High-silicon low-grade gelled ore concentration process

By using freshly ground phosphate slurry, controlling the concentration and adding TY inhibitors during the flotation process, the problem of deterioration of flotation indicators caused by aging of phosphate slurry in the storage tank has been solved, and the recovery rate and grade of phosphate concentrate have been improved. , achieving a more efficient flotation effect.

CN118719334APending Publication Date: 2024-10-01湖北宜化环保科技有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410889926.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The aging of phosphate ore slurry in the storage tank leads to deterioration of flotation indicators and low recovery rate of phosphate concentrate, and unreasonable concentration and inhibitor selection of phosphate ore slurry result in low recovery rate of phosphate concentrate.

Method used

Use freshly ground phosphate ore slurry for flotation, control the concentration of phosphate ore slurry at 20-25%, add TY inhibitors to the water glass solution, and add reagents in multiple stages for reaction to increase the recovery rate of phosphate concentrate.

Benefits of technology

It improves the recovery rate and grade of phosphate concentrate, reduces the taste of tailings, enhances the flotation effect, and significantly increases the recovery rate of phosphate concentrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719334A_ABST
    Figure CN118719334A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of flotation of phosphorite pulp, and discloses a high-silicon low-grade gelled ore concentration process which comprises the following steps: S1, pilot-scale ore grinding operation of phosphorite, S2, direct flotation primary roughing, S3, direct flotation secondary roughing, S4, direct flotation primary concentration, S5, direct flotation secondary concentration and S6, reverse flotation roughing. The aging time of the phosphoric ore pulp in the storage tank is too long, so that the grade of concentrate is reduced, the recovery rate is greatly reduced, and the freshly ground phosphoric ore pulp is selected during flotation of the phosphoric ore pulp; during direct flotation operation of the phosphoric ore pulp, the concentration of the phosphoric ore pulp is controlled to be 20-25%, the recovery rate of the phosphate concentrate can be increased, and the grade of the phosphate concentrate is 19-20%; during the direct flotation operation of the phosphoric ore pulp, a TY inhibitor is added into a water glass solution, so that the recovery rate of phosphate concentrate is further improved; and during reverse flotation operation of the phosphoric ore pulp, the concentration of the phosphoric ore pulp is controlled to be 25% or above, and the recovery rate of phosphate concentrate can be further increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of phosphate slurry flotation, in particular to a high-silicon low-grade gelled ore beneficiation process. Background Art

[0002] Flotation of phosphate slurry is an important part of the phosphate beneficiation process. It is based on the difference in surface properties between phosphate minerals and impurity minerals. Through the action of flotation agents, phosphate minerals are separated from impurity minerals to obtain high-grade phosphate concentrate.

[0003] The flotation of phosphate slurry includes direct forward flotation, single reverse flotation, forward-reverse flotation, reverse-forward flotation and double reverse flotation.

[0004] The current flotation process of phosphate slurry has the following defects:

[0005] 1. Due to the limitation of the grinding capacity of the pilot line, the ore must be ground into slurry in advance and stored in two 1000L storage tanks. Considering that the slurry is aged in the storage tank for too long, the surface ions of calcium-containing minerals in the slurry may be dissolved, and the Ca in the solution may be 2+ Mg 2+ Accumulation leads to deterioration of flotation indicators;

[0006] 2. In the positive flotation operation of phosphate slurry, the unreasonable selection of the concentration of phosphate slurry can easily lead to low recovery rate of phosphate concentrate;

[0007] 3. In the reverse flotation operation of phosphate slurry, unreasonable selection of phosphate slurry concentration will also lead to low recovery rate of phosphate concentrate;

[0008] 4. In the positive flotation operation of phosphate slurry, if the selection and dosage of inhibitors are not accurately controlled, the tailings obtained will have a high grade, thereby reducing the recovery rate of phosphate concentrate.

[0009] Therefore, we need to propose a high-silicon low-grade gelled ore beneficiation process to improve the recovery rate of phosphate concentrate. Summary of the invention

[0010] The object of the present invention is to provide a high-silicon low-grade gelled ore beneficiation process. By comparing the flotation test of freshly ground phosphate slurry and storage tank phosphate slurry, it is found that the aging time of the phosphate slurry in the storage tank is too long, which not only reduces the grade of the concentrate, but also leads to a significant reduction in the recovery rate. Therefore, freshly ground phosphate slurry is selected for phosphate slurry flotation; during the positive flotation operation of the phosphate slurry, the concentration of the phosphate slurry is controlled at 20-25%, which can improve the recovery rate of the phosphate concentrate, and the grade of the phosphate concentrate is 19-20%; during the positive flotation operation of the phosphate slurry, TY inhibitor is added to the water glass solution, which can not only reduce the grade of the tailings, but also improve the flotation effect, thereby further improving the recovery rate of the phosphate concentrate; and during the reverse flotation operation of the phosphate slurry, the concentration of the phosphate slurry is controlled at more than 25%, which can further improve the recovery rate of the phosphate concentrate, so as to solve the problems raised in the above background technology.

