Preparation method and application of wood-based boron adsorbent

By carrying out epoxylation, amination and functional modification of boron adsorbent on wood, an efficient wood-based boron adsorbent is prepared, which solves the problem of excess boron in water and achieves low-cost and efficient boron adsorption effect. , and improve the mechanical properties and environmental friendliness of the material.

CN118719010AInactive Publication Date: 2024-10-01QINGHAI NORMAL UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411107789.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-01
Estimated Expiration
Not applicable · inactive patent
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a wood-based boron adsorbent, the wood-based boron adsorbent takes a wood block as a base material, the wood block is treated by epichlorohydrin to obtain an epoxy-terminated wood-based material, then the epoxy-terminated wood-based material is treated by ethylenediamine to obtain an aminated wood-based material, and finally the aminated wood-based material is treated by glycidyl to obtain the wood-based boron adsorbent. Under the conditions that the pH is 2-13 and the temperature is 10 DEG C or above, the adsorption capacity of the wood-based boron adsorbent to boron can reach 25 mg / g or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of acid radical ion treatment of boron elements, and more particularly to a preparation method and application of a wood-based boron adsorbent. Background Art

[0002] Wood-based materials are a natural organic polymer material with the advantages of low density, high modulus, high strength, and biodegradability. They are widely used in engineering such as building bridge structures, and civil fields such as furniture and home furnishings. In modern times, wood science has been cross-integrated with other disciplines. Among them, the use of natural biomass materials (mainly wood materials and their derivatives) to manufacture adsorption materials for wastewater treatment has become a research hotspot in recent years. Wood is composed of vessels, tracheids, pits, wood fiber cell cavities, etc., and microfibrils are deposited on the surface of the cell wall to form microscopic gaps, which makes wood have a unique high porosity and three-dimensional structure, and has excellent mechanical strength and more potential functions.

[0003] Boron plays a key role in modern industry and is widely used in glass, ceramics, medicine, fertilizer, aerospace and other fields. However, with the rapid development of my country's social economy and industrial production, the boron content in many water bodies has exceeded the standard, posing a potential danger to the ecological environment. It is urgent to develop a good boron adsorption material to remove the threat of boron to the natural ecology.

[0004] The adsorption method has the advantages of simple process, low cost and high efficiency. Based on the extremely low price cost of wood and its rich active functional groups, a low-cost adsorption material with specific boron adsorption properties can be developed through functional modification, which has important application prospects. Summary of the invention

[0005] In view of this, the present invention provides a preparation method and application of a wood-based boron adsorbent to solve the threat to the natural ecology caused by excessive boron content in many water bodies.

[0006] In order to achieve the above object, the present invention adopts the following technical solution:

[0007] A method for preparing a wood-based boron adsorbent comprises the following steps:

[0008] (1) placing a wood block in a reaction kettle, adding N,N-dimethylformamide and a catalyst, dropping epichlorohydrin during the stirring process, and reacting for a period of time after the dropping is completed; cooling, then dropping sodium hydroxide solution, and continuing to react for a period of time after heating, and then washing with distilled water for 3-5 times to obtain an epoxy-terminated wood-based material;

[0009] (2) placing the epoxy-terminated wood-based material into a reaction kettle, adding ethylenediamine and N,N-dimethylformamide, heating the reaction for a period of time under nitrogen protection, naturally cooling to room temperature, washing with distilled water for 3-5 times, and then vacuum drying or naturally drying to obtain an amino-modified wood-based material;

[0010] (3) The amino-modified wood-based material is placed in a reaction kettle, glycidol and water are added, the temperature is raised under nitrogen protection and reacted for a period of time, the mixture is naturally cooled to room temperature, the mixture is washed with distilled water for 3-5 times, and then vacuum-dried or naturally air-dried to obtain a wood-based boron adsorbent.

[0011] Preferably, the amount of N,N-dimethylformamide added in step (1) is 200-300 mL;

[0012] The mass ratio of the wood block, epichlorohydrin and sodium hydroxide solution is: (30-50): (61.7-102.8): (33.4-55.6).

