Corrosion-resistant and weather-resistant heat insulation plate and preparation process thereof

By forming a paint layer, an adhesive layer, an alloy aluminum plate and a modified PET layer on a galvanized plate, and performing a hot-pressing composite process, the deficiencies in weather resistance and cost of existing materials are solved, and a corrosion-resistant, corrosion-resistant Anti-corrosion and weather-resistant insulation panels with high heat and strength extend service life and improve thermal insulation effect.

CN118721889APending Publication Date: 2024-10-01FUJIAN XINHONGHUA MASCH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410749993.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing materials used for outdoor ceilings such as galvanized sheets, color steel sheets and stainless steel sheets have shortcomings in terms of weather resistance and cost. In particular, galvanized sheets have a short service life and low strength, and color steel sheets have a longer service life but higher costs. There is a lack of a composite panel with relatively low cost and good weather resistance.

Method used

The galvanized sheet is used as the substrate, and the paint layer, the first adhesive layer, the alloy aluminum plate, the second adhesive layer and the modified PET layer are sequentially coated on the surface, and the hot pressing composite process is performed to form an anti-corrosion weather-resistant heat insulation board, which improves the Its corrosion resistance, heat resistance and thermal insulation properties.

Benefits of technology

The prepared heat insulation board has excellent corrosion resistance, heat resistance, high strength, fire protection grade A2, a service life of up to 8-10 years, a temperature resistance of up to 120°C, and long-term use between minus 40°C and 100°C. , and has good thermal insulation effect and weather resistance, extending the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118721889A_ABST
    Figure CN118721889A_ABST
Patent Text Reader

Abstract

An anti-corrosion weather-proof heat insulation plate comprises a base plate and two composite plates compounded on the top face and the bottom face of the base plate respectively, and each composite plate comprises a paint layer, a first adhesive layer, an alloy aluminum plate, a second adhesive layer and a modified PET layer which are sequentially arranged from inside to outside with the base plate as the main part; the heat insulation plate prepared by the invention has the advantages of excellent corrosion resistance, heat resistance, high strength, A2 fireproof grade and the like, can be pressed into tiles on site, and is more suitable for roofs and wall panels of outdoor unit industry factories; compared with a resin tile, the temperature resistance can reach 120 DEG C, the preparation length is not limited, the types are diversified, the wave crests of the hidden buttons 760 and 820 are high, and water leakage is not prone to occurring.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heat insulation board preparation, and specifically relates to an anti-corrosion and weather-resistant heat insulation board and a preparation process thereof. Background Art

[0002] At present, the materials used for window awnings or outdoor ceilings are mainly the following: one is galvanized sheet, which is characterized by low price but short service life, generally only 3-4 years, and low strength, and is often blown down and torn in strong winds; the second is color steel plate, which has a longer service life than galvanized sheet, generally 6-8 years, and higher strength; the third is stainless steel plate, which has good service life and strength, but a higher price; therefore, there is an urgent need for a composite plate for outdoor use with relatively low cost and good weather resistance. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an anti-corrosion and weather-resistant heat-insulating board and a preparation process thereof.

[0004] The present invention adopts the following technical solution:

[0005] An anti-corrosion and weather-resistant heat-insulating board comprises a substrate and two composite boards respectively composited on the top and bottom surfaces of the substrate, wherein the composite board comprises a paint layer, a first adhesive layer, an alloy aluminum plate, a second adhesive layer and a modified PET layer sequentially arranged from the inside to the outside with the substrate as the main component.

[0006] The first adhesive layer comprises the following raw materials in parts by weight:

[0007]

[0008]

[0009] Furthermore, the second adhesive layer comprises the following raw materials in parts by weight:

[0010] Further, the modified PET layer is prepared from the following raw materials in parts by weight:

[0011] Furthermore, the substrate is a galvanized sheet.