[0011] To achieve the above object, the present invention provides the following technical solution: a high-silicon low-grade gelled ore beneficiation process, comprising the following steps:

[0012] S1. Pilot grinding of phosphate rock: grinding phosphate rock into fine particles and making phosphate slurry;

[0013] S2. First roughing of positive flotation: add the following reagents to the phosphate slurry in sequence: sodium carbonate solution, water glass solution, TY inhibitor, MG-3 solution, so that the reagents react with the phosphate slurry;

[0014] S3, positive flotation secondary roughing: continue to add MG-3 solution to the phosphate slurry after the reaction with the reagent to continue the reaction, and filter out the obtained tailings X1;

[0015] S4, positive flotation primary concentration: adding sodium carbonate solution and water glass solution to the phosphate slurry from which the tailing X1 is filtered out, and continuing the reaction, filtering out the obtained middling ore 1;

[0016] S5, positive flotation secondary concentration: sodium carbonate solution and water glass solution are continuously added to the phosphate slurry from which the medium ore 1 is filtered out to react, and the obtained medium ore 2 is filtered out;

[0017] S6, reverse flotation roughing: add the reagents phosphoric acid solution, sulfuric acid solution and MG-7 solution to the phosphate slurry from which the middling ore 2 is filtered out to react again, and filter out the obtained tailings X2 and concentrate K.

[0018] Preferably, in step S1, the phosphate slurry is freshly ground phosphate slurry, and the pilot grinding operation of the phosphate ore adopts a two-stage grinding process of a first-stage ball mill and a second-stage stirred mill. Among the ground phosphate ore particles, the proportion of particles with a mesh size of less than 200 mesh is greater than 92%.

[0019] Preferably, in step S2, the solubility of the added pharmaceutical agents is respectively:

[0020] Concentration of sodium carbonate solution: 4KG / t;

[0021] Concentration of water glass solution: 1.3KG / t;

[0022] TY inhibitor concentration: 0.5KG / t;

[0023] Concentration of MG-3 solution: 1.25KG / t.

[0024] Preferably, in step S3, the concentration of the added MG-3 solution is 0.5 KG / t.

[0025] Preferably, in step S4, the concentration of the sodium carbonate solution added in the primary flotation concentration process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

[0026] Preferably, in step S5, the concentration of the sodium carbonate solution added in the positive flotation secondary concentration process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

[0027] Preferably, in step S6, the concentrations of reagents added in the reverse flotation roughing process are:

[0028] Concentration of phosphoric acid solution: 3KG / t;

[0029] Concentration of sulfuric acid solution: 16KG / t;

[0030] Concentration of MG-7 solution: 0.8KG / t.

[0031] Preferably, in the positive flotation operation of phosphate slurry, the concentration of the phosphate slurry is controlled at 20%-25%.

[0032] Preferably, in the reverse flotation roughing operation of the phosphate slurry, the concentration of the phosphate slurry is controlled to be above 25%.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The present invention compares the flotation test of freshly ground phosphate slurry and storage tank phosphate slurry, and finds that the aging time of phosphate slurry in the storage tank is too long, which not only reduces the grade of the concentrate, but also leads to a significant reduction in the recovery rate. Therefore, freshly ground phosphate slurry is used in the flotation of phosphate slurry;

[0035] 2. During the positive flotation operation of the phosphate slurry of the present invention, the concentration of the phosphate slurry is controlled at 20-25%, which can improve the recovery rate of the phosphate concentrate, and the grade of the phosphate concentrate is 19-20%;

[0036] 3. In the present invention, when the phosphate slurry is flotated, the TY inhibitor is added to the water glass solution, which can not only reduce the taste of the tailings, but also improve the flotation effect, thereby further improving the recovery rate of the phosphate concentrate;

[0037] 4. In the present invention, during the reverse flotation operation of phosphate slurry, the concentration of phosphate slurry is controlled at more than 25%, which can further improve the recovery rate of phosphate concentrate. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a flowchart of the present invention;

[0039] Figure 2 It is a flow chart of the flotation test of the freshly ground phosphate slurry and the storage tank phosphate slurry of the present invention;

