High-strength fastener surface treatment process and processing method thereof

Through high-strength fastener surface treatment process, including oil removal, shot blasting and coating steps, the problem of insufficient fatigue and corrosion resistance of grade 12.9 bolts is solved, and high corrosion resistance and fatigue resistance of fasteners are achieved, which is suitable for In the engine cylinder head and anti-collision beam, etc.

CN118719503APending Publication Date: 2024-10-01NINGBO JISHI METAL NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410926620.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The existing grade 12.9 bolts have low fatigue strength, poor environmental corrosion resistance, and low delayed fracture performance, and cannot meet the application needs in engine cylinder heads, anti-collision beams, etc.

Method used

A high-strength fastener surface treatment process is adopted, including incoming material inspection, oil removal treatment, shot blasting treatment, primer coating and topcoat coating, through strong alkaline solution, shot blasting machine and baking steps to improve Corrosion resistance and friction coefficient of fasteners.

Benefits of technology

It achieves good corrosion resistance and high fatigue strength of the fasteners. It passes the salt spray test without white rust for 240 hours and without red rust for 850 hours. It meets the requirements of friction coefficient in the range of 0.10-0.16 and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118719503A_ABST
    Figure CN118719503A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fastener surface treatment and machining, and particularly discloses a high-strength fastener surface treatment process and a machining method thereof.The high-strength fastener surface treatment process comprises the following steps that after incoming materials are inspected, products are put on line and poured; performing oil removal treatment; shot blasting treatment; carrying out primer coating treatment; carrying out finish paint coating treatment; and detecting, selecting and packaging. The fastener disclosed by the invention has good corrosion resistance, and is free of white rust after being tested by salt spray for 240 hours and free of red rust after being tested by salt spray for 850 hours; and the friction coefficient is good, tests show that mu tot is 0.10-0.16, the fatigue resistance is high, and the delayed fracture performance is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fastener surface treatment and processing, and in particular to a high-strength fastener surface treatment process and a processing method thereof. Background Art

[0002] Bolts are a common fastener, usually consisting of a rod-shaped part with threads and a connected part (usually a nut) with a threaded hole. Bolts are screwed into nuts or threaded holes to clamp the connected parts to achieve the purpose of mechanical connection. Bolts are widely used in various fields such as machinery, construction, automobiles, aerospace, etc.

[0003] The main components of a bolt include:

[0004] Threaded portion: The main part of the bolt, usually spiral, that is used to screw into a nut or threaded hole;

[0005] Head: The top of a bolt, used for tools such as a spanner or wrench to install and remove the bolt. Bolt heads come in different shapes and designs, with hexagonal, square, and round heads being common.

[0006] Bolt body: The part connecting the threaded part and the head, usually a cylinder with a larger diameter and a certain length;

[0007] Thread: The spiral groove on the bolt is used to cooperate with the nut or threaded hole to tighten and loosen the bolt;

[0008] Tail: The end of a bolt, usually the smaller diameter portion of the bolt body used to provide additional tension and support.

[0009] There are many types of bolts, which can be divided into many types according to different shapes, materials, thread types, surface treatments and other factors, such as hexagonal head bolts, round head bolts, high-strength bolts, stainless steel bolts, etc. Choosing the right type of bolt depends on the specific application scenario and requirements. When using bolts, you need to pay attention to the correct selection and installation to ensure the reliability and safety of the connection.

[0010] Grade 12.9 bolts are high-strength bolts that are often used in engineering applications that need to withstand high loads or high tension. Bolts of this grade are often used in important structures and connection parts in the engineering and mechanical fields, such as bridges, high-rise buildings, aerospace devices, etc., because they can provide reliable connections and tensile resistance to ensure the safety and stability between connected parts. When using grade 12.9 bolts, you need to pay attention to the correct installation and tightening force to ensure the quality and reliability of the connection.

