-10 parts of ferromagnesian amphibole powder, 10-20 parts of copper-aluminum-zinc alloy powder, 80-100 parts of polyvinyl chloride fiber, and 2-4 parts of nano zinc oxide.

[0007] Furthermore, the surface layer material is divided into an inner layer and an outer layer. The inner surface layer material includes 60 parts of lotus leaf fiber, 35 parts of coconut leaf fiber, 25 parts of cassava stalk fiber, and 25 parts of mountain bark strip fiber. The outer surface layer material includes 8 parts of ferromagnesian amphibole powder, 15 parts of copper-aluminum-zinc alloy powder, 90 parts of polyvinyl chloride fiber, and 3 parts of nano zinc oxide.

[0008] Furthermore, a method for preparing a nano zinc oxide antibacterial and sterilization surface material for diapers comprises the following steps:

[0009] S1: Preparation of inner layer fiber: Weigh lotus leaf fiber, coconut leaf fiber, cassava stalk fiber, and mountain bark fiber according to weight, mix and place in a mixer, then place in a screw for melting and plasticization to obtain a melt. The melt is sent to a spinning box to obtain an inner layer fiber tow with a fineness of 1.50-1.60 dtex.

[0010] S2: Preparation of outer fiber: Weigh ferromagnesian amphibole powder, copper-aluminum-zinc alloy powder, and polyvinyl chloride fiber by weight, mix and add 3-5 times of flow aid, knead at 150-200°C for 20-30 minutes, and put into a spinning box after kneading and melting to obtain an outer fiber bundle with a fineness of 1.60-1.70 dtex.

[0011] S3: Combing into a web: Combing the inner fiber bundles and the outer fiber bundles into fiber webs respectively.

[0012] S4: Hydroentanglement: The inner and outer fiber webs are hydroentangled by flat mesh hydroentanglement, and four hydroentanglements are used for reinforcement. The hydroentanglement speed is 3-5m / min, of which 1 and 3 are front hydroentanglements, and 2 and 4 are back hydroentanglements.

[0013] S5: Dehydration and compaction: The hydroentangled fiber web is fed into a press, pre-pressed at a pressure of 0.05-0.20 MPa for 1-2 min, and then pressed again at a pressure of 0.30-0.80 MPa for 2-4 min.

[0014] S6: Spraying nano zinc oxide by atomization: Weigh nano zinc oxide by weight, add it to 100-120 parts of deionized water, and place it in an ultrasonic device for ultrasonic dispersion for 20-30 minutes under the conditions of ultrasonic power of 1000-2000W and ultrasonic frequency of 12-20Hz to obtain a nano zinc oxide suspension. The nano zinc suspension is loaded into the atomization spray device, and the outer layer material is sprayed with the nano zinc suspension by atomization, and the atomization spray flow rate is controlled to 30-40mL / min and the gas pressure is controlled to 0.20-0.40Mpa.

[0015] S7: Drying: Place the inner surface layer material obtained in S5 and the outer surface layer material obtained in S6 into a baking machine, bake at 60-80°C for 5-10 minutes, and then bake at 100-130°C for 1-3 minutes.

[0016] S8: Hot rolling bonding: The inner surface layer material and the outer surface layer material obtained in S7 are hot rolled and bonded under the conditions of hot rolling temperature of 140-150°C, hot pressing pressure of 0.10-0.20MPa, and hot rolling speed of 1-1.5m / min to obtain the nano zinc oxide antibacterial and sterilization surface layer material for diapers.

[0017] Furthermore, the stirring rate of the S1 mixer is 200-400 r / min, and the stirring time is 5-15 min.

[0018] Furthermore, the melting temperature of S1 is 250-300°C, and the melting time is 5-20 min.

[0019] Furthermore, the flow aid is mannan, mucin, and olive oil with a mass volume ratio g / mL of (2-3):(1-2):1.

[0020] Furthermore, in S4, the pressure of the first hydroentanglement is 20-25 bar, the pressure of the second hydroentanglement is 30-35 bar, the pressure of the third hydroentanglement is 40-45 bar, and the pressure of the fourth hydroentanglement is 50-55 bar.

