Carbon-plastic composite board as well as preparation method, preparation device and application thereof
By adhering the carbon powder to the resin liquid column in situ and forming a fiber network structure, the problem of conductivity and strength of the carbon-plastic composite sheet is solved, high conductivity and mechanical strength are achieved, and the conductivity is improved of uniformity.
Patent Information
- Application Number
- CN202410722373.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-01
AI Technical Summary
It is difficult for existing carbon-plastic composite sheets to achieve high conductivity, high strength and high uniformity, and existing processes cannot effectively improve their conductivity uniformity.
By uniformly adhering the carbon powder to the resin fine liquid column in situ, and forming flexible resin fibers by cooling or heating to the glass transition temperature, a fiber network structure is constructed to improve the conductivity and strength of the carbon-plastic composite sheet.
It achieves high electrical conductivity and improved mechanical strength of the carbon-plastic composite sheet, while improving the uniformity of electrical conductivity and ensuring the high strength of the sheet under low resin content.
Smart Images

Figure CN118721804A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of bipolar plates of batteries, and in particular relates to a carbon-plastic composite plate, a preparation method, a preparation device and applications thereof. Background Art
[0002] As a key material in liquid flow and fuel cells, bipolar plates play the role of connecting the positive and negative electrodes of adjacent single cells in series, conducting the internal circuit, supporting the positive and negative electrodes, and blocking the electrolytes or reaction gases on both sides. Therefore, the bipolar plates are required to have high conductivity, excellent conductivity uniformity, good tensile / bending strength, good chemical stability and corrosion resistance. Graphite materials have excellent conductivity and corrosion resistance, but their tensile and compressive properties are poor, and they are easy to break during the battery assembly process. Metal bipolar plates have high mechanical strength and good conductivity, but they are easily corroded by electrolytes in strong acid and strong oxidizing environments. In contrast, carbon-plastic composite plates have both the corrosion resistance of graphite materials and the high strength of metal materials, and are one of the directions to reduce the cost of bipolar plate materials and increase battery life.
[0003] The ratio of carbon to resin content in carbon-plastic composite panels will have an important impact on the strength and conductivity of the panels. The higher the ratio of carbon to resin content, the higher the conductivity, but the strength is significantly reduced; the lower the ratio of carbon to resin content, the higher the strength, but the conductivity is reduced. In addition, the uniformity of the mixing of resin and carbon is closely related to the uniformity of conductivity and strength of carbon-plastic composite panels. Uneven mixing of resin and carbon will cause the same panel to exhibit different conductivity in different areas, reducing the performance and consistency of the battery stack. At present, carbon-plastic composite panels are mainly produced by physical mixing-hot pressing, resin impregnation-hot pressing or spraying-hot pressing. These processes cannot achieve the preparation of high-conductivity, high-strength carbon-plastic composite panels, and the conductivity uniformity of the produced panels is poor.
[0004] Therefore, there is an urgent need to develop a carbon-plastic composite sheet with high conductivity, high strength and high uniformity and a preparation method thereof. Summary of the invention
[0005] In order to solve the problems existing in the prior art, the present invention provides a carbon-plastic composite board, a preparation method, a preparation device and an application thereof. In the present invention, a large amount of carbon material powder is in-situ and evenly adhered to a thin resin liquid column. After adhering to the carbon material powder, the resin liquid column is cooled and solidified / heated to the glass transition temperature to form a flexible resin fiber, and finally a carbon material-resin composite is obtained. In the carbon-plastic composite board of the present invention, the carbon material content is high and evenly dispersed, so that the carbon-plastic composite board has excellent conductivity and uniformity. In the present invention, the resin fibers formed after the liquid-solid phase transition construct a fiber network structure in the board, so that the carbon-plastic composite board can still have a high strength when the resin content is low.
[0006] The present invention provides a method for preparing a carbon-plastic composite plate, the preparation method comprising the following steps:
[0007] (1) Liquid resin is introduced into the inner cavity of a rotating disk with a spray hole, the rotating disk is placed in a mixing chamber, and the rotating disk is rotated, so that the resin is sprayed out from the spray hole in the form of a liquid column and enters the mixing chamber;
[0008] (2) using gas to blow the carbon material powder into the mixing chamber, so that the carbon material powder adheres to the liquid column resin in situ and evenly, and then collects the resin-carbon material mixture;
[0009] (3) hot pressing the resin-carbon material mixture to obtain the carbon-plastic composite plate after cooling.