[0011] The existing 12.9 grade bolts have low fatigue strength, poor environmental corrosion resistance, and low delayed fracture performance, which are not conducive to application in engine cylinder heads, anti-collision beams and other locations, and their performance cannot meet the requirements of use.

[0012] At present, there is no surface treatment process for zinc-aluminum coating in China. Therefore, we need to research the zinc-aluminum coating process. Summary of the invention

[0013] In view of the problems in the related technology, the present invention proposes a high-strength fastener surface treatment process and a processing method thereof to overcome the above-mentioned technical problems existing in the existing related technology. The purpose of the present invention is to make the fastener have good corrosion resistance and friction coefficient, high fatigue strength and strong delayed fracture performance.

[0014] To achieve the above object, the present invention provides the following technical solutions:

[0015] A high-strength fastener surface treatment process comprises the following steps:

[0016] S1. After the incoming materials are inspected, the products are put on line for unloading;

[0017] S2. Oil removal treatment:

[0018] Clean the waste oil on the workpiece in a strong alkaline solution, then pour the workpiece into the upper hopper and soak it in the alkaline tank. After two alkaline washes for a total of 15 minutes;

[0019] After the alkali cleaning is completed, the workpieces are sequentially put into the water tank next to the alkali tank and cleaned with clean water;

[0020] After being washed with clean water, the workpiece enters the hot water tank, which not only cleans the workpiece but also heats the workpiece;

[0021] S3, shot blasting:

[0022] Pour the cleaned workpiece into the shot blasting machine and take it out after 25 minutes;

[0023] S4, Primer coating treatment:

[0024] The workpieces after shot blasting are poured into the basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0025] S5. Topcoat coating treatment:

[0026] The workpieces with primer are introduced into the topcoat basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0027] S6, inspection, selection and packaging.

[0028] Preferably, in S2, the strong alkaline solution is composed of sodium hydroxide, potassium hydroxide and an auxiliary agent, and each liter of the strong alkaline solution contains 6-10g of sodium hydroxide and 10-15g of potassium hydroxide. The reaction temperature is 55-75°C, and the hot water temperature is 60-80°C.

[0029] Preferably, in S3, the shot blasting time is 25 min and the current is 20 A.

[0030] Preferably, in S4, the baking time is 20-40 min, the temperature is 220-250° C., and the coating amount is 90-130 mg / dm 2 .

[0031] Preferably, in S5, the baking time is 15-30 min, the temperature is 190-210° C., and the coating amount is 50-80 mg / dm 2 .

[0032] To achieve the above object, the present invention also provides the following technical solutions:

[0033] A method for processing a high-strength fastener comprises any one of the above-mentioned surface treatment processes for the high-strength fastener.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention discloses a surface treatment process and a processing method for a high-strength fastener, which enables the fastener to have good corrosion resistance, and has no white rust after 240 hours of salt spray test and no red rust after 850 hours; and has a good friction coefficient, which fully meets μtot: 0.10-0.16 after testing, has high fatigue resistance and strong delayed fracture performance. The fastener of the present invention is applied to engine cylinder heads, anti-collision beams and other positions, and its performance meets the use requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] The invention discloses a high-strength fastener surface treatment process, comprising the following steps:

[0040] S1. After the incoming materials are inspected, the products are put on line for unloading;

[0041] S2. Oil removal treatment:

[0042] Clean the waste oil on the workpiece in a strong alkaline solution, then pour the workpiece into the upper hopper and soak it in the alkaline tank. After two alkaline washes for a total of 15 minutes;

[0043] After the alkali cleaning is completed, the workpieces are sequentially put into the water tank next to the alkali tank and cleaned with clean water;

[0044] After being washed with clean water, the workpiece enters the hot water tank, which not only cleans the workpiece but also heats the workpiece;

[0045] Furthermore, the strong alkaline solution is composed of sodium hydroxide, potassium hydroxide and an auxiliary agent, each liter of the strong alkaline solution contains 8g of sodium hydroxide and 12g of potassium hydroxide, the reaction temperature is 55°C, and the hot water temperature is 60°C;