[0012] A preparation process of an anticorrosive and weather-resistant heat-insulating board specifically comprises the following steps:

[0013] Step 1: coating the top and bottom surfaces of the substrate with paint slurry, drying and curing to form a paint layer;

[0014] Step 2, stacking the first adhesive layer and the alloy aluminum plate outward on the two formed paint layers in sequence, sending them into a hot pressing device for hot pressing and laminating, and cooling under pressure to laminate the alloy aluminum plate on the paint layer;

[0015] Step three, stacking the second adhesive layer and the modified PET film on the two alloy aluminum plates in turn, sending them into a hot pressing device for secondary hot pressing and compounding, and cooling under pressure to form a modified PET layer on the alloy aluminum plates respectively to obtain the anti-corrosion and weather-resistant insulation board.

[0016] Furthermore, the one-time hot pressing composite specifically includes: sending the substrate superimposed with the first adhesive layer and the alloy aluminum plate into the hot pressing equipment, first pre-pressing at a pressure of 75MPa for 45s at room temperature, then gradually heating to 135°C at a rate of 2°C / min, and then increasing the pressure to 130MPa and maintaining for 30s; then turning off the heating device, maintaining pressure and cooling to composite the alloy aluminum plate on the paint layer.

[0017] Furthermore, the secondary hot pressing composite specifically includes: sending the substrate superimposed with the second adhesive layer and the modified PET film into the hot pressing equipment, first pre-pressing at a pressure of 40MPa for 30s at room temperature, then gradually heating to 120°C at a rate of 1.5°C / min, and then increasing the pressure to 95MPa and maintaining for 40s; then turning off the heating device, maintaining pressure and cooling, to form a modified PET layer on the alloy aluminum plate.

[0018] Furthermore, the preparation method of the modified PET film is as follows:

[0019] Step 1, add 100 parts of polyethylene terephthalate, 20-30 parts of butylphenol formaldehyde resin, and 6-8 parts of terpene resin into a high-speed mixer, and mix and stir for 20 minutes;

[0020] Step 2: add the premix obtained in step 1 and 2-3 parts of ethyl p-hydroxybenzoate, 1-2 parts of antioxidant 1010, and 0.5-0.6 parts of antioxidant BH into a twin-screw extruder for extrusion granulation to obtain PET masterbatch, and then extrude and cast the mixture into a film through an extrusion casting machine to obtain the modified PET film.

[0021] Furthermore, the temperature of each section of the twin-screw extruder is 250-280°C, and the extrusion temperature of the extrusion casting machine is 270-280°C.

[0022] It can be seen from the above description of the present invention that, compared with the prior art, the present invention has the following beneficial effects:

[0023] First, the heat insulation board prepared by the present application has the advantages of excellent corrosion resistance, heat resistance, high strength, and fireproof grade A2. It can be pressed on site and is more suitable for outdoor industrial factory roofs and wall panels. Compared with resin tiles, the temperature resistance can reach 120°C, and there is no limit on the preparation length. The version is diverse, the hidden buckle 760 and hidden buckle 820 have higher peaks and are not easy to leak. Among them, the structure of the heat insulation board is specifically defined, and a modified PET layer is set on its surface, which is acid-resistant, alkali-resistant and has super strong gas and liquid barrier, so that the outdoor aging of the heat insulation board can reach 8-10 years, extending the service life of the heat insulation board. At the same time, it has good temperature resistance, so that the heat insulation board can be used for a long time between minus 40°C and 100°C; greatly improve the weather resistance of the heat insulation board;

[0024] Second, adding an alloy aluminum plate on the substrate can reflect 85% of the sunlight, reduce the temperature of the board surface, and achieve a good heat insulation effect; and when the alloy aluminum comes into contact with the outside air, a dense protective layer will be generated, which improves the corrosion resistance of the insulation board and extends the service life of the product. Among them, under the same ambient temperature, the board surface temperature of the insulation board prepared in this application is 15-25°C lower than that of the color-coated board, and the actual indoor temperature of the steel structure workshop is 4-6°C lower than that of the color-coated board;

