Preparation method and application of bone repair composite material
By polymerizing magnesium oxide and lactide monomers in bone repair composite materials to form magnesium oxide grafted polylactic acid, the problems of poor mechanical properties and acidic degradation of polylactic acid are solved, and the mechanical properties and biocompatibility of the material are improved. , promotes the osteogenesis process.
Patent Information
- Application Number
- CN202410724925.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
Polylactic acid has poor mechanical properties in bone repair applications, the acidic degradation products lead to local inflammatory reactions, and magnesium oxide is prone to agglomeration in the polylactic acid matrix, reducing the mechanical properties of composite materials.
By causing magnesium oxide to undergo a hydration reaction under heating conditions and polymerizing with lactide monomer, magnesium oxide grafted polylactic acid is formed, which is dispersed in the polylactic acid, thereby improving the dispersion of magnesium oxide in the polylactic acid matrix and improving mechanical properties. performance and avoid acidic degrading environments through the synergistic effect of magnesium oxide and polylactic acid.
It improves the mechanical properties of bone repair composite materials, promotes osteoblast differentiation, reduces tissue inflammation, and ensures the stability and biocompatibility of composite materials during the degradation process.
Smart Images

Figure HDA0004878329750000011 
Figure HDA0004878329750000021 
Figure HDA0004878329750000031
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of biofunctional polymer materials, and in particular to a method for preparing a bone repair composite material. Background Art
[0002] As a biodegradable polymer approved by the U.S. Food and Drug Administration (FDA), polylactic acid has good biocompatibility and can be degraded into water and carbon dioxide after implantation. The degradation products are non-toxic and can be excreted from the body through normal metabolism. However, polylactic acid lacks osteogenic activity, has poor mechanical properties, and its degradation products are acidic and easily induce local inflammatory reactions, thus affecting tissue regeneration. In addition, polylactic acid is hydrophobic, which hinders the proliferation and differentiation of osteoblasts.
[0003] Magnesium is an essential element in the human body and has an important impact on life activities. Magnesium usually exists in the form of ions, and its content is second only to calcium, sodium, and potassium. Magnesium can promote calcium deposition, promote the formation of bone cells, and accelerate bone healing. Magnesium oxide has good biocompatibility, and its degradation products are alkaline. After being compounded with polylactic acid, it maintains the pH value of the implant environment through synergistic effects. However, after magnesium oxide is compounded with polylactic acid, it is easy to "agglomerate" in the polylactic acid matrix, thereby reducing the mechanical properties of the composite material. Modifying magnesium oxide is one of the methods to increase the dispersibility of magnesium oxide, which can effectively improve the mechanical properties of magnesium oxide composite polylactic acid materials. Summary of the invention
[0004] The present application aims to solve at least one of the technical problems existing in the prior art. To this end, one purpose of the present application is to propose a preparation method of a bone repair composite material to improve the mechanical properties of the composite material.
[0005] The present application provides a method for preparing a bone repair composite material, comprising the following steps:
[0006] (A) causing magnesium oxide to undergo a hydration reaction under heating conditions;
[0007] (B) polymerizing the hydrated magnesium oxide with a lactide monomer to form magnesium oxide-grafted polylactic acid;
[0008] (C) Dispersing magnesium oxide grafted with polylactic acid in polylactic acid to form a bone repair composite material.
[0009] In any embodiment, the heating temperature is 40-100° C., and the hydration reaction time is 0.5-8 h.
[0010] In any embodiment, in step (A), the ratio of the mass of magnesium oxide to the mass of water is 1:5-1:10.
[0011] In any embodiment, in step (A), the particle size of magnesium oxide is 5-100 μm.
[0012] In any embodiment, in step (A), after the hydration reaction is completed, the solid phase is separated from the hydration reaction solution by vacuum drying at 40-80° C. for 20-40 hours.
[0013] In any embodiment, in step (B), the magnesium oxide subjected to hydration reaction is 0.1-20 parts by mass, the lactide monomer is 80-99.9 parts by mass, and the molar ratio of the catalyst to the lactide monomer is 0.1% to 0.5%.
[0014] In any embodiment, in step (B), the polymerization reaction is carried out in an anhydrous and oxygen-free environment, the polymerization reaction temperature is 110-160° C., and the polymerization reaction time is 12-30 hours.
[0015] In any embodiment, in step (C), the viscosity average molecular weight of the polylactic acid is 50 kDa-150 kDa.