[0021] Furthermore, the surface density of the inner layer material obtained by S7 is 35-45g / m 2 , thickness is 0.030-0.040mm, the surface density of the outer layer material is 45-55g / m 2 , thickness is 0.040-0.050mm.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention selects lotus leaf fiber, coconut leaf fiber, cassava stalk fiber, and mountain bark fiber to be melted and made into fiber bundles. The four fibers are mutually infiltrated and interwoven so that the prepared fiber bundles have a unique interwoven structure of warp and weft interwoven forms, and in the melting process, chemical bonding occurs between the four fibers to form a stronger fiber connection, which has both good hygroscopicity and air permeability, and sufficient strength and wear resistance. The present invention adds ferromagnesian amphibole powder when preparing the outer layer material. The ferromagnesian amphibole powder has good hygroscopicity and air permeability, can help urination, keep the skin dry and comfortable, which is very beneficial for preventing baby diaper rash and keeping skin healthy. At the same time, the ferromagnesian amphibole powder can produce a certain warming effect, help promote blood circulation, and relieve muscle fatigue and stiffness caused by wearing diapers. The polyvinyl chloride fiber structure selected by the present invention is relatively tight, which can be used as a supporting skeleton to enhance the overall stability and shape retention of the diaper surface layer, and help the surface layer material to provide certain support and stability after absorbing urine, and prevent the liquid from penetrating into the bottom layer too quickly. At the same time, the present invention adds copper-aluminum-zinc alloy powder when preparing the outer layer material to enhance the shape memory of the diaper surface layer, thereby avoiding deformation caused by movement during the wearing of diapers, thereby causing urine leakage. The addition of aluminum-zinc alloy powder can make the diaper surface layer produce a memory effect according to the human body shape when worn, and is not deformed by external forces, conforming to ergonomics, and more comfortable to wear. The present invention uses a banburying process to obtain an outer fiber bundle with a microporous structure, and nano zinc oxide can be effectively adsorbed on the surface of the outer fiber mesh and form a stable attachment, thereby enhancing the antibacterial and bactericidal effect of the surface layer. Mannan, mucin, and olive oil are added during the banburying process to play a role in plasticization and toughening, enhance the flexibility and elasticity of the outer fiber bundle, and improve the comfort and performance of the outer fiber bundle.

[0023] The invention sprays the nano zinc oxide on the outer layer of the surface material so that the nano zinc oxide does not come into direct contact with the skin, thereby protecting the natural barrier of the skin and reducing the influence of external substances on the skin. DETAILED DESCRIPTION

[0024] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0025] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0026] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0027] Example 1

[0028] A nano zinc oxide antibacterial and sterilizing surface material for diapers, the surface material is divided into an inner layer and an outer layer, the inner layer material comprises 50 parts of lotus leaf fiber, 30 parts of coconut leaf fiber, 20 parts of cassava stalk fiber, and 20 parts of mountain bark fiber, and the outer layer material comprises 6 parts of ferromagnesian amphibole powder, 10 parts of copper-aluminum-zinc alloy powder, 80 parts of polyvinyl chloride fiber, and 2 parts of nano zinc oxide. Nano zinc oxide is added to 100 parts of deionized water, and placed in an ultrasonic device for ultrasonic dispersion for 30 minutes under the conditions of ultrasonic power of 1000W and ultrasonic frequency of 12Hz to obtain a nano zinc oxide suspension for standby use.

[0029] Example 2

[0030] A nano zinc oxide antibacterial and sterilizing surface material for diapers, the surface material is divided into an inner layer and an outer layer, the inner layer material comprises 70 parts of lotus leaf fiber, 40 parts of coconut leaf fiber, 30 parts of cassava stalk fiber, and 30 parts of mountain bark fiber, and the outer layer material comprises 10 parts of ferromagnesian amphibole powder, 20 parts of copper-aluminum-zinc alloy powder, 100 parts of polyvinyl chloride fiber, and 4 parts of nano zinc oxide. Nano zinc oxide is added to 120 parts of deionized water, and placed in an ultrasonic device for ultrasonic dispersion for 30 minutes under the conditions of an ultrasonic power of 1000 W and an ultrasonic frequency of 12 Hz to obtain a nano zinc oxide suspension for standby use.