[0010] In one or more embodiments, in the carbon-plastic composite plate, the content of the resin is 5wt% to 30wt%, and the content of the carbon material powder is 70wt% to 95wt%.
[0011] In one or more embodiments, the resin is a thermoplastic resin that is solid at room temperature. In step (1), the thermoplastic resin is first heated and melted into a liquid in a heating tank at a temperature of T1, and then the liquid is passed into the inner cavity of a turntable with a spray hole through a conveying pipe at a temperature of T1, and the temperature of the mixing chamber is controlled to be T2.
[0012] In one or more embodiments, the thermoplastic resin is selected from one or more of polypropylene, polytetrafluoroethylene, polyethylene, and polyphenylene sulfide.
[0013] In one or more embodiments, T1 is 85°C to 350°C, T2 is 85°C to 350°C, and T2 ≤ T1.
[0014] In one or more embodiments, the resin is a thermosetting resin that is liquid at room temperature. In step (1), the thermosetting resin is passed from a heating tank at room temperature through a conveying pipe at room temperature into the inner cavity of a turntable with a spray hole, and the temperature of the mixing chamber is controlled to be room temperature.
[0015] In one or more embodiments, the thermosetting resin is selected from one or more of epoxy resins, phenolic resins, and polyvinyl esters.
[0016] In one or more embodiments, in step (1), the air in the mixing chamber is first replaced with a protective gas, and then the turntable is rotated, and the protective gas is selected from one or more of nitrogen, argon and carbon dioxide.
[0017] In one or more embodiments, in step (1), the rotation speed of the turntable is 3000 r / min to 30000 r / min.
[0018] In one or more embodiments, in step (1), the spray hole on the rotating disk is a conical through hole, and the outer hole diameter of the spray hole is 0.01 mm to 1 mm.
[0019] In one or more embodiments, in step (1), the diameter of the liquid columnar resin sprayed through the spray hole is less than or equal to the diameter of the spray hole.
[0020] In one or more embodiments, in step (1), the liquid columnar resin sprayed out through the spray hole is a fine liquid columnar resin.
[0021] In one or more embodiments, in step (1), the diameter of the liquid columnar resin ejected through the nozzle hole is ≤1 mm. In one or more embodiments, in step (1), the diameter of the liquid columnar resin ejected through the nozzle hole is 0.01 mm to 1 mm, for example, 0.01 nm, 0.05 mm, 0.15 nm, 0.20 mm, 0.30 nm, 0.40 mm, 0.50 nm, 0.60 mm, 0.70 nm, 0.80 mm, 0.90 nm, 1.00 mm.
[0022] In one or more embodiments, in step (2), after the liquid columnar resin adheres to the carbon material powder, the resin is cooled and solidified or heated to the glass transition temperature to become resin fibers, forming a structure in which the carbon material powder is coated with the resin fibers. In one or more embodiments, the resin fibers are flexible resin fibers. In one or more embodiments, the resin is a thermoplastic resin that is solid at room temperature, and after the liquid columnar resin adheres to the carbon material powder, the resin is cooled and solidified to become resin fibers. In one or more embodiments, the resin is a thermosetting resin that is liquid at room temperature, and after the liquid columnar resin adheres to the carbon material powder, the resin is heated to the glass transition temperature to become resin fibers. Appropriate heating conditions can be selected according to the type of resin.
[0023] In one or more embodiments, in step (2), the gas is selected from one or more of nitrogen, argon and carbon dioxide.
[0024] In one or more embodiments, in step (2), the carbon material powder is selected from one or more of natural graphite, expanded graphite, conductive carbon black and graphene.
[0025] In one or more embodiments, in step (2), the particle size of the carbon material powder is 10 to 200 μm.
[0026] In one or more embodiments, in step (3), the hot pressing molding is continuous roll pressing or mold hot pressing.
[0027] The invention provides a carbon-plastic composite material prepared by the method for preparing the carbon-plastic composite material of the invention.