[0016] In any embodiment, in step (C), the amount of magnesium oxide is 0.1-30 parts by mass, and the amount of polylactic acid is 70-99.9 parts by mass.
[0017] In any embodiment, in step (C), the polylactic acid is in the form of a solution, and the concentration of the polymer solution is 5 to 20 g / mL.
[0018] Another purpose of the present application is to propose the application of the bone repair composite material obtained by the above preparation method.
[0019] The bone repair composite material obtained by the above preparation method is used in cell-compatible materials.
[0020] The bone repair composite material obtained by the above preparation method is used in osteogenic active materials.
[0021] In the preparation method disclosed in the present application, the magnesium oxide particles are subjected to a hydration reaction, which can achieve the purpose of increasing the grafting rate. The magnesium oxide particles subjected to the hydration reaction are polymerized in situ with the lactide monomer to obtain magnesium oxide grafted polylactic acid, and the magnesium oxide grafted polylactic acid is dispersed in the polylactic acid, which effectively improves the "agglomeration phenomenon" of magnesium oxide in the polylactic acid matrix, and can improve the mechanical properties of the polylactic acid-based composite material. At the same time, under the synergistic effect of magnesium oxide and polylactic acid, the problem of the acidic degradation environment of polylactic acid can be effectively avoided. At the same time, the composite material continuously and slowly releases magnesium ions during the degradation process, which can promote osteoblast differentiation, and under the synergistic effect of magnesium oxide and polylactic acid, the acidic degradation environment of polylactic acid can be avoided, reducing the occurrence of tissue inflammation. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.
[0023] Figure 1 Fourier transform infrared spectra of magnesium oxide modified by melt copolymerization (A) and solution copolymerization (B) at different temperatures provided in the examples of the present application.
[0024] Figure 2 The X-ray diffraction patterns of magnesium oxide modified by melt copolymerization (A) and solution copolymerization (B) at different temperatures provided in the examples of the present application.
[0025] Figure 3 Scanning electron microscope images of magnesium oxide modified by melt copolymerization (A) and solution copolymerization (B) provided in the examples of the present application.
[0026] Figure 4(a) is a mechanical property test diagram of the left-handed polylactic acid film (PLLA), magnesium oxide composite polylactic acid film (MgO / PLLA), and magnesium oxide modified polylactic acid-based composite material film (g-MH-SC / PLLA) modified by solution copolymerization provided in the examples of the present application.
[0027] FIG4( b ) is a graph showing the mechanical properties of the g-SC / PLLA composite material membrane provided in an embodiment of the present application.
[0028] Figure 5 The following are test graphs of the contact angles of water at room temperature for the PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film provided in the embodiments of the present application.
[0029] Figure 6 Surface and cross-sectional scanning electron microscope images of the PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film provided in the examples of the present application.
[0030] FIG7( a ) shows the staining of live cells and dead cells on the PLLA membrane, MgO / PLLA membrane, and g-MH-SC / PLLA membrane provided in the examples of the present application after culturing for 1 and 3 days.
[0031] FIG. 7( b ) shows the staining of live cells and dead cells on the g-SC / PLLA membrane after 1 and 3 days of culture provided in the examples of the present application.
[0032] FIG8( a ) is an ARS staining analysis diagram of the PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film provided in the examples of the present application.
[0033] FIG8( b ) is an ARS staining analysis diagram of the g-SC / PLLA membrane provided in an example of the present application. DETAILED DESCRIPTION
[0034] Hereinafter, the embodiments of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there may be cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0035] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0036] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0037] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0038] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0039] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0040] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0041]
Preparation method
[0042] This preparation method comprises the following steps:
[0043] (A) causing magnesium oxide to undergo a hydration reaction under heating conditions;
[0044] (B) polymerizing the hydrated magnesium oxide with a lactide monomer to form magnesium oxide-grafted polylactic acid;
[0045] (C) Dispersing magnesium oxide grafted with polylactic acid in polylactic acid to form a bone repair composite material.
[0046]
Hydration reaction
[0047] It is to be understood that the "hydration reaction" herein refers to the process in which the surface of magnesium oxide is hydrated to form a hydroxylation.
[0048] The hydration reaction can be carried out in pure water. Of course, acid-base regulators can be added according to the actual needs of the conversion rate and reaction rate of the hydration reaction. Of course, some polar solvents can also be added, such as organic alcohols, amine compounds, etc. The hydration reaction can be carried out under normal pressure or under pressure.
