Neutron absorbing material-polypropylene blended hydrophobic microporous membrane as well as preparation method and application thereof

Highly radiation-resistant hydrophobic microporous membranes are prepared by blending polypropylene and neutron absorbing materials through a thermally induced phase separation method, which solves the problem of insufficient service life of existing membrane materials in radioactive and highly oxidizing environments, and achieves efficient radioactive wastewater treatment. treatment, maintaining the hydrophobic and mechanical properties of the membrane.

CN118718759APending Publication Date: 2024-10-01TIANJIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410752309.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing membrane materials are difficult to operate stably for a long time in radioactive and highly oxidizing environments, resulting in insufficient service life for the vacuum membrane distillation method to treat radioactive wastewater.

Method used

The thermally induced phase separation method is used to blend polypropylene and neutron absorbing materials to prepare highly radiation-resistant hydrophobic microporous membranes. The industrial wastewater containing radioactive salts with a concentration of 2g/L is treated by vacuum membrane distillation to maintain hydrophobic and mechanical properties. and high levels of interception rates.

Benefits of technology

In a radioactive environment, the hydrophobic performance of the polypropylene blend hydrophobic microporous membrane remains >95%, the mechanical properties (tensile strength and elongation at break) remain >95%, and the rejection rate remains >85%, significantly improving the performance of the membrane. long-term operating capability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118718759A_ABST
    Figure CN118718759A_ABST
Patent Text Reader

Abstract

The invention discloses a neutron absorbing material-polypropylene blended hydrophobic microporous membrane as well as a preparation method and application thereof. The hydrophobic microporous membrane comprises polypropylene and a neutron absorbing material. The prepared polypropylene blended hydrophobic microporous membrane has high mechanical stability in the uranium-containing radioactive wastewater environment, after industrial wastewater containing radioactive salt with the concentration of 2 g / L is treated with a vacuum membrane distillation method for one month, the hydrophobic performance of the membrane without a neutron absorption material is reduced by 13.57%, the mechanical performance is reduced by 55.73%, and the rejection rate is reduced by 50%; the hydrophobic performance of the polypropylene hydrophobic microporous membrane added with the neutron absorbing material is kept to be greater than 95%, the mechanical properties (tensile strength and elongation at break) are still kept to be greater than 95%, and the rejection rate is kept to be greater than 85%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane treatment of radioactive wastewater, and in particular to a neutron absorbing material-polypropylene blended hydrophobic microporous membrane and a preparation method and application thereof. Background Art

[0002] Radioactive wastewater refers to wastewater from nuclear fuel pre-treatment (including wastewater containing uranium, radium, etc. generated during uranium mining, hydrometallurgy, refining, and nuclear fuel manufacturing), and other processes of fuel post-treatment, as well as wastewater discharged from nuclear power plants, research institutions that use radioactive isotopes, hospitals, factories, etc. Typical radionuclides in water sources are mainly isotopes of radium (Ra), uranium (U), and radon (Rn). In recent years, it is believed that the fission products of nuclear reactions have also attracted widespread attention, especially radioactive cesium (Cs) and iodine (I), such as 137Cs and 131I, which are the main radioactive pollutants in water after nuclear accidents. The three basic radiations are alpha rays, beta rays, and gamma rays. Alpha rays are a stream of positively charged helium nuclei, beta rays are a stream of negatively charged electrons, and gamma rays are high-energy electromagnetic waves. The World Health Organization (WHO) lists the guidance limits of more than 190 radionuclides, including metals and non-metals, in its water quality directive, including total alpha radioactivity and total beta radioactivity, with limits of 0.5Bq / L and 1Bq / L respectively. The current drinking water standards for radionuclides in the United States stipulate that the uranium limit is 30μg / L, the total alpha radioactivity does not exceed 15pCi / L, and the beta radioactivity does not exceed 4mrem / yr. If the total alpha or total beta activity exceeds the standard, a more comprehensive analysis is conducted to identify the specific radioactive isotopes. The "Sanitary Standard for Drinking Water" (GB5749-2006) newly promulgated and implemented in my country in 2006 further stipulates that the limits of total alpha and total beta radioactivity are 0.5Bq / L and 1Bq / L respectively, which is consistent with the WHO standards, and indicates that when the radioactive index exceeds the guidance value, the nuclide analysis and evaluation should be carried out to determine whether it can be cited.