[0040] Figure 3 It is a flow chart of the positive flotation pulp concentration test of the present invention;

[0041] Figure 4 It is a flowchart of the positive flotation inhibitor dosage test of the present invention;

[0042] Figure 5 It is a flow chart of the reverse flotation roughing pulp concentration test of the present invention;

[0043] Figure 6 is a process flow chart of the present invention;

[0044] Figure 7 The process flow chart of the flotation test of the freshly ground phosphate slurry and the storage tank phosphate slurry of the present invention;

[0045] Figure 8 It is a process flow chart of the positive flotation pulp concentration test of the present invention;

[0046] Fig. 9 The process flow chart of the positive flotation inhibitor dosage test of the present invention is as follows;

[0047] Fig.10 It is a process flow chart of the reverse flotation roughing pulp concentration test of the present invention. DETAILED DESCRIPTION

[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] See also Figure 1-10The present invention provides a technical solution: a high-silicon low-grade gelled ore beneficiation process, which adopts a desiliconization positive flotation-demagnesiumization reverse flotation process to achieve the flotation of phosphate slurry, comprising the following steps:

[0050] S1. Pilot grinding of phosphate rock: grinding phosphate rock into fine particles and making phosphate slurry;

[0051] In step S1, the phosphate slurry is freshly ground phosphate slurry, and the pilot grinding operation of the phosphate ore adopts a two-stage grinding process of a first-stage ball mill and a second-stage stirred mill. Among the ground phosphate ore particles, the proportion of particles with a mesh size of less than 200 mesh is greater than 92%.

[0052] S2. First roughing of positive flotation: add the following reagents to the phosphate slurry in sequence: sodium carbonate solution, water glass solution, TY inhibitor, MG-3 solution, so that the reagents react with the phosphate slurry;

[0053] In step S2, the solubility of the added agents is respectively:

[0054] Concentration of sodium carbonate solution: 4KG / t;

[0055] Concentration of water glass solution: 1.3KG / t;

[0056] TY inhibitor concentration: 0.5KG / t;

[0057] Concentration of MG-3 solution: 1.25KG / t.

[0058] S3, positive flotation secondary roughing: continue to add MG-3 solution to the phosphate slurry after the reaction with the reagent to continue the reaction, and filter out the obtained tailings X1;

[0059] In step S3, the concentration of the added MG-3 solution is 0.5 KG / t.

[0060] S4, positive flotation primary concentration: adding sodium carbonate solution and water glass solution to the phosphate slurry from which the tailing X1 is filtered out, and continuing the reaction, filtering out the obtained middling ore 1;

[0061] In step S4, the concentration of the sodium carbonate solution added in the primary flotation concentration process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

[0062] S5, positive flotation secondary concentration: sodium carbonate solution and water glass solution are continuously added to the phosphate slurry from which the medium ore 1 is filtered out to react, and the obtained medium ore 2 is filtered out;

[0063] In step S5, the concentration of the sodium carbonate solution added in the secondary flotation selection process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

[0064] S6, reverse flotation roughing: add the reagents phosphoric acid solution, sulfuric acid solution and MG-7 solution to the phosphate slurry from which the middling ore 2 is filtered out to react again, and filter out the obtained tailings X2 and concentrate K.

[0065] In step S6, the concentrations of reagents added in the reverse flotation roughing process are:

[0066] Concentration of phosphoric acid solution: 3KG / t;

[0067] Concentration of sulfuric acid solution: 16KG / t;

[0068] Concentration of MG-7 solution: 0.8KG / t.

[0069] In the positive flotation operation of phosphate slurry, the concentration of phosphate slurry is controlled at 20%-25%.

[0070] In the reverse flotation roughing operation of phosphate slurry, the concentration of phosphate slurry is controlled at above 25%.

[0071] Table 1 Phosphate slurry flotation process results

[0072]

[0073] Specifically, the flotation process of the above phosphate slurry needs to be verified through the following multiple tests:

[0074] Comparison of flotation test between freshly ground phosphate slurry and storage tank phosphate slurry: Compared with freshly ground phosphate slurry, the effect of dissolved calcium ions and magnesium ions on flotation index after aging of storage tank phosphate slurry was verified;

[0075] The prepared phosphate slurry is stored in two 1000L storage tanks, and after the phosphate slurry is aged in the storage tanks for a period of time, calcium ions and magnesium ions on the surface of calcium minerals in the phosphate slurry are dissolved and accumulated.