[0049] As a more suitable but non-limiting specific example, the heating temperature is 40-100°C, for example 40°C, 45°C, 48°C, 50°C, 55°C, 60°C, 65°C, 80°C, 85°C, 90°C, 97°C, 100°C, and the hydration reaction time is 0.5-8h, for example 0.5h, 0.75h, 1h, 2h, 3h, 4h, 4.5h, 6h, 7h, 7.5h, 8h, etc.
[0050] As a more suitable but non-limiting specific example, the mass ratio of magnesium oxide to water is 1:5-1:10.
[0051] As a more suitable but non-limiting specific example, the particle size of magnesium oxide as a reaction raw material can be 5-100μm, for example, 5μm, 6μm, 8μm, 10μm, 20μm, 30μm, 50μm, 60μm, 70μm, 80μm, 90μm, 100μm, etc.
[0052] It is understood that after the hydration reaction is completed, the solid phase can be separated from the hydration reaction solution to facilitate the subsequent step (B). The solid separation operation includes but is not limited to suction filtration, washing and drying. Here, based on the consideration of the drying effect, the drying conditions can be exemplified as vacuum drying at 40-80°C for 20-40h.
[0053]
Magnesium oxide grafted polylactic acid
[0054] The polymerization conditions for forming the magnesium oxide grafted polylactic acid can adopt the conventional polymerization conditions for polylactic acid.
[0055] For example, the monomer type is: L-lactide, D-lactide, racemic lactide or a combination thereof.
[0056] Catalyst types may include, but are not limited to, stannous octoate.
[0057] Organic solvents include, but are not limited to, anhydrous toluene and xylene.
[0058] The copolymerization method includes, but is not limited to, melt copolymerization and solution copolymerization.
[0059] As a more suitable but non-limiting specific example, the ratio of each material in the polymerization reaction is: 0.1-20 mass parts of magnesium oxide after hydration reaction, for example, 0.1 mass parts, 0.5 mass parts, 0.8 mass parts, 1 mass parts, 2 mass parts, 5 mass parts, 8 mass parts, 10 mass parts, 15 mass parts, 18 mass parts, 20 mass parts, etc.; 80-99.9 mass parts of lactide monomer, for example, 80 mass parts, 82 mass parts, 85 mass parts, 90 mass parts, 92 mass parts, 95 mass parts, 98 mass parts, 99.9 mass parts, etc.; the molar ratio of the catalyst to the lactide monomer is 0.1% to 0.5%, for example, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.4%, 0.45%, 0.5%, etc.
[0060] Under the above material ratio, the volume of the organic solvent can be 50-300 ml.
[0061] As a more suitable but non-limiting specific example, the polymerization reaction is carried out in an anhydrous and oxygen-free environment, and the polymerization reaction temperature is 110-160°C, for example, 110°C, 112°C, 115°C, 120°C, 130°C, 135°C, 140°C, 150°C, 155°C, 160°C, etc.; the polymerization reaction time is 12-30h, for example, 12h, 13h, 15h, 20h, 25h, 28h, 30h, etc.
[0062] It is easy to imagine that, if one wants to obtain solid-phase magnesium oxide grafted polylactic acid, a solvent can be added to the polymerization reaction solution to further dissolve it, and the precipitate can be collected after centrifugation, and the precipitate can be dried to obtain magnesium oxide grafted polylactic acid.
[0063] Here, the solvent includes but is not limited to dichloromethane and chloroform.
[0064] Here, the centrifugal operation conditions may be: pouring the mixed solution into a centrifuge tube, placing it into a centrifuge after balancing, centrifuging at 8-15° C. and 6000-10000 rpm for 10-15 minutes, and then collecting the precipitate.
[0065] Here, the drying step is: putting the collected precipitate into a vacuum drying oven and vacuum drying it at 40-80° C. for 20-40 hours.
[0066]
Magnesium oxide grafted polylactic acid dispersed in polylactic acid
[0067] As a more suitable but non-limiting specific example, the viscosity-average molecular weight of polylactic acid is 50 kDa-150 kDa, for example, 50 kDa, 55 kDa, 60 kDa, 70 kDa, 80 kDa, 100 kDa, 110 kDa, 120 kDa, 130 kDa, 140 kDa, 150 kDa, etc.
