Modified cellulose bacteriostatic agent as well as preparation method and application thereof
By introducing carboxyl groups and phenolic hydroxyl groups into the cellulose main chain, carboxymethyl cellulose grafted with gallic acid was prepared, which solved the problem of poor biological pollution inhibition in the existing technology and achieved effective control of E. coli and golden yellow. Effective inhibition of Staphylococcus aureus and anti-scaling effect of inorganic scale, suitable for a variety of water treatment systems.
Patent Information
- Application Number
- CN202410656303.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-10-01
AI Technical Summary
Existing modified cellulose scale inhibitors are difficult to effectively inhibit biological pollution in circulating water or desalination systems, and their inhibitory effects on Escherichia coli and Staphylococcus aureus are particularly poor.
By introducing carboxyl groups and phenolic hydroxyl groups into the cellulose main chain, carboxymethyl cellulose grafted with gallic acid is prepared as a modified cellulose bacteriostatic agent, and its free radical grafting reaction is used to prepare products with bacteriostatic effects.
This modified cellulose bacteriostatic agent can significantly inhibit the growth of Escherichia coli and Staphylococcus aureus, reduce the risk of biological contamination, and has a strong chelating effect in the water treatment process, inhibiting the formation of inorganic scale, and is suitable for reverse osmosis systems and circulating cooling water system.
Smart Images

Figure CN118725147A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water treatment agents, and in particular to a modified cellulose antibacterial agent and a preparation method and application thereof. Background Art
[0002] As people's environmental awareness gradually increases, more and more researchers are focusing on green scale inhibitors. Since cellulose is a natural polymer compound with abundant sources and wide distribution, and its sugar ring contains abundant active hydroxyl groups, modifying cellulose to obtain modified cellulose that can inhibit scale formation has become a research hotspot.
[0003] At present, this type of scale inhibitor has a strong inhibitory effect on inorganic scale, but it is difficult to avoid biological contamination in circulating water or desalination systems. However, the existing modified cellulose scale inhibitor cannot exert a good inhibitory effect on it.
[0004] To this end, the present invention is proposed. Summary of the invention
[0005] The main purpose of the present invention is to provide a modified cellulose antibacterial agent and a preparation method and application thereof. The modified cellulose antibacterial agent in the present invention can effectively inhibit the growth of Escherichia coli and Staphylococcus aureus and reduce biological contamination in the water treatment process.
[0006] In order to achieve the above objectives, the present invention provides the following technical solutions.
[0007] The first aspect of the present invention provides a modified cellulose antibacterial agent, which is carboxymethyl cellulose grafted with gallic acid. The carboxymethyl cellulose grafted with gallic acid has carboxymethyl cellulose as the main chain, and the carboxyl group in the gallic acid molecule reacts with the hydroxyl group in the carboxymethyl cellulose to be grafted onto the main chain.
[0008] In an embodiment of the present invention, the mass proportion of the carboxymethyl group in the carboxymethyl cellulose grafted gallic acid is 10-40%.
[0009] In an embodiment of the present invention, the gallic acid accounts for 10-15% of the mass of the carboxymethyl cellulose grafted with gallic acid.
[0010] The second aspect of the present invention provides a method for preparing the modified cellulose antibacterial agent according to the first aspect of the present invention, comprising the following steps:
[0011] dissolving carboxymethyl cellulose and gallic acid in water to obtain an aqueous solution;
[0012] After nitrogen is introduced into the aqueous solution, a hydrogen peroxide solution is added to obtain the carboxymethyl cellulose grafted with gallic acid through free radical grafting.
[0013] In an embodiment of the present invention, ascorbic acid is also added into the aqueous solution.
[0014] In an embodiment of the present invention, the mass ratio of the ascorbic acid to the gallic acid is (0.15-0.4):1.
[0015] In an embodiment of the present invention, the mass ratio of the gallic acid to the carboxymethyl cellulose is (0.5-2):1.
[0016] In an embodiment of the present invention, the reaction temperature of the free radical grafting is 70-85° C., and the time is 0.5-6 hours.