[0028] The present invention provides a preparation device for implementing the preparation method of the carbon-plastic composite material described in the present invention, the preparation device comprises a first storage tank, a second storage tank, a heating tank, a metering pump, a turntable, a mixing chamber, a collecting tank and a hot pressing molding device; wherein the first storage tank, the heating tank, the metering pump and the turntable are connected in sequence by pipelines, the second storage tank, the mixing chamber and the collecting tank are connected in sequence by pipelines, the turntable is placed inside the mixing chamber, the turntable has an inner cavity, and there are spray holes on the turntable; the first storage tank is used to store resin; the heating tank is used to heat solid resin into liquid; the metering pump is used to feed liquid resin into the turntable; the turntable is used to rotate so that the liquid resin is sprayed out from the spray hole in the form of a liquid column; the second storage tank is used to store carbon material powder and allows gas to blow the carbon material powder into the mixing chamber; the collecting tank is used to collect the resin-carbon material mixture; the hot pressing molding device is used to perform hot pressing molding on the resin-carbon material mixture.
[0029] The present invention provides a bipolar plate prepared by using the carbon-plastic composite material of the present invention.
[0030] The present invention provides a battery comprising the bipolar plate of the present invention.
[0031] In one or more embodiments, the battery is a flow battery or a fuel cell.
[0032] In one or more embodiments, the battery is an all-vanadium flow battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Schematic diagram of a device for preparing a carbon-plastic composite plate in some embodiments of the present invention.
[0034] Figure 2 It is a partially enlarged schematic diagram of a turntable in a device for preparing a carbon-plastic composite board in some embodiments of the present invention.
[0035] In the figure, 1 is a first storage tank, 2 is a second storage tank, 3 is a heating tank, 4 is a metering pump, 5 is a turntable, 6 is a mixing chamber, 7 is a collecting tank, and 11 is a tapered through hole. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the text. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0037] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0038] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0039] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0040] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0041] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope defined by the present invention.
[0042] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0043] In some embodiments, the method for preparing the carbon-plastic composite sheet of the present invention comprises the following steps:
[0044] (1) Liquid resin is introduced into the inner cavity of a rotating disk with a spray hole, the rotating disk is placed in the mixing chamber, and the rotating disk is rotated, so that the resin is sprayed out from the spray hole in the form of a thin liquid column and enters the mixing chamber;
[0045] (2) using gas to blow carbon material powder into the mixing chamber so that the carbon material powder adheres to the thin liquid column-shaped resin to obtain a resin-carbon material mixture;
[0046] (3) hot pressing the resin-carbon material mixture to obtain a carbon-plastic composite sheet after cooling;
[0047] In the carbon-plastic composite board, the resin content can be 5wt% to 30wt%, for example, 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, and the carbon powder content is 70wt% to 95wt%, for example, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt%.
[0048] In the present invention, the resin is a thermoplastic resin that is solid at room temperature. In step (1), the thermoplastic resin can be first heated and melted into a liquid in a heating tank at a temperature of T1, and then introduced into the inner cavity of a rotating disk with a spray hole through a delivery pipe at a temperature of T1, and the temperature of the mixing chamber is controlled to be T2. In the present invention, room temperature refers to 20°C-30°C, for example, 25°C.
[0049] In the present invention, the thermoplastic resin may be one or more selected from polypropylene, polytetrafluoroethylene, polyethylene and polyphenylene sulfide.
[0050] In the present invention, T1 can be 85°C-350°C, for example, 90°C, 110°C, 130°C, 150°C, 170°C, 190°C, 210°C, 230°C, 250°C, 270°C, 290°C, 310°C, 330°C, and 350°C.
[0051] In the present invention, T2 can be 85℃-350℃, for example, 90℃, 110℃, 130℃, 150℃, 170℃, 190℃, 210℃, 230℃, 250℃, 270℃, 290℃, 310℃, 330℃, 350℃.
[0052] In the present invention, T2≤T1. In some embodiments, T2 and T1 are the same temperature.
[0053] In the present invention, the resin is a thermosetting resin that is liquid at room temperature. In step (1), the thermosetting resin can be introduced from a heating tank at room temperature through a delivery pipe at room temperature into the inner cavity of a rotating disk with a spray hole, and the temperature of the mixing chamber is controlled to be room temperature. In some embodiments, the resin is a thermosetting resin that is liquid at 25°C. The thermosetting resin is introduced from a heating tank at 25°C through a delivery pipe at 25°C into the inner cavity of a rotating disk with a spray hole, and the temperature of the mixing chamber is controlled to be 25°C.