[0025] Third, the raw material composition of the first adhesive layer is specifically limited, with phenolic resin as the main raw material, ethylene-methacrolein copolymer and maleic rosin resin are added to adjust the viscosity of the first adhesive layer to improve the bonding force between the paint layer and the alloy aluminum plate; at the same time, polyoxyethylene sorbitan monopalmitate is introduced to cooperate with the subsequent hot pressing process, so that the adhesive in the hot pressing process can penetrate into the paint layer, improve the adhesion of the first adhesive layer to the paint layer, and thus ensure the stability of the composite between the substrate and the alloy aluminum plate;

[0026] Fourth, the raw material composition of the second adhesive layer is specifically limited, with bisphenol A epoxy resin as the main raw material, and end-carboxyl liquid nitrile rubber is added to match other raw materials, so that the second adhesive layer has good bonding strength, and the bonding force between the alloy aluminum plate and the modified PET is improved; at the same time, polyethersulfone is introduced to match other raw materials to ensure the size of the second adhesive layer after pressure-maintaining cooling, solve the problem of easy shrinkage during the curing of bisphenol A epoxy resin, and effectively improve the product yield;

[0027] Fifth, butylphenol formaldehyde resin and ethyl paraben are introduced to cooperate with polyethylene terephthalate to improve the corrosion resistance of the prepared insulation board. At the same time, terpene resin is introduced to increase the compatibility and adhesion between the raw materials. Antioxidant 1010 and antioxidant BHT can be used to improve the anti-aging performance of the modified PET film. The UV blocking rate is as high as 99%. The UV accelerated weathering test is more than 5500h, which is equivalent to 8-10 years of outdoor use, greatly improving the service life of the insulation board.

[0028] Sixth, the processes of primary hot pressing and secondary hot pressing are specifically defined. First, pre-press at room temperature to eliminate as much as possible the gaps between the layers when they are stacked. When the temperature is gradually increased, the adhesive layer gradually melts from the outside to the inside, allowing the adhesive layer to penetrate into the paint layer or the modified PET layer, thereby increasing the bonding strength between the layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the structure of the heat insulation board;

[0030] In the figure, 1-substrate, 2-composite board, 21-paint layer, 22-first adhesive layer, 23-alloy aluminum plate, 24-second adhesive layer, 25-modified PET layer. DETAILED DESCRIPTION

[0031] The present invention is further described below through specific implementation modes.

[0032] A corrosion-resistant and weather-resistant heat-insulating board comprises a substrate 1 and two composite boards 2 respectively composited on the top and bottom surfaces of the substrate 1. Specifically, the composite board 2 comprises a paint layer 21, a first adhesive layer 22, an alloy aluminum plate 23, a second adhesive layer 24 and a modified PET layer 25 which are sequentially arranged from the inside to the outside with the substrate 1 as the main body; further, the substrate 21 is a galvanized plate.

[0033] The first adhesive layer includes the following raw materials in parts by weight:

[0034]

[0035]

[0036] The second adhesive layer includes the following raw materials in parts by weight:

[0037] The modified PET layer is prepared from the following raw materials in parts by weight:

[0038] Specifically, the preparation method of the modified PET film is as follows:

[0039] Step 1, adding required weight portions of polyethylene terephthalate, butylphenol formaldehyde resin and terpene resin into a high-speed mixer, and mixing and stirring for 20 minutes;

[0040] Step 2, adding the premix obtained in step 1 and ethyl paraben, antioxidant 1010, and antioxidant BH into a twin-screw extruder for extrusion granulation to obtain PET masterbatch, and then passing through an extrusion casting machine for extrusion casting to obtain the modified PET film, wherein the temperature of each section of the twin-screw extruder is 250-280°C, and the extrusion temperature of the extrusion casting machine is 270-280°C.