[0076] The flotation test comparison of freshly ground phosphate slurry and storage tank phosphate slurry includes the following processes:

[0077] S21, respectively selecting freshly ground phosphate slurry and storage tank phosphate slurry having the same concentration, volume and flotation temperature;

[0078] S22, direct flotation primary roughing: sodium carbonate solution, water glass solution, TY inhibitor and MG-3 solution are added to the ground phosphate slurry and the storage tank phosphate slurry in sequence to react;

[0079] S23, after a period of reaction, the concentrate K is filtered out, and a secondary roughing separation is performed by positive flotation, and then MG-3 solution is added to the phosphate slurry. After a period of reaction, the tailings X is filtered out.

[0080] The temperature of positive flotation is controlled at 47-53℃, the concentration of sodium carbonate solution is 4KG / t, the concentration of water glass solution is 1.3KG / t, the concentration of TY inhibitor is 0.5KG / t, the concentration of MG-3 solution added in the first roughing of positive flotation is 1.25KG / t, and the concentration of MG-3 solution added in the second roughing of positive flotation is 0.5KG / t.

[0081] Table 2 Results of positive flotation pulp aging test

[0082]

[0083] From the results in Table 2, it can be seen that compared with the freshly ground slurry, the long aging time of the slurry in the storage tank not only reduces the grade of the concentrate, but also leads to a significant decrease in the recovery rate.

[0084] Direct flotation phosphate slurry concentration test: verify the effect of the concentration of direct flotation phosphate slurry on the direct flotation index;

[0085] The positive flotation slurry concentration test includes the following processes:

[0086] S31, selecting three groups of phosphate slurries with concentrations of 21.26%, 28.66%, and 34.28%, respectively, and the volumes and flotation temperatures of the three groups of phosphate slurries are the same;

[0087] S32, direct flotation primary roughing: sodium carbonate solution, water glass solution, TY inhibitor and MG-3 solution are sequentially added to the three groups of phosphate slurries to react;

[0088] S33, after a period of reaction, the concentrate K is filtered out, and a secondary roughing separation is performed by positive flotation, and then MG-3 solution is added to the phosphate slurry. After a period of reaction, the tailings X is filtered out.

[0089] The temperature of the positive flotation was controlled at 47-53°C, and the order and concentration of addition of sodium carbonate solution, water glass solution, TY inhibitor and MG-3 solution were the same as those in the flotation test comparison of freshly ground phosphate slurry and storage tank phosphate slurry.

[0090] Table 3 Results of positive flotation pulp concentration test

[0091]

[0092] From the results in Table 3, it can be seen that as the concentration of the positive flotation pulp increases from 21.26% to 34.28%, the grade of the flotation tailings gradually increases and the recovery rate decreases significantly; the grade of the flotation concentrate is between 19% and 20%; from the perspective of improving the recovery rate, it is more appropriate to control the concentration of the positive flotation operation at 20% to 25%.

[0093] Positive flotation inhibitor dosage test: verify the effect of positive flotation inhibitor dosage on positive flotation indicators;

[0094] The positive flotation depressant dosage test includes the following process:

[0095] S41, select three groups of phosphate slurries with a concentration of 28%, and control the positive flotation temperature at 47-53°C;

[0096] S42, adding a sodium carbonate solution with a concentration of 4 KG / t, a water glass solution with a concentration of 2980 g / t, and an MG-3 solution with a concentration of 1.25 KG / t to the first group of phosphate slurry for reaction;

[0097] Adding a sodium carbonate solution with a concentration of 4 KG / t, a water glass solution with a concentration of 5559 g / t, and an MG-3 solution with a concentration of 1.25 KG / t to the second group of phosphate slurry for reaction;

[0098] Adding a sodium carbonate solution with a concentration of 4 KG / t, a TY inhibitor with a concentration of 1111 g / t, and an MG-3 solution with a concentration of 1.25 KG / t to the third group of phosphate slurry for reaction;

[0099] S43, after a period of reaction, the concentrate K is filtered out, and a secondary roughing separation is performed by positive flotation, and then MG-3 solution is added to the three groups of phosphate slurries respectively, and after a period of reaction, the tailings X is filtered out.

[0100] Table 4 Test results of positive flotation depressant dosage

[0101]

[0102] From the results in Table 4, it can be seen that increasing the amount of water glass can effectively reduce the tailings grade, and the addition of TY inhibitor can improve the fragility of the foam and the flotation selectivity. The use of mixed inhibitors (water glass combined with TY) in the pilot test has better separation effect.

[0103] Reverse flotation roughing slurry concentration test: verify the effect of reverse flotation roughing phosphate slurry concentration on reverse flotation indicators.