[0054] In the present invention, the thermosetting resin may be one or more selected from epoxy resin, phenolic resin and polyvinyl ester.
[0055] In step (1), it is preferred to replace the air in the mixing chamber with a protective gas before rotating the turntable. The protective gas may be one or more selected from nitrogen, argon and carbon dioxide.
[0056] In step (1), the rotation speed of the turntable can be 3000 r / min to 30000 r / min, for example, 3000 r / min, 6000 r / min, 9000 r / min, 12000 r / min, 15000 r / min, 18000 r / min, 21000 r / min, 24000 r / min, 27000 r / min, and 30000 r / min.
[0057] In step (1), the nozzle hole on the rotating disk can be a tapered through hole, and the outer diameter of the nozzle hole can be 0.01 mm to 1 mm, for example, 0.01 nm, 0.05 mm, 0.15 nm, 0.20 mm, 0.30 nm, 0.40 mm, 0.50 nm, 0.60 mm, 0.70 nm, 0.80 mm, 0.90 nm, 1.00 mm. Generally, the inner diameter of the tapered through hole (the side facing the inner cavity of the rotating disk) is larger than the outer diameter.
[0058] In step (1), the diameter of the thin liquid columnar resin sprayed through the spray hole is less than or equal to the diameter of the spray hole. In the embodiment where the spray hole is a tapered through hole, the diameter of the thin liquid columnar resin is less than or equal to the outer hole diameter of the spray hole.
[0059] In step (2), the gas may be one or more selected from nitrogen, argon and carbon dioxide. In some embodiments, the gas used is a high-pressure gas, which may be a high-pressure gas cylinder sold by a common manufacturer.
[0060] In step (2), the carbon material powder may be one or more selected from natural graphite, expanded graphite, conductive carbon black and graphene.
[0061] In step (2), the particle size of the carbon powder can be 10 to 200 μm, for example, 20 μm, 40 μm, 60 μm, 80 μm, 100 μm, 120 μm, 140 μm, 160 μm, 180 μm, or 200 μm.
[0062] In step (3), the hot pressing molding can be continuous roll pressing or mold hot pressing.
[0063] In step (3), the temperature of hot pressing can be 70-300°C, for example, 70°C, 100°C, 130°C, 160°C, 190°C, 220°C, 250°C, 280°C, 300°C.
[0064] In step (3), the pressure of hot pressing can be 5 to 40 MPa, for example, 5 MPa, 10 MPa, 15 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, or 40 MPa.
[0065] The present invention provides a carbon-plastic composite material obtained by the preparation method of the carbon-plastic composite material of the present invention. The carbon-plastic composite plate comprises 5wt% to 30wt% of resin and 70wt% to 95wt% of carbon material. In the present invention, a large amount of carbon material is in situ and evenly adhered to a thin resin liquid column. After adhering to the carbon material, the resin liquid column is slowly cooled and solidified / heated to the glass transition temperature to form a flexible resin fiber, and finally a carbon material-resin composite is obtained. In the carbon-plastic composite plate of the present invention, the carbon material content is high and evenly dispersed, so that the carbon-plastic composite plate has excellent conductivity and uniformity. In the present invention, the resin fibers formed after the liquid-solid phase transition construct a fiber network structure in the plate, so that the carbon-plastic composite plate can still have a high strength when the resin content is low.
[0066] The present invention provides a preparation device for implementing the preparation method of the carbon-plastic composite material of the present invention, the preparation device comprises a first storage tank, a second storage tank, a heating tank, a metering pump, a turntable, a mixing chamber, a collecting tank and a hot pressing molding device; wherein the first storage tank, the heating tank, the metering pump and the turntable are connected in sequence by pipelines, the second storage tank, the mixing chamber and the collecting tank are connected in sequence by pipelines, the turntable is placed inside the mixing chamber, the turntable has an inner cavity, and there are spray holes on the turntable, the spray holes are tapered through holes, and the tapered through holes are used to spray out fibrous polymer resin; the first storage tank is used to store resin; the heating tank is used to heat solid resin into liquid; the metering pump is used to feed liquid resin into the turntable; the turntable is used to rotate so that the liquid resin is sprayed out from the spray hole in a liquid column; the second storage tank is used to store carbon material powder and allow gas to blow the carbon material powder into the mixing chamber; the collecting tank is used to collect the resin-carbon material mixture; the hot pressing molding device is used to perform hot pressing molding on the resin-carbon material mixture.