[0031] Next, the nano zinc oxide antibacterial and sterilization surface layer material for diapers in Example 1 and Example 2 is prepared by the following steps:

[0032] S1: Preparation of inner layer fiber: lotus leaf fiber, coconut leaf fiber, cassava stalk fiber and mountain bark fiber were weighed by weight, mixed and placed in a mixer at 200 r / min for 15 min, then placed in a screw for melt plasticization, and melted at 250°C for 20 min to obtain a melt. The melt was sent to a spinning box to obtain an inner layer fiber tow with a fineness of 1.50 dtex.

[0033] S2: Preparation of outer fiber: Magnesium ferromagnesium amphibole powder, copper aluminum zinc alloy powder, and polyvinyl chloride fiber were weighed by weight, mixed, and 3 times of flow aid was added, the flow aid was composed of mannan, mucin, and olive oil with a mass volume ratio of g / mL of 2:1:1, and kneaded at 150°C for 30 minutes. After kneading and melting, it was put into the spinning box to obtain an outer fiber tow with a fineness of 1.60 dtex.

[0034] S3: Combing into a web: Combing the inner fiber bundles and the outer fiber bundles into fiber webs respectively.

[0035] S4: Hydroentanglement: The inner and outer fiber webs are hydroentangled by flat mesh hydroentanglement, and four hydroentanglements are used for reinforcement. The hydroentanglement speed is 3m / min, the pressure of the first hydroentanglement is 20bar, the pressure of the second hydroentanglement is 30bar, the pressure of the third hydroentanglement is 40bar, and the pressure of the fourth hydroentanglement is 50bar. The first and third hydroentanglements are for the front side, and the second and fourth hydroentanglements are for the back side.

[0036] S5: Dehydration and compaction: The hydroentangled fiber web is fed into a press, pre-pressed at a pressure of 0.050 MPa for 2 min, and then pressed again at a pressure of 0.30 MPa for 4 min.

[0037] S6: Load the nano zinc suspension into the atomizing spray device, and atomize and spray the nano zinc suspension on the outer layer material. The atomizing spray flow rate is controlled to be 30 mL / min and the gas pressure is controlled to be 0.20 MPa.

[0038] S7: Drying: Place the inner surface layer material obtained in S5 and the outer surface layer material obtained in S6 into a baking machine, bake at 60°C for 10 minutes, and then bake at 100°C for 3 minutes; the surface density of the inner surface layer material obtained is 35g / m 2 , thickness is 0.030mm, the surface density of the outer layer material is 45g / m 2 , thickness is 0.040mm.

[0039] S8: Hot rolling bonding: The inner surface layer material and the outer surface layer material obtained in S7 are hot rolled and bonded under the conditions of hot rolling temperature of 140°C, hot pressing pressure of 0.10 MPa, and hot rolling speed of 1 m / min to obtain nano zinc oxide antibacterial and sterilization surface layer material for diapers.

[0040] Example 3

[0041] A nano zinc oxide antibacterial and sterilization surface layer material for diapers, the surface layer material is divided into an inner layer and an outer layer, the inner layer material comprises 60 parts of lotus leaf fiber, 35 parts of coconut leaf fiber, 25 parts of cassava stalk fiber, and 25 parts of mountain bark fiber, and the outer layer material comprises 8 parts of ferromagnesian amphibole powder, 15 parts of copper-aluminum-zinc alloy powder, 90 parts of polyvinyl chloride fiber, and 3 parts of nano zinc oxide.

[0042] Next, a nano zinc oxide antibacterial and sterilization surface material for diapers is prepared by the following steps:

[0043] S1: Preparation of inner layer fiber: lotus leaf fiber, coconut leaf fiber, cassava stalk fiber and mountain bark fiber were weighed by weight, mixed and placed in a mixer at 300 r / min for 10 min, then placed in a screw for melt plasticization, melted at 275°C for 15 min to obtain a melt. The melt was sent to a spinning box to obtain an inner layer fiber tow with a fineness of 1.55 dtex.

[0044] S2: Preparation of outer fiber: Weigh ferromagnesian amphibole powder, copper-aluminum-zinc alloy powder, and polyvinyl chloride fiber by weight, mix and add 4 times of flow aid, the flow aid is composed of mannan, mucin, and olive oil with a mass volume ratio of g / mL of 2.5:1.5:1, and knead at 175°C for 25 minutes. After kneading and melting, put it into the spinning box to obtain an outer fiber bundle with a fineness of 1.65 dtex.