[0017] In an embodiment of the present invention, the hydrogen peroxide solution is a hydrogen peroxide solution with a mass fraction of 30%.
[0018] In an embodiment of the present invention, the volume ratio of the added amount of the hydrogen peroxide solution to the carboxymethyl cellulose solution is 5-10%.
[0019] In an embodiment of the present invention, the carboxymethyl cellulose is prepared by etherifying cellulose and chloroacetic acid.
[0020] In an embodiment of the present invention, the mass ratio of the chloroacetic acid to the cellulose is (0.5-2):1.
[0021] In an embodiment of the present invention, the degree of substitution of carboxyl groups in the carboxymethyl cellulose is 0.45 to 1.55.
[0022] The second aspect of the present invention provides a use of the modified cellulose antibacterial agent described in the first aspect of the present invention or the modified cellulose antibacterial agent prepared by the preparation method described in the first aspect of the present invention in inhibiting the growth of Escherichia coli and Staphylococcus aureus.
[0023] Compared with the prior art, the present invention achieves the following technical effects:
[0024] 1. The modified cellulose antibacterial agent of the present invention can inhibit the growth of microorganisms, thereby reducing the risk of biological contamination and improving the efficiency of water treatment operation. It is suitable for processes such as reverse osmosis systems and circulating cooling water systems, and the implementation method is simple and the effect is significant.
[0025] 2. The modified cellulose antibacterial agent in the present invention has the advantages of being biodegradable and green and environmentally friendly, which is reflected in the fact that the raw materials cellulose and gallic acid used are both derived from plants and are non-toxic and free of secondary pollution.
[0026] 3. The modified cellulose antibacterial agent of the present invention introduces a phenolic hydroxyl group that can inhibit biological activity into the molecular chain, which can effectively alleviate biological pollution. In addition, in addition to the hydroxyl active group, a carboxyl group is also added, which can react with Ca in wastewater. 2 + Mg 2+ Cationic ions have strong chelating effects and can be used as water treatment agents to inhibit the formation of inorganic scale during water treatment.
[0027] 4. The preparation method provided by the present invention is simple to operate and has a short synthesis time. The main raw materials used are natural polymer materials with abundant sources, which are low in cost and suitable for industrial large-scale production. It is an economical and efficient preparation method.
[0028] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only used for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. In the accompanying drawings:
[0030] Figure 1 The infrared spectra of gallic acid, carboxymethyl cellulose and carboxymethyl cellulose grafted with gallic acid prepared in the examples;
[0031] Figure 2 The graphs show the inhibitory effects of gallic acid, carboxymethyl cellulose prepared in the examples, and carboxymethyl cellulose grafted with gallic acid on the growth of Escherichia coli in the absence of antibacterial agent;
[0032] Figure 3 The graphs show the inhibitory effects of gallic acid, carboxymethyl cellulose prepared in the examples, and carboxymethyl cellulose grafted with gallic acid on the growth of Staphylococcus aureus in the absence of antibacterial agent;
[0033] Figure 4 This is a comparison chart of the inhibitory effects of carboxymethyl cellulose grafted with gallic acid (1) prepared in Example 1 and carboxymethyl cellulose grafted with protocatechuic acid on the growth of Escherichia coli and Staphylococcus aureus; wherein, Figure 4 (a)- Figure 4 (b) shows the effect of Escherichia coli. Figure 4 (c)- Figure 4 (d) shows the effect of Staphylococcus aureus;
[0034] Figure 5This is a diagram showing the scale inhibition efficiency of carboxymethyl cellulose and carboxymethyl cellulose grafted with gallic acid on calcium sulfate prepared in the example under a static scale inhibition experiment;
[0035] Figure 6 This is a diagram showing the effect of carboxymethyl cellulose and carboxymethyl cellulose grafted with gallic acid prepared in the example on the morphology of calcium sulfate scale in a static scale inhibition experiment;
[0036] Figure 7 This is a graph showing the dispersion performance of carboxymethyl cellulose and carboxymethyl cellulose grafted with gallic acid prepared in the example under the iron oxide dispersion experiment. DETAILED DESCRIPTION
[0037] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, descriptions of known structures and technologies are omitted to avoid unnecessary confusion of the concept of the present invention.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the terms "including" and "having" in the specification and claims of the present invention and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0039] In the description of the embodiments of the present invention, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present invention, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0040] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0041] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0042] In the description of the embodiments of the present invention, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0043] The molecular structure of cellulose is mainly a linear polymer composed of β-glucosidic bonds and contains multiple hydroxyl groups. It can be modified by etherification, graft copolymerization and other methods to introduce new functional groups into the cellulose molecules or adjust their chain structures, thereby changing the natural properties of cellulose and improving its application performance. This is the direction of development of water treatment agents based on cellulose in the field of water treatment.