[0067] In the present invention, the second material storage tank, the mixing chamber and the collecting tank are connected by a pipeline, wherein the second material storage tank and the mixing chamber are connected by a pipeline to form a powdered carbon material conveying channel.
[0068] Compared with the prior art, the present invention has the following beneficial effects:
[0069] In the present invention, the high content of carbon material makes the carbon-plastic composite plate have excellent conductivity; during the preparation process, the carbon material is in situ and evenly adhered to the resin fine liquid column, so that the carbon material has good dispersion uniformity in the plate, and the uniformity of the carbon material performance is improved; the polymer resin in the fibrous form during the preparation process constructs a fiber network structure, so that the carbon-plastic composite plate has higher strength.
[0070] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0071] Equipment Example 1
[0072] This equipment example provides a device for preparing a carbon-plastic composite plate. Figure 1 As shown, the preparation device includes a first storage tank 1, a second storage tank 2, a heating tank 3, a metering pump 4, a turntable 5, a mixing chamber 6 and a collecting tank 7, and the preparation device also includes a hot pressing molding device ( Figure 1 The first storage tank 1, the heating tank 3, the metering pump 4 and the turntable 5 are connected in sequence by pipelines to form a resin delivery channel; the turntable 5 is placed inside the mixing chamber 6. Figure 2 As shown, the turntable 5 has an inner cavity, and there is a spray hole on the turntable 5. The spray hole is a conical through hole 11, and the outer aperture of the spray hole is 0.1 mm. The conical through hole 11 is used to spray out fibrous resin. The second storage tank 2, the mixing chamber 6 and the collecting tank 7 are connected in sequence by pipelines, wherein the second storage tank 2 and the mixing chamber 6 are connected by a pipeline to form a powdered carbon material conveying channel. The first storage tank 1 is used to store resin. The heating tank 3 is used to heat the solid resin into liquid. The metering pump 4 is used to feed the liquid resin into the turntable. The turntable 5 is used to rotate so that the liquid resin is sprayed out from the spray hole in a fibrous shape. The second storage tank 2 is used to store carbon material powder and allow gas to blow the carbon material powder into the mixing chamber 6. The collecting tank 7 is used to collect the resin-carbon material mixture. The hot pressing molding device is used to perform hot pressing molding on the resin-carbon material mixture.
[0073] Example 1
[0074] This embodiment uses the preparation device of Equipment Example 1 to prepare a natural graphite / epoxy resin composite plate according to the following steps:
[0075] (1) placing a liquid epoxy resin at 25° C. in a first storage tank, and introducing nitrogen into the preparation device to replace the air;
[0076] (2) Without heating, keep the heating tank, the pipe connecting the heating tank and the metering pump, the pipe connecting the turntable of the metering pump, the turntable and the mixing chamber at 25°C;
[0077] (3) After the turntable is started and reaches a speed of 15000 r / min, the epoxy resin is pumped into the turntable by a metering pump after passing through a heating tank, so that the epoxy resin is sprayed out in the form of a thin liquid column; at the same time, a natural graphite powder with a particle size of 200 μm in the second storage tank is blown into the mixing chamber using high-pressure nitrogen, so that the natural graphite powder adheres to the thin liquid columnar epoxy resin to obtain a natural graphite / epoxy resin mixture, and the natural graphite / epoxy resin mixture is discharged into a collection tank, and the liquid epoxy resin is heated to the glass transition temperature to become a flexible resin fiber, forming a structure in which the carbon material powder is coated with the resin fiber;
[0078] (4) placing the natural graphite / epoxy resin mixture in the collection tank into a mold, hot pressing at 20 MPa and 100° C. for 20 min, and cooling to obtain a natural graphite / epoxy resin composite sheet. The natural graphite content of the natural graphite / epoxy resin composite sheet is 85 wt %, and the epoxy resin content is 15 wt %.