[0068] As a more suitable but non-limiting specific example, in the dispersion process, the ratio of materials is: magnesium oxide is 0.1-30 mass parts, for example, 0.1 mass parts, 0.5 mass parts, 1 mass parts, 2 mass parts, 5 mass parts, 8 mass parts, 10 mass parts, 15 mass parts, 20 mass parts, 25 mass parts, 28 mass parts, 30 mass parts; polylactic acid is 70-99.9 mass parts, for example, 70 mass parts, 72 mass parts, 75 mass parts, 80 mass parts, 85 mass parts, 90 mass parts, 95 mass parts, 98 mass parts, 99.9 mass parts, etc.
[0069] This part is dispersed and can be stirred for 12-48 hours under mechanical stirring conditions.
[0070] It is easy to understand that, if a solid phase product is to be obtained, ethanol precipitation can be used, and the precipitate can be collected and dried to obtain a polylactic acid-based composite material modified with magnesium oxide.
[0071] Here, the volume ratio of the polymer solution to ethanol is 1:2 to 1:5.
[0072] Here, the drying conditions may be: putting the collected precipitate into a vacuum drying oven and vacuum drying it at 40-60° C. for 20-40 hours.
[0073]
application
[0074] The bone repair composite material obtained by the above preparation method is used in cell-compatible materials.
[0075] The bone repair composite material obtained by the above preparation method is used in osteogenic active materials.
[0076] The above applications will be explained in the "Evaluation" section below and will not be discussed in detail here.
[0077] [Example]
[0078] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0079] [Comparative Example 1]
[0080] (Pure polylactic acid)
[0081] Weigh a certain amount of medical-grade L-lactide into a round-bottom flask, add stannous octoate at a mass ratio of 0.5% to the monomer, pass into an argon atmosphere, and start the reaction at 140°C for 24 hours. After being completely dissolved with dichloromethane, weigh ethanol in a ratio of 1:3 between the volume of polylactic acid solution and ethanol, add the polylactic acid solution to the ethanol, then collect the precipitate and place it in a vacuum drying oven, vacuum dry it at 60°C for 24 hours, and put it in a vacuum drying oven at 60°C to dry it completely. The resulting product is recorded as PLLA.
[0082] [Comparative Example 2]
[0083] (Polylactic acid blended with magnesium oxide without polylactic acid grafting)
[0084] Comparative Example 2-1
[0085] According to the ratio of 5:95 of magnesium oxide and polylactic acid (product PLLA), 8.947g of MgO particles and 170g of left-handed polylactic acid (viscosity average molecular weight of 90kDa) were weighed and then added to a beaker in sequence. Dichloromethane was added to the beaker to prepare a polylactic acid mixture with a concentration of 10% (w / v), and mechanically stirred for 24 hours. After the stirring was completed, ethanol was weighed according to the ratio of 1:3 of the volume ratio of the polymer solution to ethanol, and the polylactic acid mixture was added to the ethanol. Then the precipitate was collected and placed in a vacuum drying oven, and vacuum dried at 60°C for 24 hours. The obtained product was recorded as MgO / PLLA5%.
[0086] Comparative Example 2-2
[0087] The only difference from Comparative Example 2-1 is that the mass ratio of magnesium oxide to polylactic acid (product PLLA) is 1:99, and the obtained product is recorded as MgO / PLLA1%.
[0088] [Example 1]
[0089] (Melt copolymerization modified magnesium oxide particles (g-MH-MC))
[0090] Example 1-1
[0091] First, 20 g of magnesium oxide was added to 160 mL of ultrapure water at a ratio of 1:8 (w / v) and heated at 80°C for 4 hours. After hydration, the product was dried and collected, and the product was labeled as MH.
[0092] First, MH magnesium oxide and L-lactide were weighed in a glove box at a mass ratio of 1:20, and then stannous octoate was weighed at a molar ratio of 0.3% of the catalyst to the monomer. The weighed MH magnesium oxide, monomer and catalyst were placed in a three-necked flask and sealed with a stopper. The flask containing the sample was then magnetically stirred at 50°C and vacuumed for 2h. After the reaction, argon was introduced, the temperature was raised to 120°C, and the reaction was carried out for 24 hours. After the reaction was completed, the product was dissolved in dichloromethane and divided into centrifuge tubes, and then placed in a centrifuge after balancing. Centrifuge at 10°C and 8000rpm for 10 minutes, and then the precipitate was collected. The collected precipitate was placed in a vacuum drying oven and vacuumed at 50°C for 24 hours. The sample obtained after drying was recorded as g-MH-MC-120.
[0093] Example 1-2
[0094] The only difference from Example 1-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 130° C., and the sample is recorded as g-MH-MC-130.