[0044] By introducing carboxyl groups into cellulose, its scale inhibition performance can be significantly improved, but this type of modified cellulose only has a certain inhibitory effect on inorganic scale pollution, but has poor performance in inhibiting biological pollution.
[0045] In order to alleviate biological contamination in cooling water or desalination systems, the present invention discloses a modified cellulose antibacterial agent and a preparation method thereof. By introducing carboxyl groups and phenolic hydroxyl groups on the cellulose main chain, the prepared modified cellulose antibacterial agent can effectively inhibit biological contamination, thereby broadening the application performance and application range of the modified cellulose.
[0046] The first aspect of the present invention provides a modified cellulose antibacterial agent, which is carboxymethyl cellulose grafted with gallic acid. The carboxymethyl cellulose grafted with gallic acid is a straight-chain structure. The carboxymethyl cellulose grafted with gallic acid has carboxymethyl cellulose as the main chain. The carboxyl group in the gallic acid molecule reacts with the hydroxyl group in the carboxymethyl cellulose to be grafted onto the main chain.
[0047] In an embodiment of the present invention, the mass proportion of carboxymethyl groups in the carboxymethyl cellulose grafted with gallic acid is 10-40%.
[0048] Exemplarily, the mass proportion of carboxymethyl in carboxymethyl cellulose grafted gallic acid can be one of 10%, 12%, 15%, 18%, 20%, 25%, 28%, 30%, 35%, 38%, 40% or any value satisfying the above range.
[0049] In the embodiment of the present invention, the gallic acid accounts for 10-15% of the mass of the carboxymethyl cellulose grafted with gallic acid.
[0050] Illustratively, the gallic acid accounts for one of 10%, 11%, 12%, 13%, 14%, 15% of the mass of the carboxymethyl cellulose grafted with gallic acid, or any value satisfying the above range.
[0051] The second aspect of the present invention provides a method for preparing the modified cellulose antibacterial agent described in the first aspect of the present invention.
[0052] The preparation method of the modified cellulose antibacterial agent of the present invention is carried out according to the following steps.
[0053] (1) Preparation of carboxymethyl cellulose.
[0054] In an embodiment of the present invention, carboxymethyl cellulose is prepared by etherifying cellulose with chloroacetic acid.
[0055] In an embodiment of the present invention, the cellulose is α-cellulose.
[0056] In an embodiment of the present invention, the particle size of α-cellulose is 20-40 μm.
[0057] Exemplarily, the particle size of α-cellulose can be one of 20μm, 21μm, 22μm, 23μm, 24μm, 25μm, 26μm, 27μm, 28μm, 29μm, 30μm, 31μm, 32μm, 33μm, 34μm, 35μm, 36μm, 37μm, 38μm, 39μm, 40μm or any value satisfying the above range.
[0058] In an embodiment of the present invention, the mass ratio of chloroacetic acid to cellulose is (0.5-2):1.
[0059] Illustratively, the mass ratio of chloroacetic acid to cellulose can be one of 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1 or any value satisfying the above range.
[0060] In an embodiment of the present invention, the degree of substitution of carboxyl groups in the carboxymethyl cellulose is 0.45 to 1.55.