[0079] Example 2
[0080] This embodiment uses the preparation device of Equipment Example 1 to prepare expanded graphite-conductive carbon black / polypropylene composite sheet according to the following steps:
[0081] (1) placing polypropylene in a solid state at 25° C. in a first storage tank, and introducing nitrogen into the preparation device to replace the air;
[0082] (2) After heating the heating tank, the pipe connecting the heating tank and the metering pump, the pipe connecting the turntable of the metering pump, the turntable and the mixing chamber to 170° C., the polypropylene is transported to the heating tank through the pipe to completely melt the polypropylene into a liquid state;
[0083] (3) After the turntable is started and reaches a speed of 30,000 r / min, polypropylene is pumped into the turntable through a metering pump so that the polypropylene is ejected in a thin liquid column; at the same time, high-pressure nitrogen is used to blow the expanded graphite powder with a particle size of 150 μm and the conductive carbon black powder with a particle size of 50 μm in the second storage tank into the mixing chamber, so that the expanded graphite powder and the conductive carbon black powder adhere to the fine liquid columnar polypropylene to obtain an expanded graphite-conductive carbon black / polypropylene mixture, and the expanded graphite-conductive carbon black / polypropylene mixture is discharged into a collection tank, and the liquid polypropylene is slowly cooled and solidified to become flexible resin fibers, forming a structure in which the carbon material powder is coated with the resin fibers;
[0084] (4) placing the expanded graphite-conductive carbon black / polypropylene mixture in the collection tank into a mold, hot pressing for 15 min at 160° C. and 25 MPa, and cooling to obtain an expanded graphite-conductive carbon black / polypropylene composite sheet. In the expanded graphite-conductive carbon black / polypropylene composite sheet, the content of expanded graphite is 80wt%, the content of conductive carbon black is 5wt%, and the content of polypropylene is 15wt%.
[0085] Example 3
[0086] This embodiment uses the preparation device of Equipment Example 1 to prepare a natural graphite / polypropylene composite sheet according to the following steps:
[0087] (1) placing polypropylene in a solid state at 25° C. in a first storage tank, and introducing nitrogen into the preparation device to replace the air;
[0088] (2) After heating the heating tank, the pipe connecting the heating tank and the metering pump, the pipe connecting the turntable of the metering pump, the turntable and the mixing chamber to 180° C., the polypropylene is transported to the heating tank through the pipe, and the polypropylene is completely melted into a liquid state;
[0089] (3) After the turntable is started and reaches a speed of 3000 r / min, polypropylene is pumped into the turntable through a metering pump so that the polypropylene is sprayed out in the form of a thin liquid column; at the same time, natural graphite powder with a particle size of 150 μm in the second storage tank is blown into the mixing chamber using high-pressure nitrogen, so that the natural graphite powder adheres to the thin liquid columnar polypropylene to obtain a natural graphite / polypropylene mixture, and the natural graphite / polypropylene mixture is discharged into a collection tank, and the liquid polypropylene is slowly cooled and solidified to become a flexible resin fiber, forming a structure in which the carbon material powder is coated with the resin fiber;
[0090] (4) placing the natural graphite / polypropylene mixture in the collection tank into a mold, hot pressing for 15 min at 160° C. and 20 MPa, and cooling to obtain a natural graphite / polypropylene composite sheet. The natural graphite content of the natural graphite / polypropylene composite sheet is 80 wt %, and the polypropylene content is 20 wt %.
[0091] Comparative Example 1
[0092] This comparative example adopts the process of physical mixing of powder materials to prepare the natural graphite / polypropylene composite plate comparison sample:
[0093] After polypropylene powder and natural graphite powder with a particle size of 150 μm were put into a mixer and mixed for 3 hours, the obtained natural graphite / polypropylene mixed powder was put into a mold, and hot-pressed for 15 minutes at 160° C. and 20 MPa, and then cooled to obtain natural graphite / polypropylene composite sheet comparative sample 1. In the natural graphite / polypropylene composite sheet comparative sample 1, the content of natural graphite is 80wt%, and the content of polypropylene is 20wt%.