[0095] Examples 1-3
[0096] The only difference from Example 1-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 140° C., and the sample is recorded as g-MH-MC-140.
[0097] Examples 1-4
[0098] The only difference from Example 1-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 150° C., and the sample is recorded as g-MH-MC-150.
[0099] [Example 2]
[0100] (Solution copolymerization modified magnesium oxide particles (g-MH-SC))
[0101] Example 2-1
[0102] First, 20 g of magnesium oxide was added to 160 mL of ultrapure water at a ratio of 1:8 (w / v) and heated at 80°C for 4 hours. After hydration, the product was dried and collected, and the product was labeled as MH.
[0103] First, MH magnesium oxide and L-lactide were weighed in a glove box at a mass ratio of 1:20, and then stannous octoate was weighed at a molar ratio of 0.3% of the catalyst to the monomer. The weighed MH magnesium oxide, monomer and catalyst were placed in a three-necked flask, 150 mL of xylene was added to the flask and sealed with a stopper, and then the flask containing the sample was magnetically stirred at 40 ° C and vacuumed for 0.5 h until no bubbles were generated. After the reaction, argon was introduced, the temperature was raised to 120 ° C, and the reaction was carried out for 24 hours. After the reaction was completed, the product was dissolved in dichloromethane and divided into centrifuge tubes, and then placed in a centrifuge after balancing, centrifuged at 10 ° C and 8000 rpm for 10 minutes, and then the precipitate was collected. The collected precipitate was placed in a vacuum drying oven and vacuumed at 50 ° C for 24 hours. The sample obtained after drying was recorded as g-MH-SC-120.
[0104] Example 2-2
[0105] The only difference from Example 2-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 130° C., and the sample is recorded as g-MH-SC-130.
[0106] Example 2-3
[0107] The only difference from Example 2-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 140° C., and the sample is recorded as g-MH-SC-140.
[0108] Embodiment 2-4
[0109] The only difference from Example 2-1 is that the polymerization reaction temperature of MH magnesium oxide, monomer and catalyst is replaced with 150° C., and the sample is recorded as g-MH-SC-150.
[0110] [Example 3]
[0111] (Polylactic acid composite material (g-MH-SC / PLLA))
[0112] Example 3-1
[0113] According to the ratio of modified magnesium oxide and polylactic acid mass of 5:95, 8.947g of product g-MH-SC-150 particles and 170g of left-handed polylactic acid (viscosity average molecular weight of 90kDa) were weighed and then added to the beaker in sequence. Dichloromethane was added to the beaker to prepare a polylactic acid mixture with a concentration of 10% (w / v), and mechanically stirred for 24 hours. After the stirring was completed, ethanol was weighed according to the ratio of the volume ratio of the polymer solution to ethanol of 1:3, and the polylactic acid mixture was added to the ethanol. Then the precipitate was collected and placed in a vacuum drying oven, and vacuum dried at 60°C for 24 hours to obtain g-MH-SC / PLLA5%.
[0114] Example 3-2
[0115] The only difference from Example 3-1 is that the mass ratio of magnesium oxide to polylactic acid is 1:99, and the obtained product is recorded as g-MH-SC / PLLA1%.
[0116] [Comparative Example 3]
[0117] (Polylactic acid composite material (g-SC / PLLA))
[0118] Comparative Example 3-1
[0119] The only difference from Example 3-1 is that the g-MH-SC-150 magnesium oxide particles are replaced with g-SC-150 magnesium oxide particles, and the obtained product is recorded as g-SC / PLLA5%.
[0120] Among them, the preparation method of g-SC-150 magnesium oxide particles is to omit the hydration reaction process in the preparation process of g-MH-SC-150 magnesium oxide particles, that is, to omit the operation of "adding 20g of magnesium oxide to 160mL of ultrapure water at a ratio of 1:8 (w / v) and heating at 80°C for 4 hours."
[0121] Comparative Example 3-2
[0122] The only difference from Example 3-2 is that the g-MH-SC-150 magnesium oxide particles are replaced with g-SC-150 magnesium oxide particles, and the obtained product is recorded as g-SC / PLLA1%.
[0123] Among them, the preparation method of g-SC-150 magnesium oxide particles is to omit the hydration reaction process in the preparation process of g-MH-SC-150 magnesium oxide particles, that is, to omit the operation of "adding 20g of magnesium oxide to 160mL of ultrapure water at a ratio of 1:8 (w / v) and heating at 80°C for 4 hours."