[0045] S3: Combing into a web: Combing the inner fiber bundles and the outer fiber bundles into fiber webs respectively.

[0046] S4: Hydroentanglement: The inner and outer fiber webs are hydroentangled by flat mesh hydroentanglement, and four hydroentanglements are used for reinforcement. The hydroentanglement speed is 3-5m / min, the pressure of the first hydroentanglement is 22.5bar, the pressure of the second hydroentanglement is 32.5bar, the pressure of the third hydroentanglement is 42.5bar, and the pressure of the fourth hydroentanglement is 52.5bar. The first and third hydroentanglements are for the front side, and the second and fourth hydroentanglements are for the back side.

[0047] S5: Dehydration and compaction: The hydroentangled fiber web is fed into a press, pre-pressed at a pressure of 0.13 MPa for 1.5 min, and then pressed again at a pressure of 0.55 MPa for 3 min.

[0048] S6: Spraying nano zinc oxide by atomization: Weigh nano zinc oxide by weight, add it to 110 parts of deionized water, and place it in an ultrasonic device for ultrasonic dispersion for 25 minutes under the conditions of ultrasonic power of 1500W and ultrasonic frequency of 16Hz to obtain a nano zinc oxide suspension. The nano zinc suspension is loaded into the atomization spray device, and the outer layer material is sprayed with the nano zinc suspension by atomization, and the atomization spray flow rate is controlled to 35mL / min and the gas pressure is controlled to 0.30Mpa.

[0049] S7: Drying: Place the inner surface layer material obtained in S5 and the outer surface layer material obtained in S6 into a baking machine, bake at 70°C for 7.5 minutes, and then bake at 115°C for 2 minutes. The surface density of the inner surface layer material obtained is 40g / m 2 , thickness is 0.0350mm, the surface density of the outer layer material is 50g / m 2 , thickness 0.045mm

[0050] S8: Hot rolling bonding: The inner surface layer material and the outer surface layer material obtained in S7 are hot rolled and bonded under the conditions of hot rolling temperature of 145°C, hot pressing pressure of 0.15 MPa, and hot rolling speed of 1.25 m / min to obtain nano zinc oxide antibacterial and sterilization surface layer material for diapers.

[0051] Example 4

[0052] A nano zinc oxide antibacterial and sterilizing surface material for diapers, the surface material is divided into an inner layer and an outer layer, the inner layer material comprises 50 parts of lotus leaf fiber, 30 parts of coconut leaf fiber, 20 parts of cassava stalk fiber, and 20 parts of mountain bark fiber, and the outer layer material comprises 6 parts of ferromagnesian amphibole powder, 10 parts of copper-aluminum-zinc alloy powder, 80 parts of polyvinyl chloride fiber, and 2 parts of nano zinc oxide. Nano zinc oxide is added to 100 parts of deionized water, and placed in an ultrasonic device for ultrasonic dispersion for 30 minutes under the conditions of ultrasonic power of 1000W and ultrasonic frequency of 12Hz to obtain a nano zinc oxide suspension for standby use.

[0053] Example 5

[0054] A nano zinc oxide antibacterial and sterilizing surface material for diapers, the surface material is divided into an inner layer and an outer layer, the inner layer material comprises 70 parts of lotus leaf fiber, 40 parts of coconut leaf fiber, 30 parts of cassava stalk fiber, and 30 parts of mountain bark fiber, and the outer layer material comprises 10 parts of ferromagnesian amphibole powder, 20 parts of copper-aluminum-zinc alloy powder, 100 parts of polyvinyl chloride fiber, and 4 parts of nano zinc oxide. Nano zinc oxide is added to 120 parts of deionized water, and placed in an ultrasonic device for ultrasonic dispersion for 30 minutes under the conditions of an ultrasonic power of 1000 W and an ultrasonic frequency of 12 Hz to obtain a nano zinc oxide suspension for standby use.