[0003] At present, the research field mainly uses adsorption, ion exchange, membrane separation, and comprehensive processes to treat uranium-containing radioactive wastewater. In the treatment process of uranium-containing radioactive wastewater, membrane treatment technology has greater cost advantages than thermal concentration technology, chemical coagulation technology, and physical adsorption technology. Membrane treatment technology has the advantages of low energy consumption, simple single-stage membrane treatment equipment, convenient operation, high separation efficiency, strong coupling, and good volume reduction effect. It is widely used in the field of water treatment and has been gradually widely used in the treatment of radioactive wastewater abroad. The vacuum membrane distillation method is mainly used for its treatment. Under the best conditions, the retention rate is 99.1%, which meets the national emission standards.

[0004] When using membrane distillation technology to treat radioactive wastewater, there is currently an important technical problem: how to ensure that the membrane material used can operate stably in a radioactive and highly oxidizing environment for a long time. At present, the most commonly used membrane materials in the membrane distillation process are polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE) and polypropylene (PP). New membrane materials such as polyethylene (PE), polyvinyl chloride (PVC) and polystyrene (PS) have also been reported. As far as the current research status is concerned, PVDF and PTFE materials have good film-forming properties, but they are difficult to meet the treatment requirements of radioactive and highly oxidizing solutions.

[0005] Polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE) are polymers containing nearly half of the CF2 chain segments. When they are exposed to radiation for a long time, their molecular chains will be damaged by cleavage, the material will age and degrade, cracks will appear, and in severe cases, powdering will occur. Especially for fluorine-containing materials, HF, TF and other corrosive and radioactive gases will be produced when they degrade. Therefore, choosing polypropylene to treat wastewater containing radioactive nuclides has the advantages of environmental protection and safety.

[0006] Polypropylene (PP) has good comprehensive mechanical properties, excellent temperature resistance and chemical resistance, low density, easy processing and low cost. It has become one of the most widely used polymers in the plastics industry.

[0007] The degradation process of PP after irradiation was studied visually by electron spin resonance and infrared spectroscopy, and it was pointed out that the radiation degradation of PP is an auto-oxidation process. The production of free radicals (alkyl free radicals PP· and alkyl peroxy free radicals PPO2·) and hydroperoxides is the main cause of PP radiation degradation. The reaction formula is as follows:

[0008]

[0009] PP·+O2→PPO2· (2)

[0010] PPO2·+PPH→PPOOH+PP· (3)

[0011]

[0012] PP· is produced when molecular bonds of PP break under γ-ray irradiation and PPO2· captures hydrogen atoms in PP. The formation of PP· is the direct cause of PP radiation degradation. Once PPO2· is produced in PP, it will capture hydrogen atoms in the PP molecular chain to form hydroperoxide. Hydroperoxide slowly decomposes and produces new free radicals at room temperature, which leads to further degradation of PP, and oxygen-containing products such as alcohols, ketones, and carboxylic acids are generated in the chain termination stage. The reaction is as follows:

[0013] PPOOH→PPO·+·OH (5)

[0014] PPOOH+PPH→PPO·+PP·+H2O (6)

[0015] 2PPOOH→PPO·+PPOO·+H2O (7)

[0016] PPO·+PPH→PPOH+PP· (8)

[0017] OH+PPH→H2O+PP (9)

[0018] Since wastewater containing radioactive salts is radioactive, and PP degrades after irradiation, resulting in a poor service life, it is difficult to meet the needs of long-term operation of vacuum membrane distillation to treat radioactive wastewater.

[0019] In order to solve the above problems, the present invention is proposed. Summary of the invention

[0020] The present invention aims to overcome the shortcomings of the prior art. In view of the problem that PP is degraded after being irradiated, resulting in its poor service life, it is difficult to meet the demand for long-term operation of vacuum membrane distillation to treat radioactive wastewater. The present invention uses a thermally induced phase separation method to blend polypropylene with a neutron absorbing material to prepare a highly radiation-resistant hydrophobic microporous membrane. After one month of treating industrial wastewater containing radioactive salts at a concentration of 2g / L by vacuum membrane distillation, the hydrophobicity of the membrane without adding neutron absorbing material decreased by 15-40%, the mechanical properties decreased by 40-80%, and the interception rate decreased by 40-80%; while the hydrophobicity of the polypropylene hydrophobic microporous membrane with added neutron absorbing material remained >95%. The mechanical properties still remained >95%, and the interception rate remained >85%.