[0124]
evaluate
[0125] In order to facilitate the performance testing of the materials, PLLA, MgO / PLLA, g-SC / PLLA, and g-MH-SC / PLLA were prepared into films by calendering method. The specific steps are as follows: first, the four products PLLA, MgO / PLLA, g-SC / PLLA, and g-MH-SC / PLLA were weighed and placed in a mold, which was then placed in a flat-plate vulcanizer and hot-pressed into films at 160°C.
[0126] Ⅰ. Structural characterization and surface morphology analysis
[0127] Figure 1 These are the Fourier infrared spectra of magnesium oxide modified by melt copolymerization (A) and solution copolymerization (B) at different temperatures.
[0128] The structures of the homemade g-MH-MC and g-MH-SC were characterized by Fourier transform infrared spectrometer (FT-IR, Nicolet 6700, Thermo Fisher Scientific). The homemade g-MH-MC and g-MH-SC were added to potassium bromide and ground into powder, and then made into tablets. The Fourier transform infrared spectroscopy test wavelength range is 4000-500cm -1 .
[0129] Figure 1 (A) Middle 867cm -1 The absorption peak at 1121 cm is the stretching vibration of the CC group of polylactic acid. -1 is the stretching vibration of the COC group, 1383 cm -1 and 1648cm -1 The absorption peak at 2993 cm corresponds to the -CH bending vibration of polylactic acid. -1 The corresponding wavelength is 3696 cm -1 is the stretching vibration of the OH group on the surface of magnesium oxide after hydration. Figure 1 (B) 864cm -1 The absorption peak at 1121 cm is the stretching vibration of the CC group of polylactic acid. -1 The stretching vibration of COC group is at 1377 cm -1 and 1644cm -1 is the bending vibration of -CH in polylactic acid, 2988cm -1 is the stretching vibration of CH and -CH3, 3694cm -1 The same is true for the stretching vibration of OH on the surface of magnesium oxide.
[0130] The results of Fourier transform infrared spectroscopy show that polylactic acid has been successfully grafted onto the surface of magnesium oxide by melt copolymerization and solution copolymerization at different temperatures. The results also show that surface hydration can increase the amount of hydroxyl groups on the surface of magnesium oxide particles.
[0131] Figure 2 These are the X-ray diffraction patterns (XRD) of magnesium oxide modified by melt copolymerization (A) and solution copolymerization (B) at different temperatures.
[0132] Figure 2 In (A) and (B), 36°, 43°, 62°, 74°, and 78° are characteristic peaks of magnesium oxide, while 18°, 38°, 50°, 58°, 68°, and 72° are characteristic peaks of magnesium hydroxide. The XRD results show that polylactic acid is grafted on the surface of magnesium oxide after hydration, and the crystal structure of magnesium oxide is not changed.
[0133] Figure 3 These are scanning electron microscope images of magnesium oxide modified by melt copolymerization (C, D) and solution copolymerization (E, F).
[0134] Figure 3 (A, B) are the surface morphologies of magnesium oxide particles after hydration. The surface of magnesium oxide after hydration is relatively dense and smooth. After being modified by melt copolymerization, the surface morphology shows a state of aggregation of rod-like small particles, and needle-like polylactic acid appears in the pores of the rod-like small particles. The specific morphology is as follows Figure 3 However, after the magnesium oxide was modified by solution copolymerization, more polylactic acid was grafted onto the surface of MgO, and the polylactic acid covered the surface of magnesium oxide in the form of filaments, and the surface of magnesium oxide was in the form of a cocoon.
[0135] The above results show that magnesium oxide can be modified by melt copolymerization and solution copolymerization at 120℃, 130℃, 140℃, and 150℃, and polylactic acid can be grafted on the surface of magnesium oxide, and polylactic acid is grafted with magnesium oxide in different forms. The surface of magnesium oxide presents different morphologies under the action of different copolymerization methods, but the two copolymerization methods will not change the crystal structure of magnesium oxide.
[0136] Ⅱ. Mechanical properties test
[0137] Figure 4(a) is a graph showing the mechanical properties of PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film.