[0104] The reverse flotation roughing pulp concentration test includes the following processes:

[0105] S51, select three groups of phosphate slurries with concentrations of 10.34%, 17.42%, and 33.56% respectively;

[0106] S52, respectively adding a phosphoric acid solution with a concentration of 3 KG / t, a sulfuric acid solution with a concentration of 16 KG / t, and an MG-7 solution with a concentration of 0.8 KG / t to the three groups of phosphate slurries to react;

[0107] S53. After the reaction, the tailings X and concentrates K in the three groups of phosphate slurries are filtered out respectively.

[0108] Table 5 Reverse flotation roughing pulp concentration test results

[0109]

[0110] From the results in Table 5, it can be seen that the higher the concentration of the roughing slurry of the magnesium removal reverse flotation, the higher the concentrate recovery rate. During the pilot test, the concentration of the roughing slurry of the magnesium removal reverse flotation was controlled above 25%, and the separation effect was better.

[0111] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-silicon low-grade gelled ore beneficiation process, characterized in that: The following steps are involved: S1. Pilot grinding of phosphate rock: grinding phosphate rock into fine particles and making phosphate slurry; S2. First roughing of positive flotation: add the following reagents to the phosphate slurry in sequence: sodium carbonate solution, water glass solution, TY inhibitor, MG-3 solution, so that the reagents react with the phosphate slurry; S3, positive flotation secondary roughing: continue to add MG-3 solution to the phosphate slurry after the reaction with the reagent to continue the reaction, and filter out the obtained tailings X1; S4, positive flotation primary concentration: adding sodium carbonate solution and water glass solution to the phosphate slurry from which the tailing X1 is filtered out, and continuing the reaction, filtering out the obtained middling ore 1; S5, positive flotation secondary concentration: sodium carbonate solution and water glass solution are continuously added to the phosphate slurry from which the medium ore 1 is filtered out to react, and the obtained medium ore 2 is filtered out; S6, reverse flotation roughing: add the reagents phosphoric acid solution, sulfuric acid solution and MG-7 solution to the phosphate slurry from which the middling ore 2 is filtered out to react again, and filter out the obtained tailings X2 and concentrate K.

2. A high-silicon low-grade gelled ore beneficiation process according to claim 1, characterized in that: In step S1, the phosphate slurry is freshly ground phosphate slurry, and the pilot grinding operation of the phosphate ore adopts a two-stage grinding process of a first-stage ball mill and a second-stage stirred mill. Among the ground phosphate ore particles, the proportion of particles with a mesh size of less than 200 mesh is greater than 92%.

3. The high-silicon low-grade gelled ore concentration process according to claim 1 is characterized in that: In step S2, the solubility of the added agents is respectively: Concentration of sodium carbonate solution: 4KG / t; Concentration of water glass solution: 1.3KG / t; TY inhibitor concentration: 0.5KG / t; Concentration of MG-3 solution: 1.25KG / t.

4. A high-silicon low-grade gelled ore beneficiation process according to claim 1, characterized in that: In step S3, the concentration of the added MG-3 solution is 0.5 KG / t.

5. The high-silicon low-grade gelled ore concentration process according to claim 1 is characterized in that: In step S4, the concentration of the sodium carbonate solution added in the primary flotation concentration process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

6. A high-silicon low-grade gelled ore concentration process according to claim 1, characterized in that: In step S5, the concentration of the sodium carbonate solution added in the secondary flotation selection process is 0.5 KG / t, the concentration of the water glass solution added is 0.5 KG / t, and the sodium carbonate solution and the water glass solution are added in sequence.

7. The high-silicon low-grade gelled ore concentration process according to claim 1 is characterized by: In step S6, the concentrations of reagents added in the reverse flotation roughing process are: Concentration of phosphoric acid solution: 3KG / t; Concentration of sulfuric acid solution: 16KG / t; Concentration of MG-7 solution: 0.8KG / t.

8. The high-silicon low-grade gelled ore concentration process according to claim 1 is characterized in that: In the positive flotation operation of phosphate slurry, the concentration of phosphate slurry is controlled at 20%-25%.

9. A high-silicon low-grade gelled ore beneficiation process according to claim 1, characterized in that: In the reverse flotation roughing operation of phosphate slurry, the concentration of phosphate slurry is controlled at above 25%.

Citation Information

Patent Citations

  • Method for performing fine sieving, regrinding and bulk flotation on low-level silicon calcium collophanite

    CN103949318A

  • Process for mineral processing of low-grade silicon calcium collophanite

    CN105597939A

  • Low-grade mixed type collophanite flotation method

    CN113731637A