[0021] The present invention adopts the following technical solutions:

[0022] A first aspect of the present invention provides a neutron absorbing material-polypropylene blended hydrophobic microporous membrane, which comprises polypropylene and a substance having neutron absorbing ability.

[0023] Preferably, the neutron absorbing material includes boron nitride, boron carbide, titanium boride, aluminum-based boron carbide, and lanthanide titanate.

[0024] The second aspect of the present invention provides a method for preparing the neutron absorbing material-polypropylene blended hydrophobic microporous membrane according to the first aspect of the present invention, wherein the neutron absorbing material-polypropylene blended hydrophobic microporous membrane is prepared by a thermally induced phase separation method, and the method comprises the following steps:

[0025] (1) Selecting polypropylene material, neutron absorbing material, diluent, and pore-forming agent for mixing;

[0026] (2) stirring and blending the uniformly mixed raw materials under a nitrogen atmosphere to ensure that the casting solution is mixed into a homogeneous phase;

[0027] (3) vacuum degassing the mixed casting solution to obtain a fully blended casting solution, which is to ensure that the surface of the prepared polypropylene microporous membrane is uniform;

[0028] (4) Pour the fully blended casting solution onto the non-woven fabric and scrape out a flat membrane with a scraper; or use a double-tube die to extrude and cast into a hollow fiber membrane;

[0029] (5) placing the prepared flat membrane or hollow fiber membrane completely in the extractant, and drying after the extraction is complete to obtain a neutron absorbing material-polypropylene blended hydrophobic microporous flat membrane and a neutron absorbing material-polypropylene blended hydrophobic microporous hollow fiber membrane.

[0030] Preferably, in step (1), the melt index of the polypropylene material is 3 to 40 g / 10 min;

[0031] The selection of neutron absorbing materials is critical to whether a homogeneous phase can be formed. Only by ensuring that the casting solution is mixed into a homogeneous phase can the performance of the obtained blended microporous membrane be guaranteed. The neutron absorbing materials described in the present invention include boron nitride, boron carbide, titanium boride, aluminum-based boron carbide, boron-containing polymers and aluminum-based tungsten-boron composite materials (Al / W / WC / B4C), lanthanide titanates, etc.

[0032] The diluent is a common polymer solvent having a similar non-polar structure to the polymer and having a viscosity adjustment function;

[0033] The pore-forming agent is an easily soluble and difficult to decompose inorganic salt;

[0034] The mixing ratios are calculated by weight percentage: PP, neutron absorbing material, diluent, pore former: 20-50%; 0.125-5%; 40-75%; 0-8%.

[0035] Preferably, in step (2), the stirring temperature is 20°C to 80°C higher than the melting point of the polymer PP, and the stirring time is 2 to 12 hours.

[0036] Preferably, in step (3), the vacuum degassing treatment condition is a vacuum degree of 0.5 to 1 bar, preferably 0.8 bar.

[0037] Preferably, in step (4), the completely blended casting liquid is placed in an environment with the same blending conditions as in step (2), and poured onto a non-woven fabric, and a flat membrane is scraped out with a scraper; or under the condition of hot nitrogen at a central tube temperature 10°C to 50°C higher than the melting point of polypropylene PP, a double-tube die is used for extrusion and casting into a hollow fiber membrane; an environment with consistent blending conditions means that the temperature and nitrogen atmosphere are consistent.

[0038] Preferably, in step (5), the extractant is a substance having greater compatibility and similar polarity to the diluent, including butanone, acetone, etc.

[0039] The third aspect of the present invention provides an application of the neutron absorbing material-polypropylene blended hydrophobic microporous membrane described in the first aspect of the present invention, which is applied to the treatment of radioactive wastewater by vacuum membrane distillation.