[0138] Figure 4(a) shows that the tensile strength of the polylactic acid film is 51.27MPa. After adding unmodified magnesium oxide, the tensile strength decreases. When the magnesium oxide content increases to 5%, the tensile strength of the composite material increases, the elastic modulus increases, and the elongation at break decreases compared with the composite material with a magnesium oxide content of 1%. This shows that the increase of magnesium oxide will increase the stiffness of the material, but because the magnesium oxide particles are large in size and easy to agglomerate, its tensile strength will decrease. After magnesium oxide is modified and compounded with polylactic acid, its tensile strength is reduced compared with that of the polylactic acid film, but compared with MgO / PLLA1% and MgO / PLLA5%, its tensile strength increases, the stiffness decreases, and the elongation at break increases, which shows that the modified magnesium oxide is better dispersed in polylactic acid and the mechanical effect is significantly improved.
[0139] Figure 4(b) is a graph showing the mechanical properties of the g-SC / PLLA membrane. It can be seen from the figure that the various types of mechanical properties of the g-SC / PLLA membrane are better than those of the MgO / PLLA membrane but lower than those of the g-MH-SC / PLLA membrane. This indicates that the unhydrated MgO particles have a small amount of surface hydroxyl groups, resulting in a small amount of polylactic acid grafted on the particle surface, which in turn causes the mechanical properties of the g-SC / PLLA composite membrane to be lower than those of the g-MH-SC / PLLA membrane. However, compared with the MgO / PLLA membrane, under the action of polylactic acid grafted on the particle surface, the compatibility of the particles with the left-handed polylactic acid matrix increases, which makes the mechanical properties of the g-SC / PLLA membrane better than those of the MgO / PLLA membrane.
[0140] The above results show that the magnesium oxide modification method proposed in this application can solve the "agglomeration" phenomenon and effectively improve the mechanical properties of the composite material.
[0141] Ⅲ. Contact angle test
[0142] Figure 5 This is the contact angle test diagram of PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film at room temperature.
[0143] The contact angle of water of PLLA film at room temperature is 87.42°, and the degrees of MgO / PLLA1%, MgO / PLLA 5%, g-MH-SC / PLLA1%, and g-MH-SC / PLLA 5% are 86.42°, 83.67°, 77.83°, and 69.17°, respectively. With the increase of the content of hydrophilic magnesium oxide, the hydrophilicity of the composite material gradually improves, and its contact angle gradually decreases. In addition, at the same content, compared with the unmodified MgO, the contact angle of the composite material with modified MgO is smaller. This shows that MgO helps to improve the hydrophilicity of the composite material, and the improvement effect increases with the increase of MgO content. At the same time, the hydrophilicity of the composite material can be further improved after the modification of MgO.
[0144] IV. Surface and cross-sectional morphology analysis of membranes
[0145] Figure 6 Surface and cross-sectional scanning electron micrographs of PLLA film, MgO / PLLA film (C, D), and g-MH-SC / PLLA film.
[0146] Figure 6 (A) and (B) are the surface and cross-section of polylactic acid, which are uniform and smooth, with no obvious cracks inside. (C) and (D) are the surface and cross-section of MgO / PLLA1% film, respectively. In the figure, MgO has obvious "agglomeration" phenomenon, the interface between MgO and polylactic acid matrix inside the material is obvious, and the number of cracks has increased significantly. As the MgO content increases to 5%, MgO is more dispersed on the surface of the material, the "agglomeration" phenomenon is more obvious, and the number of gaps inside the material also increases with the increase of MgO content, as shown in Figures (E) and (F). Figures (G) and (H) are the surface and cross-section of g-MH-SC / PLLA1% film. Compared with MgO / PLLA1% film, g-MH-SC / PLLA1% film has fewer surface particles. This is because the surface of MgO will be grafted with polylactic acid after modification, and the compatibility of g-MH-SC is increased. After compounding by solution blending, g-MH-SC will be better compounded into the material, which can reduce the number and size of gaps inside the composite material. In Figure (I), when the content of g-MH-SC increases to 5%, the number of particles on the membrane surface is still small and evenly dispersed, and no "agglomeration" occurs. Since g-MH-SC is wrapped by surface-grafted polylactic acid inside the material, it has better compatibility in the polylactic acid matrix, so there is no obvious crack at the interface between g-MH-SC and polylactic acid, as shown in Figure (J).
[0147] V. Evaluation of membrane cell compatibility
[0148] Figure 7(a) shows the staining of live and dead cells on PLLA membrane, MgO / PLLA membrane, and g-MH-SC / PLLA membrane after 1 and 3 days of culture.
[0149] The results in Figure 7(a) show that all groups have good cell compatibility. Among them, the number of cells on the PLLA membrane is the least, and the number of cells and the density of cells on the g-MH-SC / PLLA membrane are the largest. This shows that the cell compatibility of the material increases after adding magnesium oxide, and the modification of magnesium oxide helps to further improve the biocompatibility of the composite material.