[0094] Comparative Example 2
[0095] This comparative example prepares a natural graphite / polypropylene composite sheet comparative sample according to the following steps:
[0096] (1) Using the preparation device of Equipment Example 1, solid polypropylene at 25° C. is placed in a first storage tank, and nitrogen is introduced into the preparation device to replace the air;
[0097] (2) After heating the heating tank, the pipe connecting the heating tank and the metering pump, the pipe connecting the turntable of the metering pump, the turntable and the mixing chamber to 180° C., the polypropylene is transported to the heating tank through the pipe, and the polypropylene is completely melted into a liquid state;
[0098] (3) After the turntable is started and reaches a speed of 3000 r / min, polypropylene is pumped into the turntable through a metering pump, so that the polypropylene is sprayed out in the form of a thin liquid column; at the same time, high-pressure nitrogen is blown into the mixing chamber, and the resin fibers formed after the polypropylene liquid column is cooled are discharged into a collection tank;
[0099] (4) The polypropylene fiber in the collection tank and the natural graphite powder with a particle size of 150 μm were placed in a mixer and mixed for 3 hours, and then the obtained natural graphite / polypropylene fiber mixture was placed in a mold, and hot-pressed at 160° C. and 20 MPa for 15 minutes for hot pressing. After cooling, the natural graphite / polypropylene composite plate comparative sample 2 was obtained. In the natural graphite / polypropylene composite plate comparative sample 2, the content of natural graphite is 80wt%, and the content of polypropylene is 20wt%.
[0100] Test Case
[0101] Conductivity test method: Cut a 5cm×5cm sample and use a four-probe low-resistance measuring instrument to measure the volume resistivity values of 9 points around and in the middle of the sample. The test results are averaged; the single board conductivity range is the difference between the maximum and minimum values at the test site.
[0102] Tensile strength test method: Cut a 15cm×1cm sample and stretch it at a speed of 5mm / min using a universal material testing machine. Record the load value when the sample breaks. There should be no less than 5 valid specimens, and the test results should be taken as the average.
[0103] Bending strength test method: Cut a 10cm×1cm sample strip, bend and pressurize it at a speed of 2mm / min using a universal material testing machine, record the load value when the sample breaks, there are no less than 5 valid specimens, and the test results are taken as the average.
[0104] Vertical resistance test method (overall resistance of two electrodes and the plate): Take a sample with a diameter of 5 cm and place it between the two measuring electrodes of the microresistance tester. Apply a pressure of 0.3 MPa on both sides of the measuring electrodes to test the overall resistance value of the two electrodes and the bipolar plate sample. There should be no less than 3 valid sample strips, and the test result should be taken as the average.
[0105] The test results of the electrical conductivity, single plate electrical conductivity difference, tensile strength, flexural strength and vertical resistance of the carbon-plastic composite plates prepared in Examples 1-3 and Comparative Examples 1-2 are shown in Table 1.
[0106] Table 1: The conductivity, tensile strength, bending strength, vertical resistance and single board conductivity of the carbon-plastic composite board of Examples 1-3 and Comparative Examples 1-2 are very different
[0107]
[0108] It can be seen from Table 1 that compared with the natural graphite / polypropylene composite plate prepared by the powder physical mixing process in Comparative Example 1, the natural graphite / polypropylene composite plate prepared by the preparation method of the present invention in Example 3 has higher electrical conductivity, tensile strength, flexural strength and lower vertical resistance. It can be further seen that the carbon-plastic composite plate prepared by the present invention has excellent electrical conductivity and mechanical strength.
[0109] In addition, compared with the method of preparing a composite plate by step-by-step mixing of polypropylene fiber and natural graphite in Comparative Example 2, the plate prepared by in-situ adhesion of carbon material powder to fine liquid columnar resin in Example 3 not only has higher conductivity, but also has a lower conductivity difference, indicating that the carbon-plastic composite plate prepared by the present invention has good conductive uniformity.