[0046] S3, shot blasting:

[0047] Pour the cleaned workpiece into the shot blasting machine and take it out after 25 minutes;

[0048] Furthermore, the shot blasting time was 25 min and the current was 20 A;

[0049] S4, Primer coating treatment:

[0050] The workpieces after shot blasting are poured into the basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0051] Furthermore, the baking time is 32 min, the temperature is 220 ° C, and the coating amount is 90 mg / dm 2 ;

[0052] S5. Topcoat coating treatment:

[0053] The workpieces with primer are introduced into the topcoat basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0054] Furthermore, in S5, the baking time is 15 min, the temperature is 190° C., and the coating amount is 50 mg / dm 2 ;

[0055] S6, inspection, selection and packaging.

[0056] To achieve the above object, the present invention also provides the following technical solutions:

[0057] A method for processing a high-strength fastener comprises any one of the above-mentioned surface treatment processes for the high-strength fastener.

[0058] Example 2

[0059] The invention discloses a high-strength fastener surface treatment process, comprising the following steps:

[0060] S1. After the incoming materials are inspected, the products are put on line for unloading;

[0061] S2. Oil removal treatment:

[0062] Clean the waste oil on the workpiece in a strong alkaline solution, then pour the workpiece into the upper hopper and soak it in the alkaline tank. After two alkaline washes for a total of 15 minutes;

[0063] After the alkali cleaning is completed, the workpieces are sequentially put into the water tank next to the alkali tank and cleaned with clean water;

[0064] After being washed with clean water, the workpiece enters the hot water tank, which not only cleans the workpiece but also heats the workpiece;

[0065] Furthermore, the strong alkaline solution is composed of sodium hydroxide, potassium hydroxide and an auxiliary agent, each liter of the strong alkaline solution contains 10g of sodium hydroxide and 10g of potassium hydroxide, the reaction temperature is 55°C, and the hot water temperature is 60°C;

[0066] S3, shot blasting:

[0067] Pour the cleaned workpiece into the shot blasting machine and take it out after 25 minutes;

[0068] Furthermore, the shot blasting time was 25 min and the current was 20 A;

[0069] S4, Primer coating treatment:

[0070] The workpieces after shot blasting are poured into the basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0071] Furthermore, the baking time is 20 min, the temperature is 220 ° C, and the coating amount is 90 mg / dm 2 ;

[0072] S5. Topcoat coating treatment:

[0073] The workpieces with primer are introduced into the topcoat basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0074] Furthermore, in S5, the baking time is 15 min, the temperature is 190° C., and the coating amount is 50 mg / dm 2 ;

[0075] S6, inspection, selection and packaging.

[0076] To achieve the above object, the present invention also provides the following technical solutions:

[0077] A method for processing a high-strength fastener comprises any one of the above-mentioned surface treatment processes for the high-strength fastener.

[0078] Example 3

[0079] The invention discloses a high-strength fastener surface treatment process, comprising the following steps:

[0080] S1. After the incoming materials are inspected, the products are put on line for unloading;

[0081] S2. Oil removal treatment:

[0082] Clean the waste oil on the workpiece in a strong alkaline solution, then pour the workpiece into the upper hopper and soak it in the alkaline tank. After two alkaline washes for a total of 15 minutes;

[0083] After the alkali cleaning is completed, the workpieces are sequentially put into the water tank next to the alkali tank and cleaned with clean water;

[0084] After being washed with clean water, the workpiece enters the hot water tank, which not only cleans the workpiece but also heats the workpiece;

[0085] Furthermore, the strong alkaline solution is composed of sodium hydroxide, potassium hydroxide and an auxiliary agent, each liter of the strong alkaline solution contains 7g of sodium hydroxide and 11g of potassium hydroxide, the reaction temperature is 64°C, and the hot water temperature is 76°C;

[0086] S3, shot blasting:

[0087] Pour the cleaned workpiece into the shot blasting machine and take it out after 25 minutes;

[0088] Furthermore, the shot blasting time was 25 min and the current was 20 A;

[0089] S4, Primer coating treatment:

[0090] The workpieces after shot blasting are poured into the basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0091] Furthermore, the baking time is 32 min, the temperature is 245 ° C, and the coating amount is 112 mg / dm 2 ;

[0092] S5. Topcoat coating treatment:

[0093] The workpieces with primer are introduced into the topcoat basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking.