[0055] Next, the nano zinc oxide antibacterial and sterilization surface layer material for diapers in Example 4 and Example 5 is prepared by the following steps:

[0056] S1: Preparation of inner layer fiber: lotus leaf fiber, coconut leaf fiber, cassava stalk fiber and mountain bark fiber were weighed by weight, mixed and placed in a mixer at 400 r / min for 5 minutes, then placed in a screw for melt plasticization, and melted at 300°C for 10 minutes to obtain a melt. The melt was sent to a spinning box to obtain an inner layer fiber tow with a fineness of 1.60 dtex.

[0057] S2: Preparation of outer fiber: Weigh ferromagnesian amphibole powder, copper-aluminum-zinc alloy powder, and polyvinyl chloride fiber by weight, mix and add 5 times of flow aid, the flow aid is composed of mannan, mucin, and olive oil with a mass volume ratio of 3:2:1 g / mL, and knead at 200°C for 20 minutes. After kneading and melting, put it into the spinning box to obtain an outer fiber bundle with a fineness of 1.70 dtex.

[0058] S3: Combing into a web: Combing the inner fiber bundles and the outer fiber bundles into fiber webs respectively.

[0059] S4: Hydroentanglement: The inner and outer fiber webs are hydroentangled by flat net hydroentanglement, and four hydroentanglements are used for reinforcement. The hydroentanglement speed is 5m / min, the pressure of the first hydroentanglement is 25bar, the pressure of the second hydroentanglement is 35bar, the pressure of the third hydroentanglement is 45bar, and the pressure of the fourth hydroentanglement is 55bar. The first and third hydroentanglements are for the front side, and the second and fourth hydroentanglements are for the back side.

[0060] S5: Dehydration and compaction: The hydroentangled fiber web is fed into a press, pre-pressed at a pressure of 0.20 MPa for 1 min, and then pressed again at a pressure of 0.80 MPa for 2 min.

[0061] S6: Load the nano zinc suspension into the atomizing spray device, and atomize and spray the nano zinc suspension on the outer layer material. The atomizing spray flow rate is controlled to be 40 mL / min and the gas pressure is controlled to be 0.40 MPa.

[0062] S7: Drying: Place the inner layer material obtained in S5 and the outer layer material obtained in S6 into a baking machine, bake at 80°C for 5 minutes, and then bake at 130°C for 1 minute. The surface density of the inner layer material obtained is 45g / m 2 , thickness is 0.040mm, the surface density of the outer layer material is 55g / m 2 , thickness is 0.050mm.

[0063] S8: Hot rolling bonding: The inner surface layer material and the outer surface layer material obtained in S7 are hot rolled and bonded at a hot rolling temperature of 150°C, a hot pressing pressure of 0.20 MPa, and a hot rolling speed of 1.5 m / min to obtain a nano zinc oxide antibacterial and sterilization surface layer material for diapers.

[0064] Comparative Example 1

[0065] The difference between this comparative example and Example 3 is that the outer surface layer material does not contain ferromagnesian amphibole powder.

[0066] Comparative Example 2

[0067] The difference between this comparative example and Example 3 is that the outer surface layer material does not contain copper-aluminum-zinc alloy powder.

[0068] Comparative Example 3

[0069] The difference between this comparative example and Example 3 is that the flow aid is an equal mass of olive oil.

[0070] Comparative Example 4

[0071] The difference between this comparative example and implementation 3 is that the inner surface layer material includes 75 parts of lotus leaf fiber, 43 parts of coconut leaf fiber, 34 parts of cassava stalk fiber, and 37 parts of mountain bark strip fiber, and the outer surface layer material includes 3 parts of ferromagnesian amphibole powder, 8 parts of copper-aluminum-zinc alloy powder, 110 parts of polyvinyl chloride fiber, and 1 part of nano zinc oxide.

[0072] 1. Liquid penetration time measurement

[0073] Referring to the requirements of GB / T 24218.3-2010, a liquid penetrometer was used for measurement. The surface materials prepared in Examples 1-5 and Comparative Examples 1-4 were cut into samples of 125 mm × 125 mm in size, and then placed flat on the standard absorbent pad of the penetrometer test platform, with the front of the surface material facing up. 5 mL of artificial urine was measured and continuously added to the penetration plate through a burette and a funnel. When the liquid contacts the surface material, the timing is started, and the time for all liquids to penetrate is recorded after the reading is stable. Each sample is tested 3 times and the average value is taken. The test results are shown in Table 1.