[0013] Preferably, the catalyst in step (1) is boron trifluoride diethyl ether;

[0014] The dripping speed of the epichlorohydrin is 20-60 drops / min;

[0015] The concentration of the sodium hydroxide solution is 20-30%.

[0016] Preferably, after the dropwise addition in step (1) is completed, the reaction period is reflux at a constant temperature of 40-80° C. for 1-6 hours;

[0017] The cooling is to cool to below 40°C;

[0018] The step of continuing the reaction for a period of time after the temperature is raised is to raise the temperature to 65-85° C. and continue the reaction at a constant temperature for 2-6 hours.

[0019] Preferably, the mass ratio of the terminal epoxy wood-based material to ethylenediamine in step (2) is (30-50): (20-33.4);

[0020] The amount of N,N-dimethylformamide added is 300-8000mL.

[0021] Preferably, the heating reaction period in step (2) is heating to 50-90° C. for 2-8 hours.

[0022] Preferably, the mass ratio of the amino wood-based material to glycidol in step (3) is: (30-50): (10.2-17);

[0023] The amount of water added is 500-1000mL.

[0024] Preferably, the heating and reaction for a period of time in step (3) is heating to 50-90° C. and reacting for 2-8 hours.

[0025] Another object of the present invention is to provide an application of the wood-based boron adsorbent prepared by the preparation method of the above-mentioned wood-based boron adsorbent in boron adsorption, specifically: using the wood-based boron adsorbent to adsorb boron under the conditions of pH 2-13 and temperature>10°C.

[0026] It can be seen from the above technical solutions that, compared with the prior art, the present invention has the following technical effects:

[0027] The adsorbent prepared by the present invention uses wood as a substrate, has a low production cost, and has high material porosity and strong mechanical properties, and can achieve efficient adsorption and rapid separation of boron. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] This embodiment provides a method for preparing a wood-based boron adsorbent, comprising the following steps:

[0031] (1) 30 parts of wood blocks of a certain size are placed in a reactor, 200 mL of N,N-dimethylformamide (DMF) is added, and 1 part of boron trifluoride diethyl ether is added as a catalyst. During the stirring process, 61.7 parts of epichlorohydrin are added dropwise at a rate of about 60 drops / min. After the addition is completed, the mixture is refluxed at a constant temperature of 40° C. for 6 hours; then the mixture is naturally cooled to below 40° C., 33.4 parts of a 30% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 75° C. and the reaction is continued at a constant temperature for 3 hours; after washing with distilled water for 4 times, an epoxy-terminated wood-based material is obtained;

[0032] (2) 30 parts of the epoxy-terminated wood-based material are placed in a reaction kettle, 20.0 parts of ethylenediamine and 300 mL of DMF are added, the temperature is raised to 50° C. under nitrogen protection for reaction for 8 hours, the reaction is naturally cooled to room temperature, the reaction is performed 4 times with distilled water, and the reaction is performed in a vacuum oven or naturally air-dried to obtain an amino-modified wood-based material;

[0033] (3) 30 parts of amino wood-based material were placed in a reactor, 10.2 parts of glycidol and 500 mL of water were added, the temperature was raised to 50 °C under nitrogen protection for 8 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 5 times and then vacuum dried or naturally air-dried to obtain a novel wood-based boron adsorbent.

[0034] The obtained novel wood-based boron adsorbent is used as a boron adsorbent for removing boron from irrigation water. Under the conditions of pH 7.5 and temperature 10°C, its adsorption capacity for HBO2 can reach 25 mg / g.