[0094] Furthermore, in S5, the baking time is 21 minutes, the temperature is 198°C, and the coating amount is 75 mg / dm 2 ;

[0095] S6, inspection, selection and packaging.

[0096] To achieve the above object, the present invention also provides the following technical solutions:

[0097] A method for processing a high-strength fastener comprises any one of the above-mentioned surface treatment processes for the high-strength fastener.

[0098] Table 1 below shows the different data.

[0099]

[0100]

[0101] Table 1

[0102] μtot: ①0.127②0.120③0.122④0.121⑤0.120

[0103] The fastener of the present invention has good corrosion resistance, and after a salt spray test, there is no white rust for 240 hours and no red rust for 850 hours; and has a good friction coefficient, and after a test, it fully meets μtot: 0.10-0.16, has high fatigue resistance, and has strong delayed fracture performance. The fastener of the present invention is applied to engine cylinder heads, anti-collision beams and other positions, and its performance meets the use requirements, is better than 12.9 grade bolts, and prolongs the service life.

[0104] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength fastener surface treatment process, characterized in that: The following steps are involved: S1. After the incoming materials are inspected, the products are put on line for unloading; S2. Oil removal treatment: Clean the waste oil on the workpiece in a strong alkaline solution, then pour the workpiece into the upper hopper and soak it in the alkaline tank. After two alkaline washes for a total of 15 minutes; After the alkali cleaning is completed, the workpieces are sequentially put into the water tank next to the alkali tank and cleaned with clean water; After being washed with clean water, the workpiece enters the hot water tank, which not only cleans the workpiece but also heats the workpiece; S3, shot blasting: Pour the cleaned workpiece into the shot blasting machine and take it out after 25 minutes; S4, Primer coating treatment: The workpieces after shot blasting are poured into the basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking. S5. Topcoat coating treatment: The workpieces with primer are introduced into the topcoat basket. After dipping and centrifugation, the surface of the parts absorbs the coating liquid and is poured onto the conveyor belt for baking. S6, inspection, selection and packaging.

2. A high-strength fastener surface treatment process according to claim 1, characterized in that: In S2, the strong alkaline solution is composed of sodium hydroxide, potassium hydroxide and an auxiliary agent. Each liter of the strong alkaline solution contains 6-10g of sodium hydroxide and 10-15g of potassium hydroxide. The reaction temperature is 55-75°C, and the hot water temperature is 60-80°C.

3. The high-strength fastener surface treatment process and processing method according to claim 1, characterized in that: In S3, the shot blasting time is 25 minutes and the current is 20A.

4. The high-strength fastener surface treatment process according to claim 1, characterized in that: In S4, the baking time is 20-40 minutes, the temperature is 220-250° C., and the coating amount is 90-130 mg / dm 2 .

5. The high-strength fastener surface treatment process according to claim 1, characterized in that: In S5, the baking time is 15-30 minutes, the temperature is 190-210° C., and the coating amount is 50-80 mg / dm 2 .

6. A method for processing a high-strength fastener, characterized in that: A high-strength fastener surface treatment process comprising the process described in any one of claims 1-5.

Citation Information

Patent Citations

  • Anticorrosive technology used for marine environment fastener

    CN102974519A

  • Fastener surface treatment method

    CN108187992A

  • Fastener surface treatment process

    CN108893729A

  • Processing method of fastener anticorrosive coating

    CN110961324A

  • Dacromet coating method for anti-loose fastener

    CN114453225A