[0074] 2. Air permeability measurement

[0075] Referring to the requirements of GB / T 5453-1997, the air permeability of the surface materials prepared in Examples 1-5 and Comparative Examples 1-4 was measured using an air permeability meter. The surface materials prepared in Examples 1-5 and Comparative Examples 1-4 were cut into samples of 5 cm×4 cm in size and tested under a pressure difference of 200 Pa. Each sample was tested 10 times and the average value was taken. The test results are shown in Table 1.

[0076] 3. Determination of moisture regeneration

[0077] Referring to the requirements of GB / T 24218.14-2010, take the sample after the liquid penetration time is determined, place a 6kg block with a bottom size of 15cm×15cm on the sample for 3 minutes; then place a medium-speed qualitative filter paper of known mass on the tested material, and place the block on the filter paper for 2 minutes, record the mass of the liquid absorbed by the filter paper as the rewetting amount, test each sample 3 times, take the average value, and the test results are shown in Table 1.

[0078] 4. Determination of breaking strength

[0079] Referring to the requirements of GB / T 24218.3-2010, the tensile tester was used to measure the breaking strength of the surface layer materials prepared in Examples 1-5 and Comparative Examples 1-4. The surface layer materials prepared in Examples 1-5 and Comparative Examples 1-4 were cut into specimens of 20 cm×5 cm in size, and each specimen was tested 5 times to take the average value. The test results are shown in Table 1.

[0080] Table 1

[0081]

[0082]

[0083] It can be seen from Table 1 that the nano zinc oxide antibacterial and sterilization surface material for diapers prepared by the present invention has the advantages of large air permeability, short penetration time, small rewetting amount, high breaking strength, etc., especially Example 3 has a better effect.

[0084] Compared with Comparative Example 1, when urine contacts the surface layer containing ferromagnesian ... Magnesium ferromagnesium quartz powder has high hardness and wear resistance. When magnesium ferromagnesium quartz powder is added to the surface material of diapers, the strength and durability of the surface material can be increased. Therefore, compared with comparative example 1, the breaking strength of example 3 is higher.

[0085] Compared with Comparative Example 2, in the process of preparing the outer fiber layer, the copper-aluminum-zinc alloy powder and the polyvinyl chloride fiber are interfacially bonded, so that a strong bonding interface is formed between the alloy powder particles and the fiber matrix, forming a metal-based composite fiber structure. This interfacial bonding can effectively transfer stress, thereby improving the load-bearing capacity and strength of the outer fiber layer, so the surface layer material prepared therefrom also has a higher breaking strength.

[0086] Compared with Comparative Example 3, when mannan and mucin are added as flow aids, mannan and mucin, as polymer substances, can penetrate into the interface of the fiber during mixing to form an adhesion layer. At the same time, the molecular chains of mannan and mucin can form a bridging structure between adjacent fibers to tightly bind the fibers together, so that the prepared outer fiber has a higher breaking strength. At the same time, the polymer chains occupy a large amount of space in the mixed mixture, forming a steric hindrance. This steric hindrance can reduce the mutual attraction of molecules on the surface of the liquid, thereby reducing the surface tension of the fiber, so that the surface layer of the diaper prepared therefrom has good penetration performance. Mannan and mucin help the fiber absorb and disperse urine faster, reduce the residence time of urine on the fiber surface, and thus reduce the amount of rewetting.

[0087] Comparison of Example 3 with Comparative Example 4 shows that the ratio of each raw material is extremely important, and a reasonable combination has a significant impact on the penetration time, air permeability, moisture resorption, and breaking strength of the diaper surface material. Only by formulating materials with a specific ratio can a diaper with better performance be obtained.

[0088] A comparative example was added to carry out the determination of antibacterial and bactericidal properties.

[0089] Comparative Example 5

[0090] The difference between this comparative example and Example 3 is that the raw materials do not contain nano zinc oxide.