[0150] Figure 7(b) is the cell compatibility evaluation of g-SC / PLLA membrane. As can be seen from the figure, after 1 day and 3 days of co-culture of g-SC / PLLA membrane with cells, the results in the figure show a large number of living cells (green), which indicates that g-SC / PLLA membrane has good cell compatibility.
[0151] VI. Evaluation of the osteogenic activity of the membrane
[0152] Figure 8(a) is the ALP and ARS staining analysis of PLLA film, MgO / PLLA film, and g-MH-SC / PLLA film.
[0153] Figure 8(a) shows the ALP activity of the materials after 7 and 14 days of culture on PLLA membrane, MgO / PLLA membrane, and g-MH-SC / PLLA membrane. There are fewer purple spots on PLLA, indicating that PLLA lacks osteoinduction ability, while there are more purple spots on the g-MH-SC / PLLA membrane, and the color is the darkest. This shows that after the addition of magnesium oxide, the osteogenic activity of the composite material increases, and the osteogenic activity of the material increases with the increase of magnesium oxide content, and after the magnesium oxide is modified, the osteogenic activity of the material is further improved.
[0154] Similarly, using Alizarin Red Staining (ARS) to mark calcium, Figure 8 shows that after adding magnesium oxide, the mineralization degree of the material is significantly higher than that of PLLA, and the calcium mineralization degree of the g-MH-SC / PLLA composite material is the best. This shows that magnesium oxide can improve the calcium mineralization degree of the material, and after magnesium oxide is modified, the mineralization degree can be further improved.
[0155] Figure 8(b) shows the ALP and ARS staining results of g-SC / PLLA membrane. After 7 and 14 days of co-culture with cells, more purple spots appeared on both groups of composite membranes, and the number and color of purple spots increased with the increase of g-SC particle content. At the same time, using ARS to label calcium, red mineralization marks were also observed on both groups of membranes. These results indicate that g-SC / PLLA membrane has osteogenic differentiation ability.
[0156] The above results show that the osteogenic activity of the composite material can be improved after magnesium oxide is modified and composited with polylactic acid.
[0157] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them; although the present application is described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A method for preparing a bone repair composite material, characterized in that: The following steps are involved: (A) causing magnesium oxide to undergo a hydration reaction under heating conditions; (B) polymerizing the hydrated magnesium oxide with a lactide monomer to form magnesium oxide-grafted polylactic acid; (C) Dispersing magnesium oxide grafted with polylactic acid in polylactic acid to form a bone repair composite material.
2. The method for preparing the bone repair composite material according to claim 1, characterized in that: The heating temperature is 40-100° C., and the hydration reaction time is 0.5-8 h. Preferably, in step (A), the mass ratio of magnesium oxide to water is 1:5-1:
10. Preferably, in step (A), the particle size of magnesium oxide is 5-100 μm.
3. The method for preparing the bone repair composite material according to claim 1, characterized in that: In step (A), after the hydration reaction is completed, the solid phase is separated from the hydration reaction solution by vacuum drying at 40-80° C. for 20-40 hours.
4. The method for preparing the bone repair composite material according to claim 1, characterized in that: In step (B), the magnesium oxide that has undergone hydration reaction is 0.1-20 parts by mass, the lactide monomer is 80-99.9 parts by mass, and the molar ratio of the catalyst to the lactide monomer is 0.1% to 0.5%.
5. The method for preparing the bone repair composite material according to claim 1, characterized in that: In step (B), the polymerization reaction is carried out in an anhydrous and oxygen-free environment, the polymerization reaction temperature is 110-160° C., and the polymerization reaction time is 12-30 hours.
6. The method for preparing the bone repair composite material according to claim 1, characterized in that: In step (C), the viscosity average molecular weight of the polylactic acid is 50 kDa-150 kDa.
7. The method for preparing the bone repair composite material according to claim 1, characterized in that: In step (C), the amount of magnesium oxide is 0.1-30 parts by mass, and the amount of polylactic acid is 70-99.9 parts by mass.
8. The method for preparing the bone repair composite material according to claim 7, characterized in that: In step (C), the polylactic acid is in the form of a solution, and the concentration of the polymer solution is 5 to 20 g / mL.
9. Use of the bone repair composite material obtained by the preparation method of claim 1 in cell-compatible materials.
10. Use of the bone repair composite material obtained by the preparation method according to claim 1 in osteogenic active materials.