Claims
1. A method for preparing a carbon-plastic composite sheet, characterized in that: The preparation method comprises the following steps: (1) Liquid resin is introduced into the inner cavity of a rotating disk with a spray hole, the rotating disk is placed in a mixing chamber, and the rotating disk is rotated, so that the resin is sprayed out from the spray hole in the form of a liquid column and enters the mixing chamber; (2) using gas to blow the carbon material powder into the mixing chamber, so that the carbon material powder adheres to the liquid columnar resin in situ and evenly, and then collects the resin-carbon material mixture; (3) hot pressing the resin-carbon material mixture to obtain the carbon-plastic composite sheet after cooling; In the carbon-plastic composite plate, the content of the resin is 5wt% to 30wt%, and the content of the carbon material powder is 70wt% to 95wt%.
2. The method for preparing the carbon-plastic composite sheet according to claim 1, characterized in that: The resin is a thermoplastic resin that is solid at room temperature. In step (1), the thermoplastic resin is first heated and melted into a liquid in a heating tank at a temperature of T1, and then the liquid is passed into the inner cavity of a turntable with a spray hole through a conveying pipe at a temperature of T1, and the temperature of the mixing chamber is controlled to be T2.
3. The method for preparing the carbon-plastic composite sheet according to claim 2, characterized in that: The thermoplastic resin is selected from one or more of polypropylene, polytetrafluoroethylene, polyethylene and polyphenylene sulfide; and / or T1 is 85°C-350°C, T2 is 85°C-350°C, and T2≤T1.
4. The method for preparing the carbon-plastic composite sheet according to claim 1, characterized in that: The resin is a thermosetting resin that is liquid at room temperature. In step (1), the thermosetting resin is passed from a heating tank at room temperature through a conveying pipe at room temperature into the inner cavity of a turntable with a spray hole, and the temperature of the mixing chamber is controlled to be room temperature.
5. The method for preparing the carbon-plastic composite sheet according to claim 4, characterized in that: The thermosetting resin is selected from one or more of epoxy resin, phenolic resin and polyvinyl ester.
6. The method for preparing the carbon-plastic composite sheet according to claim 1, characterized in that: The method has one or more of the following features: In step (1), the air in the mixing chamber is first replaced with a protective gas, and then the turntable is rotated, wherein the protective gas is selected from one or more of nitrogen, argon and carbon dioxide; In step (1), the rotation speed of the turntable is 3000 r / min to 30000 r / min; In step (1), the spray hole on the rotating disk is a conical through hole, and the outer diameter of the spray hole is 0.01 mm to 1 mm; In step (1), the diameter of the liquid columnar resin sprayed through the spray hole is less than or equal to the diameter of the spray hole; In step (2), after the liquid columnar resin adheres to the carbon material powder, the resin is cooled and solidified or heated to the glass transition temperature to become resin fibers, forming a structure in which the carbon material powder is coated with the resin fibers; In step (2), the gas is selected from one or more of nitrogen, argon and carbon dioxide; In step (2), the carbon material powder is selected from one or more of natural graphite, expanded graphite, conductive carbon black and graphene; In step (2), the particle size of the carbon powder is 10 to 200 μm; In step (3), the hot pressing molding is continuous roller pressing or mold hot pressing.
7. A carbon-plastic composite material obtained by the method for preparing a carbon-plastic composite material according to any one of claims 1 to 6.
8. A preparation device for implementing the preparation method of the carbon-plastic composite material according to any one of claims 1 to 6, characterized in that: The preparation device comprises a first material storage tank, a second material storage tank, a heating tank, a metering pump, a turntable, a mixing chamber, a collecting tank and a hot pressing molding device; Wherein, the first material storage tank, the heating tank, the metering pump and the turntable are connected in sequence by pipelines, the second material storage tank, the mixing chamber and the collecting tank are connected in sequence by pipelines, the turntable is placed inside the mixing chamber, the turntable has an inner cavity, and there are spray holes on the turntable; The first storage tank is used to store resin; The heating tank is used to heat the solid resin into liquid; The metering pump is used to deliver liquid resin into the turntable; The rotating disk is used to rotate so that the liquid resin is sprayed out from the spray hole in the form of a liquid column; The second storage tank is used to store carbon material powder and allows gas to blow the carbon material powder into the mixing chamber; The collecting tank is used to collect the resin-carbon material mixture; The hot pressing molding device is used for hot pressing the resin-carbon material mixture.
9. A bipolar plate prepared using the carbon-plastic composite material according to claim 7.
10. A battery, characterized in that: The battery comprises the bipolar plate of claim 9.