[0091] 4. Antibacterial Determination

[0092] Referring to the requirements of GB / T 20944.3-2008, the surface layer materials prepared in Example 3 and Comparative Example 5 were tested for antibacterial properties. Escherichia coli and Staphylococcus aureus were selected as test bacteria. 20 mL of nutrient broth was added to a 100 mL conical flask, and 0.4 mL of Escherichia coli and Staphylococcus aureus were inoculated into two conical flasks respectively. The culture was shaken at 37°C and 130 r / min for 20 h. The concentration of the culture solution after culture was 10 7 CFU / mL. Dilute the broth 20 times with distilled water to adjust the bacterial concentration to 1×10 5 -3×10 5 CFU / mL, used as inoculum.

[0093] The surface layer materials prepared in Example 3 and Comparative Example 5 were cut into 2 mm × 2 mm samples, and 0.4 g of each sample was weighed and placed in a conical flask. Six portions of each sample were taken for testing, and two empty conical flasks were taken as a control group. All conical flasks were placed in a sterilizer and sterilized at 121°C for 15 min.

[0094] Add 5 mL of diluted Escherichia coli bacterial solution to three conical flasks containing samples of surface materials of Example 3 and Comparative Example 5 respectively; add 5 mL of diluted Staphylococcus aureus bacterial solution to three conical flasks containing samples of surface materials of Example 3 and Comparative Example 5 respectively; prepare two blank conical flasks, add 5 mL of diluted Escherichia coli bacterial solution to one conical flask, and add 5 mL of diluted Staphylococcus aureus bacterial solution to the other conical flask. Place the above 8 conical flasks in a constant temperature shaking incubator and culture at 24°C and 150 r / min for 18 hours.

[0095] After 18 hours of shaking contact, dilute the bacterial solution in the conical flask 10 times and apply it to the plate. Then put the plate in an incubator and culture it at 37°C for 24 hours. Count the number of colonies on each plate and calculate the inhibition rate according to the following formula:

[0096]

[0097] Where Y is the inhibition rate, in %; A is the concentration of the bacterial solution in the conical flask after the blank control sample is shaken and contacted with the bacterial solution, in CFU / mL; B is the concentration of the bacterial solution in the conical flask after the sample is shaken and contacted with the bacterial solution, in CFU / mL. The test results are shown in Table 2:

[0098] Table 2

[0099] Example 3 Comparative Example 5 Escherichia coli inhibition rate (%) 99.5 79.3 Staphylococcus aureus inhibition rate (%) 98.3 80.6

[0100] As shown in Table 2, the surface material prepared by the present invention has good antibacterial and bactericidal properties. Compared with Comparative Example 5, the nano zinc oxide in Example 3 has a large specific surface area and a high curvature, which enables it to directly contact with microorganisms. Its surface also has certain charge characteristics, which can adsorb negatively charged substances on the surface of microorganisms and interfere with their cell structure, thereby achieving an antibacterial effect. When nano zinc oxide contacts microorganisms, zinc ions will be continuously released, and the bactericidal effect will be achieved by destroying the normal structural function of the cell membrane and causing protein denaturation. Moreover, after killing bacteria, zinc ions can be freed from the cells, and the above process is repeated, thereby achieving a stable and lasting antibacterial effect.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A nano zinc oxide antibacterial and sterilization surface material for diapers, characterized in that: The surface layer material is divided into an inner layer and an outer layer. The inner layer material includes the following raw materials by weight: 50-70 parts of lotus leaf fiber, 30-40 parts of coconut leaf fiber, 20-30 parts of cassava stalk fiber, and 20-30 parts of mountain bark fiber. The outer layer material includes the following raw materials by weight: 6-10 parts of ferromagnesian amphibole powder, 10-20 parts of copper-aluminum-zinc alloy powder, 80-100 parts of polyvinyl chloride fiber, and 2-4 parts of nano zinc oxide.

2. The nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 1, characterized in that: The surface layer material is divided into an inner layer and an outer layer. The inner surface layer material includes the following raw materials by weight: 60 parts of lotus leaf fiber, 35 parts of coconut leaf fiber, 25 parts of cassava stalk fiber, and 25 parts of mountain bark fiber. The outer surface layer material includes the following raw materials by weight: 8 parts of ferromagnesian amphibole powder, 15 parts of copper-aluminum-zinc alloy powder, 90 parts of polyvinyl chloride fiber, and 3 parts of nano zinc oxide.