[0041] A preparation process of an anticorrosive and weather-resistant heat-insulating board specifically comprises the following steps:

[0042] Step 1: coating the paint slurry on the top and bottom surfaces of the substrate respectively, and drying and curing at 65° C. to form a paint layer;

[0043] Step 2: stack the first adhesive layer and the alloy aluminum plate outward on the two paint layers formed in sequence, send them into a hot pressing device, first pre-press them at room temperature at a pressure of 75 MPa for 45 seconds, then gradually heat them to 135°C at a rate of 2°C / min, and then increase the pressure to 130 MPa and maintain it for 30 seconds; then turn off the heating device, cool them under pressure, and laminate the alloy aluminum plate on the paint layer;

[0044] Step three, respectively stacking the second adhesive layer and the modified PET film on the two alloy aluminum plates in turn, sending them into a hot pressing device, first pre-pressing them at room temperature at a pressure of 40MPa for 30s, then gradually heating them to 120°C at a rate of 1.5°C / min, and then increasing the pressure to 95MPa and maintaining it for 40s; then turning off the heating device, maintaining the pressure and cooling, to form a modified PET layer on the alloy aluminum plate; and obtaining the anti-corrosion and weather-resistant insulation board.

[0045] Example 1

[0046] A corrosion-resistant and weather-resistant heat-insulating board comprises a substrate 1 and two composite boards 2 respectively composited on the top and bottom surfaces of the substrate 1. Specifically, the composite board 2 comprises a paint layer 21, a first adhesive layer 22, an alloy aluminum plate 23, a second adhesive layer 24 and a modified PET layer 25 which are sequentially arranged from the inside to the outside with the substrate 1 as the main body; further, the substrate 21 is a galvanized plate.

[0047] The first adhesive layer includes the following raw materials in parts by weight:

[0048] The second adhesive layer includes the following raw materials in parts by weight:

[0049]

[0050] The modified PET layer is prepared from the following raw materials in parts by weight:

[0051]

[0052]

[0053] Process test: The prepared insulation board was immersed in 5% sulfuric acid for 120 hours, and there was no obvious change on the board surface; after the salt spray test for 1000 hours, there was no obvious change on the board surface; this shows that the insulation board prepared in this application has excellent corrosion resistance and weather resistance.

[0054] Example 2

[0055] A corrosion-resistant and weather-resistant heat-insulating board comprises a substrate 1 and two composite boards 2 respectively composited on the top and bottom surfaces of the substrate 1. Specifically, the composite board 2 comprises a paint layer 21, a first adhesive layer 22, an alloy aluminum plate 23, a second adhesive layer 24 and a modified PET layer 25 which are sequentially arranged from the inside to the outside with the substrate 1 as the main body; further, the substrate 21 is a galvanized plate.

[0056] The first adhesive layer includes the following raw materials in parts by weight:

[0057]

[0058]

[0059] The second adhesive layer includes the following raw materials in parts by weight:

[0060]

[0061] The modified PET layer is prepared from the following raw materials in parts by weight:

[0062]

[0063] Process test: The prepared insulation board was immersed in 5% sulfuric acid for 120 hours, and there was no obvious change on the board surface; after the salt spray test for 1000 hours, there was no obvious change on the board surface; this shows that the insulation board prepared in this application has excellent corrosion resistance and weather resistance.

[0064] Example 3

[0065] A corrosion-resistant and weather-resistant heat-insulating board comprises a substrate 1 and two composite boards 2 respectively composited on the top and bottom surfaces of the substrate 1. Specifically, the composite board 2 comprises a paint layer 21, a first adhesive layer 22, an alloy aluminum plate 23, a second adhesive layer 24 and a modified PET layer 25 which are sequentially arranged from the inside to the outside with the substrate 1 as the main body; further, the substrate 21 is a galvanized plate.