[0035] Example 2

[0036] This embodiment provides a method for preparing a wood-based boron adsorbent, comprising the following steps:

[0037] (1) 50 parts of wood blocks of a certain size are placed in a reactor, 300 mL of N,N-dimethylformamide (DMF) is added, and 0.9 parts of boron trifluoride diethyl ether is added as a catalyst, and 102.8 parts of epichlorohydrin is added dropwise at a rate of about 50 drops / min during stirring. After the addition is completed, the mixture is refluxed at a constant temperature of 70° C. for 2 hours; then the mixture is naturally cooled to below 40° C., 55.6 parts of a 25% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 85° C. and the reaction is continued at a constant temperature for 2 hours; after washing with distilled water for 3 times, an epoxy-terminated wood-based material is obtained;

[0038] (2) 30 parts of the epoxy-terminated wood-based material are placed in a reaction kettle, 20.0 parts of ethylenediamine and 500 mL of DMF are added, the temperature is raised to 90° C. under nitrogen protection for reaction for 2 h, the mixture is naturally cooled to room temperature, the mixture is washed with distilled water for 4 times, and then vacuum dried or naturally air-dried to obtain an amino-modified wood-based material;

[0039] (3) 50 parts of amino wood-based material were placed in a reactor, 17.0 parts of glycidol and 1000 mL of water were added, the temperature was raised to 60°C under nitrogen protection for 6 hours, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 5 times and then vacuum dried or naturally air-dried to obtain a novel wood-based boron adsorbent.

[0040] The obtained novel wood-based boron adsorbent is used as a boron adsorbent for removing boron from industrial wastewater. Under the conditions of pH 5 and temperature 20°C, its adsorption capacity for HBO2 can reach 32 mg / g.

[0041] Example 3

[0042] This embodiment provides a method for preparing a wood-based boron adsorbent, comprising the following steps:

[0043] (1) 50 parts of wood blocks of a certain size are placed in a reactor, 300 mL of N,N-dimethylformamide (DMF) is added, and 2.5 parts of boron trifluoride diethyl ether is added as a catalyst, and 102.8 parts of epichlorohydrin is added dropwise at a rate of about 30 drops / min during stirring. After the addition is completed, the mixture is refluxed at a constant temperature of 80° C. for 1 hour; then the mixture is naturally cooled to below 40° C., 55.6 parts of a 20% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 65° C. and the reaction is continued at a constant temperature for 6 hours; after washing with distilled water for 3 times, an epoxy-terminated wood-based material is obtained;

[0044] (2) 50 parts of the end-epoxy wood-based material are placed in a reaction kettle, 33.4 parts of ethylenediamine and 800 mL of DMF are added, the temperature is raised to 80° C. under nitrogen protection for reaction for 4 hours, the reaction is naturally cooled to room temperature, the reaction is performed 4 times with distilled water, and the reaction is performed in a vacuum oven or naturally air-dried to obtain an amino-treated wood-based material;

[0045] (3) 40 parts of amino wood-based material were placed in a reactor, 13.6 parts of glycidol and 800 mL of water were added, the temperature was raised to 90 °C under nitrogen protection for reaction for 2 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 5 times and then vacuum dried or naturally air-dried to obtain a novel wood-based boron adsorbent.

[0046] The obtained new wood-based boron adsorbent is used as a boron adsorbent for removing boron from salt lake brine. Under the conditions of pH 9 and temperature 30°C, its adsorption capacity for HBO2 can reach 42 mg / g.

[0047] Example 4

[0048] This embodiment provides a method for preparing a wood-based boron adsorbent, comprising the following steps:

[0049] (1) 40 parts of wood blocks of a certain size are placed in a reactor, 250 mL of N,N-dimethylformamide (DMF) is added, and 1.5 parts of boron trifluoride diethyl ether is added as a catalyst, and 82.3 parts of epichlorohydrin is added dropwise at a rate of about 20 drops / min during stirring. After the addition is completed, the mixture is refluxed at a constant temperature of 65° C. for 3 hours; then the mixture is naturally cooled to below 40° C., 44.5 parts of a 25% aqueous solution of sodium hydroxide is slowly added dropwise to the mixture, and the mixture is heated to 80° C. and the reaction is continued at a constant temperature for 3 hours; after washing with distilled water for 4 times, an epoxy-terminated wood-based material is obtained;

[0050] (2) 40 parts of the end-epoxy wood-based material are placed in a reaction kettle, 26.7 parts of ethylenediamine and 600 mL of DMF are added, the temperature is raised to 60° C. under nitrogen protection for reaction for 7 hours, the reaction is naturally cooled to room temperature, the reaction is performed 4 times with distilled water, and the reaction is performed in a vacuum oven or naturally air-dried to obtain an amino-treated wood-based material;

[0051] (3) 40 parts of amino wood-based material were placed in a reactor, 13.6 parts of glycidol and 500 mL of water were added, the temperature was raised to 80°C under nitrogen protection for reaction for 3 h, and the mixture was naturally cooled to room temperature. The mixture was washed with distilled water for 5 times and then vacuum dried or naturally air-dried to obtain a novel wood-based boron adsorbent.