3. The method for preparing the nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 1 or 2, characterized in that: The following steps are involved: S1: Preparation of inner layer fiber: lotus leaf fiber, coconut leaf fiber, cassava stalk fiber and mountain bark fiber are weighed by weight, mixed and placed in a mixer for stirring, and then placed in a screw for melting and plasticization to obtain a melt; the melt is sent to a spinning box to obtain an inner layer fiber tow with a fineness of 1.50-1.60 dtex; S2: Preparation of outer fiber: Weigh ferromagnesian amphibole powder, copper-aluminum-zinc alloy powder, and polyvinyl chloride fiber by weight, mix and add 3-5 times of flow aid, knead at 150-200°C for 20-30 minutes, and put into a spinning box after kneading and melting to obtain an outer fiber tow with a fineness of 1.60-1.70 dtex; S3: Combing into a web: combing the inner fiber bundles and the outer fiber bundles into a fiber web respectively; S4: Hydroentanglement: The inner and outer fiber webs are hydroentangled by flat mesh hydroentanglement, and four hydroentanglements are used for reinforcement. The hydroentanglement speed is 3-5m / min, of which 1 and 3 are front hydroentanglements, and 2 and 4 are back hydroentanglements. S5: Dehydration and compaction: The hydroentangled fiber web is fed into a press, pre-pressed at a pressure of 0.05-0.20 MPa for 1-2 min, and then pressed again at a pressure of 0.30-0.80 MPa for 2-4 min; S6: spraying nano zinc oxide by atomization: weigh nano zinc oxide by weight, add it to 100-120 parts of deionized water, and put it into an ultrasonic device for ultrasonic dispersion for 20-30 minutes under the conditions of ultrasonic power of 1000-2000W and ultrasonic frequency of 12-20Hz to obtain a nano zinc oxide suspension; load the nano zinc suspension into the atomization spray device, spray the nano zinc suspension on the outer layer material by atomization, and control the atomization spray flow rate to 30-40mL / min and the gas pressure to 0.20-0.40Mpa; S7: Drying: placing the inner surface layer material obtained in S5 and the outer surface layer material obtained in S6 into a baking machine, baking at 60-80°C for 5-10 minutes, and then baking at 100-130°C for 1-3 minutes; S8: Hot rolling bonding: The inner surface layer material and the outer surface layer material obtained in S7 are hot rolled and bonded under the conditions of hot rolling temperature of 140-150°C, hot pressing pressure of 0.10-0.20MPa, and hot rolling speed of 1-1.5m / min to obtain the nano zinc oxide antibacterial and sterilization surface layer material for diapers.

4. The method for preparing a nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 3, characterized in that: The stirring rate of the S1 mixer is 200-400 r / min, and the stirring time is 5-15 min.

5. The method for preparing the nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 3, characterized in that: The melting temperature of S1 is 250-300°C, and the melting time is 5-20min.

6. The method for preparing the nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 3, characterized in that: The flow aid in S2 is mannan, mucin and olive oil with a mass volume ratio of g / mL of (2-3):(1-2):

1.

7. The method for preparing the nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 3, characterized in that: In the S4, the pressure of the first hydroentanglement is 20-25 bar, the pressure of the second hydroentanglement is 30-35 bar, the pressure of the third hydroentanglement is 40-45 bar, and the pressure of the fourth hydroentanglement is 50-55 bar.

8. The method for preparing the nano zinc oxide antibacterial and sterilization surface material for diapers according to claim 3, characterized in that: The surface density of the inner surface layer material obtained in S7 is 35-45g / m 2 , thickness is 0.030-0.040mm, the surface density of the outer layer material is 45-55g / m 2 , thickness is 0.040-0.050mm.

Citation Information

Patent Citations

  • Health functional dry paper diaper with high body surface antibacterial property, super hydroscopicity and gas permeability

    CN104975365A

  • Novel antibacterial textile fabric special for infants and preparing method thereof

    CN105239389A

  • Soft antibacterial and deodorizing baby paper diaper

    CN107260405A

  • Preparation method of coconut leaf fiber

    CN113550016A

  • Nano-zinc antibacterial tissue and preparation method thereof

    CN117431774A