[0040] Preferably, the neutron absorbing material-polypropylene blended hydrophobic microporous membrane has high mechanical stability and high resistance to gamma rays and electron beam radiation. After the industrial wastewater containing radioactive salts at a concentration of 2 g / L is treated by vacuum membrane distillation for one month, the hydrophobicity of the neutron absorbing material-polypropylene blended hydrophobic microporous membrane remains >95%, the mechanical properties of tensile strength and elongation at break still remain >95%, and the retention rate remains >85%.

[0041] Solid neutron absorbing materials are usually metals, non-metallic elements and compounds with high thermal neutron and epithermal neutron absorption cross sections. Most of these neutron absorbing materials contain elements with high neutron absorption cross sections such as rhenium, samarium, europium, cadmium and boron.

[0042] Compared with the prior art, the present invention has the following beneficial effects:

[0043] 1. The present invention uses the thermally induced phase separation method for the first time to blend polypropylene with neutron absorbing materials to prepare highly radiation-resistant hydrophobic microporous membranes, including hydrophobic microporous flat membranes and hydrophobic microporous hollow fiber membranes. The polypropylene blended hydrophobic microporous membrane prepared by the present invention has high mechanical stability in the environment of uranium-containing radioactive wastewater. After treating industrial wastewater containing radioactive salts with a concentration of 2g / L by vacuum membrane distillation for one month, the hydrophobicity of the membrane without adding neutron absorbing materials decreased by 13.57%, the mechanical properties decreased by 55.73%, and the interception rate decreased by 50%; while the hydrophobicity of the polypropylene hydrophobic microporous membrane with added neutron absorbing materials remained >95%, the mechanical properties (tensile strength and elongation at break) still remained >95%, and the interception rate remained >85%.

[0044] 2. The selection of neutron absorbing materials is critical to whether a homogeneous phase can be formed. Only by ensuring that the casting solution is mixed into a homogeneous phase can the performance of the obtained blended microporous membrane be guaranteed. In the present invention, the neutron absorbing materials are selected from boron, lanthanide metal elements and disulfide substances (such as boron nitride, boron carbide, titanium boride, aluminum-based boron carbide, boron-containing polymers and aluminum-based tungsten-boron composite materials (Al / W / WC / B4C), lanthanide titanates, etc.) with neutron absorbing ability. In the present invention, the neutron absorbing material can be mixed with polypropylene materials and the like to form a homogeneous phase after the casting solution is mixed, and the obtained blended microporous membrane has excellent performance.

[0045] 3. The hydrophobic microporous membrane blended with polypropylene and neutron absorbing material prepared by the above method has high resistance to gamma rays and electron beam radiation, and can be used in the vacuum membrane distillation method to treat radioactive wastewater. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 The hydrophobic properties of PP membrane and PP-BN and PP-B4C blended membranes before treating wastewater with a radioactive salt content of 2g / L and 30 days after treatment.

[0047] Figure 2 The mechanical properties of PP membrane and PP-BN and PP-B4C blended membranes were studied before treating wastewater with a radioactive salt content of 2g / L.

[0048] Figure 3 The mechanical properties of PP membrane and PP-BN and PP-B4C blended membranes after treating wastewater with a radioactive salt content of 2g / L for 30 days.

[0049] Figure 4 The average flux within 30 days and the retention rate on the 30th day of PP membrane, PP-BN and PP-B4C blended membranes for treating wastewater with a radioactive salt content of 2g / L.

[0050] Figure 5 The hydrophobic properties of PP, PP-TiB2, PP-Al / B4C, and PP-LaTiO3 microporous flat membranes were studied before and 30 days after treating wastewater with a radioactive salt content of 2g / L.

[0051] Figure 6 The mechanical properties of PP, PP-TiB2, PP-Al / B4C, and PP-LaTiO3 microporous flat membranes were studied before treating wastewater with a radioactive salt content of 2g / L.

[0052] Figure 7 The mechanical properties of PP, PP-TiB2, PP-Al / B4C, and PP-LaTiO3 microporous flat membranes were investigated after 30 days of treatment of wastewater with a radioactive salt content of 2 g / L.

[0053] Figure 8 The average flux within 30 days and the retention rate on the 30th day of PP, PP-TiB2, PP-Al / B4C, and PP-LaTiO3 microporous flat membranes for treating wastewater with a radioactive salt content of 2g / L. DETAILED DESCRIPTION

[0054] The present invention is further described below by way of examples, which are not limited to the examples. Experimental methods without specific conditions specified in the examples are generally carried out under conventional conditions and conditions described in the manual, or under conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all commercially available unless otherwise specified.