[0066] The first adhesive layer includes the following raw materials in parts by weight:

[0067]

[0068] The second adhesive layer includes the following raw materials in parts by weight:

[0069]

[0070]

[0071] The modified PET layer is prepared from the following raw materials in parts by weight:

[0072]

[0073] Process test: The prepared insulation board was immersed in 5% sulfuric acid for 120 hours, and there was no obvious change on the board surface; after the salt spray test for 1000 hours, there was no obvious change on the board surface; this shows that the insulation board prepared in this application has excellent corrosion resistance and weather resistance.

[0074] The heat insulation board prepared in Example 3 was compared with other products, and the specific results are as follows:

[0075] First, the comparative advantages of the insulation board prepared in this application and the resin tile: Compared with the resin tile, the insulation board prepared in this application has a higher temperature resistance, which can reach 120°C. The fire protection level reaches A2 level. It can be pressed on site, with no length limit and various board types. The hidden buckle 760 and hidden buckle 820 have higher peaks and are not easy to leak.

[0076] Second, the comparative advantages of the heat insulation board prepared by the present application over PVC: the heat insulation board prepared by the present application is heat-resistant, sun-resistant, high-strength, the outer layer of PET outdoor aging can reach 8-10 years, can be pressed on site, and the length is not limited. It is more suitable for outdoor, industrial factory roofs and wall panels.

[0077] Third, the comparative advantages of the insulation board prepared in the present application and the fiberglass tiles: the insulation board prepared in the present application can be 60-70 meters in length, the purlin interval can be 1 meter, the nail holes are not easy to rust, and it also has a heat-insulating effect.

[0078] Fourth, the comparative advantages of the insulation board prepared in this application over cement tiles: the product has a bright and beautiful appearance and is also corrosion-resistant, durable, quick to install, not prone to water leakage, and has no length limit.

[0079] Fifth, the comparative advantages of the insulation board prepared by the present application over aluminum, magnesium and manganese are: corrosion resistance, heat resistance, sunlight resistance, high strength, good thermal insulation effect, fire protection grade A2, the outermost layer of PET is acid-resistant, alkali-resistant, and has super strong barrier to gases and liquids. The outer layer of PET can be aged outdoors for 8-10 years, can be pressed on site, and has no length restrictions; it is more suitable for outdoor and industrial factory roofs and wall panels.

[0080] In summary, the heat insulation board prepared in this application has the advantages of excellent corrosion resistance, heat resistance, high strength, fireproof grade A2, etc. It can be pressed on site and is more suitable for outdoor industrial factory roofs and wall panels; compared with resin tiles, the temperature resistance can reach 120°C, and there is no limit on the preparation length, the version is diverse, the hidden button 760 and the hidden button 820 have higher peaks, and are not easy to leak; among them, the structure of the heat insulation board is specifically limited, and a modified PET layer is set on its surface, which is acid-resistant, alkali-resistant and has super strong gas and liquid barrier, so that the heat insulation board can be aged outdoors for 8-10 years, extending the service life of the heat insulation board The invention has the advantages of high temperature resistance, long life, good temperature resistance, so that the insulation board can be used for a long time between -40℃ and 100℃; greatly improves the weather resistance of the insulation board; adds an alloy aluminum plate on the substrate, which can reflect 85% of the sunlight, reduce the board surface temperature, and play a good insulation effect; and when the alloy aluminum contacts the outside air, a dense protective layer will be generated, which improves the corrosion resistance of the insulation board and extends the service life of the product. Among them, under the same ambient temperature, the board surface temperature of the insulation board prepared in this application is 15-25℃ lower than that of the color-coated board, and the actual indoor temperature of the steel structure workshop is 4-6℃ lower than that of the color-coated board.