[0052] The obtained new wood-based boron adsorbent is used as a boron adsorbent for removing boron from geothermal water. Under the conditions of pH 8 and temperature 65°C, its adsorption capacity for HBO2 can reach 53 mg / g.

[0053] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0054] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a wood-based boron adsorbent, characterized in that: The following steps are involved: (1) placing a wood block in a reaction kettle, adding N,N-dimethylformamide and a catalyst, dropping epichlorohydrin during the stirring process, and reacting for a period of time after the dropping is completed; cooling, then dropping a sodium hydroxide solution, heating and continuing the reaction for a period of time, and then washing to obtain an epoxy-terminated wood-based material; (2) placing the epoxy-terminated wood-based material into a reaction kettle, adding ethylenediamine and N,N-dimethylformamide, heating the reaction for a period of time under nitrogen protection, naturally cooling to room temperature, washing, and drying to obtain an amino-modified wood-based material; (3) The aminated wood-based material is placed in a reaction kettle, glycidol and water are added, the temperature is raised under nitrogen protection and the reaction is carried out for a period of time, the mixture is naturally cooled to room temperature, and the mixture is washed and dried to obtain a wood-based boron adsorbent.

2. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The amount of N,N-dimethylformamide added in step (1) is 200-300 mL; The mass ratio of the wood block, epichlorohydrin and sodium hydroxide solution is: (30-50): (61.7-102.8): (33.4-55.6).

3. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The catalyst in step (1) is boron trifluoride diethyl ether; The dripping speed of the epichlorohydrin is 20-60 drops / min; The mass concentration of the sodium hydroxide solution is 20-30%.

4. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: After the dropwise addition in step (1) is completed, the reaction period is 1-6 hours at a constant temperature of 40-80° C. under reflux; The cooling is to cool to below 40°C; The step of continuing the reaction for a period of time after the temperature is raised is to raise the temperature to 65-85° C. and continue the reaction at a constant temperature for 2-6 hours.

5. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The mass ratio of the terminal epoxy wood-based material to ethylenediamine in step (2) is (30-50): (20-33.4); The amount of N,N-dimethylformamide added is 300-8000mL.

6. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The temperature-raising reaction period in step (2) is 50-90° C. for 2-8 hours.

7. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The mass ratio of the amino wood-based material to glycidol in step (3) is: (30-50): (10.2-17); The amount of water added is 500-1000mL.

8. The method for preparing a wood-based boron adsorbent according to claim 1, characterized in that: The heating and reaction for a period of time in step (3) is heating to 50-90° C. and reacting for 2-8 hours.

9. Use of a wood-based boron adsorbent prepared by the method for preparing a wood-based boron adsorbent according to any one of claims 1 to 8 in boron adsorption.

10. The use of the wood-based boron adsorbent in boron adsorption according to claim 9, characterized in that: Boron was adsorbed using a wood-based boron adsorbent at a pH of 2-13 and a temperature >10°C.

Citation Information

Patent Citations

  • Method for preparing wood-based adsorption material from benzylation wood powder and application of wood-based adsorption material

    CN103480342A

  • Method for preparing amino modified sawdust adsorbent and application of method

    CN104772123A

  • Epoxy-terminated hyperbranched polymer, preparation method and application thereof

    CN110330638A

  • Carboxyl-rich attapulgite composite material as well as preparation method and application thereof

    CN115350682A

  • Attapulgite composite material as well as preparation method and application thereof

    CN115350687A