[0055] The specific steps of the method of the present invention are as follows:

[0056] Embodiment 1, 2:

[0057] Neutron absorbing materials: Boron nitride (BN), Boron carbide (B4C)

[0058] The microporous flat membrane is prepared by the thermally induced phase separation method. First, the polypropylene material, BN or B4C, diluent, and pore-forming agent are heated at 180°C in the same proportion and uniformly mixed into a homogeneous phase; after 4 hours of degassing treatment, a scraper is used to scrape out a thin and uniform PP-BN and PP-B4C blended hydrophobic microporous flat membrane on the support layer; after curing in a 30°C water bath or oil bath for 30 seconds, extraction for 6 hours, and drying, the PP-BN and PP-B4C blended hydrophobic microporous flat membrane is obtained.

[0059] In this embodiment, BN can form a homogeneous phase with the casting liquid. The performance of the PP-BN microporous flat membrane prepared in this embodiment is: an average pore size of 0.15 μm, a porosity of 52%, a mechanical tensile strength of 16.2 MPa, an elongation at break of 31.58%, and a water contact angle of 127.7°. After using the membrane to treat industrial wastewater containing radioactive salts at a concentration of 2 g / L (wastewater with a uranium content of 2 g / L) by vacuum membrane distillation for 1 month, the membrane mechanical tensile strength is 14.7 MPa, the elongation at break is 30.9%, and the water contact angle is 123.5°. It can be clearly seen that the mechanical properties and hydrophobic properties of the polypropylene blended hydrophobic microporous membrane with BN added are maintained at more than 95%, and its retention rate is measured to be maintained at more than 85%.

[0060] In this embodiment, B4C can form a homogeneous phase with the casting liquid. The performance of the PP-B4C microporous flat membrane prepared in this embodiment is: an average pore size of 0.23 μm, a porosity of 56%, a mechanical tensile strength of 12.34 MPa, an elongation at break of 30.28%, and a water contact angle of 136.2°. After using the membrane to treat industrial wastewater containing uranium radioactive salts with a concentration of 2 g / L by vacuum membrane distillation for one month, the membrane has a mechanical tensile strength of 10.3 MPa, an elongation at break of 27.3%, and a water contact angle of 130.2°. It can be clearly seen that the mechanical properties and hydrophobic properties of the polypropylene blended hydrophobic microporous membrane with BN added are maintained at more than 95%, and its retention rate is measured to be maintained at more than 85%.

[0061] Embodiment 3-5:

[0062] The preparation conditions of Examples 3-5 are basically the same as those of Examples 1 and 2, except that the neutron absorbing materials added in Examples 3-5 are titanium boride (TiB2), aluminum-based boron carbide (Al / B4C), and lanthanum titanate (LaTiO3). In this example, titanium boride, aluminum-based boron carbide, and lanthanum titanate can form a homogeneous phase with the casting solution.

[0063] The properties of the PP-TiB2, PP-Al / B4C, and PP-LaTiO3 microporous flat membranes prepared in this embodiment are as follows: the average pore sizes are 0.24 μm, 0.18 μm, and 0.21 μm, respectively; the porosities are 51.1%, 48.3%, and 54.3%, respectively; the mechanical tensile strengths are 14.22 MPa, 16.22 MPa, and 17.23 MPa, respectively; the elongations at break are 28.44%, 28.33%, and 23.53%, respectively; the water contact angles are 121.22°, 123.21°, and 126.24°, respectively. After one month of using the membrane to treat industrial wastewater containing radioactive salts at a concentration of 2g / L by vacuum membrane distillation, the mechanical tensile strength of the membrane was 13.32MPa, 14.61MPa, and 15.92MPa, the elongation at break was 27.44%, 26.845%, and 22.03%, and the water contact angle was 116.34°, 115.23°, and 119.44°. It can be clearly seen that the mechanical properties and hydrophobic properties of the polypropylene blended hydrophobic microporous membrane with added BN are maintained above 95%, and its retention rate is measured to be maintained above 85%.