[0081] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of implementation of the present invention. That is, equivalent changes and modifications made according to the application scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. An anti-corrosion and weather-resistant insulation board, Features: It comprises a substrate and two composite plates respectively composited on the top and bottom surfaces of the substrate, wherein the composite plate comprises a paint layer, a first adhesive layer, an alloy aluminum plate, a second adhesive layer and a modified PET layer sequentially arranged from the inside to the outside with the substrate as the main body. The first adhesive layer comprises the following raw materials in parts by weight:

2. The anti-corrosion and weather-resistant insulation board according to claim 1, Features: The second adhesive layer comprises the following raw materials in parts by weight:

3. The anti-corrosion and weather-resistant heat-insulating board according to claim 1, Features: The modified PET layer is prepared from the following raw materials in parts by weight:

4. The anti-corrosion and weather-resistant heat-insulating board according to claim 1, Features: The substrate is a galvanized sheet.

5. The preparation process of the anticorrosion and weather-resistant heat insulation board according to claim 1, Features: The specific steps include: Step 1: coating the top and bottom surfaces of the substrate with paint slurry, drying and curing to form a paint layer; Step 2, stacking the first adhesive layer and the alloy aluminum plate outward on the two formed paint layers in sequence, sending them into a hot pressing device for hot pressing and laminating, and cooling under pressure to laminate the alloy aluminum plate on the paint layer; Step three, stacking the second adhesive layer and the modified PET film on the two alloy aluminum plates in turn, sending them into a hot pressing device for secondary hot pressing and compounding, and cooling under pressure to form a modified PET layer on the alloy aluminum plates respectively to obtain the anti-corrosion and weather-resistant insulation board.

6. A process for preparing an anticorrosive and weather-resistant heat-insulating board according to claim 5, Features: The one-time hot pressing composite specifically includes: sending the substrate superimposed with the first adhesive layer and the alloy aluminum plate into the hot pressing equipment, first pre-pressing at a pressure of 75MPa for 45s at room temperature, then gradually heating to 135°C at a rate of 2°C / min, and then increasing the pressure to 130MPa and maintaining for 30s; then turning off the heating device, maintaining pressure and cooling to composite the alloy aluminum plate on the paint layer.

7. The preparation process of the anticorrosion and weather-resistant heat insulation board according to claim 5, Features: The secondary hot pressing composite specifically includes: sending the substrate superimposed with the second adhesive layer and the modified PET film into the hot pressing equipment, first pre-pressing at a pressure of 40MPa for 30s at room temperature, then gradually heating to 120°C at a rate of 1.5°C / min, and then increasing the pressure to 95MPa and maintaining for 40s; then turning off the heating device, maintaining pressure and cooling, to form a modified PET layer on the alloy aluminum plate.

8. The process for preparing the anticorrosion and weather-resistant heat-insulating board according to claim 5, Features: The preparation method of the modified PET film is specifically as follows: Step 1, add 100 parts of polyethylene terephthalate, 20-30 parts of butylphenol formaldehyde resin, and 6-8 parts of terpene resin into a high-speed mixer, and mix and stir for 20 minutes; Step 2: add the premix obtained in step 1 and 2-3 parts of ethyl p-hydroxybenzoate, 1-2 parts of antioxidant 1010, and 0.5-0.6 parts of antioxidant BH into a twin-screw extruder for extrusion granulation to obtain PET masterbatch, and then extrude and cast the mixture into a film through an extrusion casting machine to obtain the modified PET film.

9. The process for preparing the anticorrosion and weather-resistant heat-insulating board according to claim 5, Features: The temperature of each section of the twin-screw extruder is 250-280°C, and the extrusion temperature of the extrusion casting machine is 270-280°C.

Citation Information

Patent Citations

  • Film for illuminated signboard

    CN1124203A

  • Resistance reducing agent with self-emulsifying and paraffin removing and inhibiting functions and preparation method thereof

    CN115011318A

  • Elastic packing film

    CN1185402A

  • Novel heat -insulating tile

    CN205000559U

  • Corrosion-resistant and heat-insulating aluminum steel plate

    CN208867659U