[0064] Comparative Example:

[0065] Under the same preparation conditions as in Examples 1-5, without adding neutron absorbing material, the prepared membrane sample had a measured mechanical tensile strength of 15.2 MPa, an elongation at break of 32.2%, and a water contact angle of 126.2°. The membrane was used to treat the same radioactive wastewater. After one month of process operation, the mechanical properties of the membrane material decreased by 57.32%, and the hydrophobic properties decreased by 18.4%. At the same time, its retention rate was measured to be reduced by 53%.

[0066] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A neutron absorbing material-polypropylene blended hydrophobic microporous membrane, characterized in that: It includes polypropylene and neutron absorbing material.

2. The neutron absorbing material-polypropylene blended hydrophobic microporous membrane according to claim 1, characterized in that: The neutron absorbing material includes boron nitride, boron carbide, titanium boride, aluminum-based boron carbide, boron-containing polymer, aluminum-based tungsten-boron composite material, and lanthanide titanate.

3. A method for preparing the neutron absorbing material-polypropylene blended hydrophobic microporous membrane according to any one of claims 1 to 2, characterized in that: The neutron absorbing material-polypropylene blended hydrophobic microporous membrane is prepared by a thermally induced phase separation method, which comprises the following steps: (1) Selecting polypropylene material, neutron absorbing material, diluent, and pore-forming agent for mixing; (2) stirring and blending the mixed raw materials under a nitrogen atmosphere to ensure that the casting solution is mixed into a homogeneous phase; (3) performing vacuum degassing on the casting solution mixed into a homogeneous phase to obtain a casting solution that is fully blended; (4) Pour the fully blended casting solution onto the non-woven fabric and scrape out a flat membrane with a scraper; or use a double-tube die to extrude and cast into a hollow fiber membrane; (5) placing the prepared flat membrane or hollow fiber membrane completely in the extractant, and drying after the extraction is complete to obtain a neutron absorbing material-polypropylene blended hydrophobic microporous flat membrane and a neutron absorbing material-polypropylene blended hydrophobic microporous hollow fiber membrane.

4. The method according to claim 3, characterized in that In step (1), the melt index of the polypropylene material is 3 to 40 g / 10 min; The neutron absorbing material includes boron nitride, boron carbide, titanium boride, aluminum-based boron carbide, boron-containing polymers, aluminum-based tungsten-boron composite materials, and lanthanide titanates; The diluent is a polymer solvent having a similar non-polar structure to the polymer and having adjustable viscosity; The pore-forming agent is an easily soluble and difficult to decompose inorganic salt; Mixing ratio by weight percentage: PP, neutron absorber, diluent, pore former: 20-50%; 0.125~5%;40~75%;0~8%。 5. The method according to claim 3, characterized in that: In step (2), the stirring temperature is 20°C to 80°C higher than the melting point of the polymer PP, and the stirring time is 2 to 12 hours.

6. The method according to claim 3, characterized in that In step (3), the vacuum degassing treatment condition is a vacuum degree of 0.5 to 1 bar.

7. The method according to claim 3, characterized in that In step (4), the fully blended casting liquid is placed in an environment consistent with the blending conditions in step (2), and poured onto a non-woven fabric, and a flat membrane is scraped out with a scraper; or under the condition of hot nitrogen at a central tube temperature 10°C to 50°C higher than the melting point of polypropylene PP, a double-tube die is used to extrude and cast into a hollow fiber membrane.

8. The method according to claim 3, characterized in that In step (5), the extractant is a substance having greater compatibility and similar polarity to the diluent, including butanone or acetone.

9. An application of the neutron absorbing material-polypropylene blended hydrophobic microporous membrane according to any one of claims 1 to 2, characterized in that: It is applied to the treatment of radioactive wastewater by vacuum membrane distillation.

10. The use according to claim 9, characterized in that: The neutron absorbing material-polypropylene blended hydrophobic microporous membrane has high mechanical stability and high resistance to gamma ray and electron beam radiation. After the industrial wastewater containing radioactive salts at a concentration of 2 g / L is treated by vacuum membrane distillation for one month, the hydrophobicity of the neutron absorbing material-polypropylene blended hydrophobic microporous membrane remains greater than 95%, the mechanical properties of tensile strength and elongation at break still remain greater than 95%, and the interception rate remains greater than 70%.