[0061] For example, the degree of substitution of carboxyl groups in carboxymethyl cellulose may be one of 0.45, 0.5, 0.54, 0.8, 1, 1.55, or any value satisfying the above range.
[0062] In an embodiment of the present invention, the preparation of carboxymethyl cellulose comprises the following steps:
[0063] The cellulose is dispersed in an ethanol solution containing hydroxide, and after alkalization for 0.5 to 1 hour, chloroacetic acid is added, and the reaction is carried out at a temperature of 55 to 65°C for 0.5 to 3 hours. After the reaction is completed, ethanol is used as a precipitant for precipitation and separation to obtain carboxymethyl cellulose.
[0064] In an embodiment of the present invention, the mass ratio of cellulose to hydroxide is 1:1.
[0065] In an embodiment of the present invention, the hydroxide is sodium hydroxide.
[0066] (2) Carboxymethyl cellulose grafted with gallic acid.
[0067] (2.1) Carboxymethyl cellulose, gallic acid and ascorbic acid are dissolved in water to obtain an aqueous solution.
[0068] In an embodiment of the present invention, the mass ratio of ascorbic acid to gallic acid is (0.15-0.4):1.
[0069] Illustratively, the mass ratio of ascorbic acid to gallic acid can be one of 0.15:1, 0.16:1, 0.17:1, 0.18:1, 0.19:1, 0.2:1, 0.21:1, 0.22:1, 0.23:1, 0.24:1, 0.25:1, 0.26:1, 0.27:1, 0.28:1, 0.29:1, 0.3:1, 0.31:1, 0.32:1, 0.33:1, 0.34:1, 0.35:1, 0.36:1, 0.37:1, 0.38:1, 0.39:1, 0.4:1 or any value satisfying the above range.
[0070] In an embodiment of the present invention, the mass ratio of gallic acid to carboxymethyl cellulose is (0.5-2):1.
[0071] Illustratively, the mass ratio of gallic acid to carboxymethyl cellulose can be one of 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1 or any value satisfying the above range.
[0072] In an embodiment of the present invention, the water is pure water.
[0073] (2.2) After nitrogen is introduced into the aqueous solution, a hydrogen peroxide solution is added to obtain carboxymethyl cellulose grafted with gallic acid via free radical grafting.
[0074] In the embodiment of the present invention, the reaction temperature of the free radical grafting is 70-85° C., and the time is 0.5-6 hours.
[0075] Illustratively, the reaction temperature can be one of 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C or any value satisfying the above range.
[0076] Illustratively, the reaction time can be one of 0.5 h, 0.6 h, 0.7 h, 0.8 h, 0.9 h, 1 h, 2 h, 3 h, 4 h, 5 h, 6 h or any value satisfying the above range.
[0077] In the embodiment of the present invention, the hydrogen peroxide solution is a hydrogen peroxide solution with a mass fraction of 30%.
[0078] In an embodiment of the present invention, the volume ratio of the added amount of hydrogen peroxide solution to the carboxymethyl cellulose solution is 5-10%.
[0079] For example, the volume ratio of the added amount of hydrogen peroxide solution to the carboxymethyl cellulose solution can be 5%, 6%, 7%, 8%, 9%, 10% or any value within the above range.
[0080] In an embodiment of the present invention, the hydrogen peroxide solution is added to the aqueous solution and then stirred uniformly.
[0081] The third aspect of the present invention provides a use of the modified cellulose antibacterial agent described in the first aspect of the present invention or the modified cellulose antibacterial agent prepared by the preparation method described in the second aspect of the present invention in inhibiting the growth of Escherichia coli and Staphylococcus aureus.
[0082] The modified cellulose antibacterial agent of the present invention and its preparation method and application will be described in detail below with reference to the accompanying drawings and specific examples.
[0083] If no specific technology or conditions are specified in the examples, the technology or conditions described in the literature in this field or the product instructions are used. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased through regular channels. The experimental methods in the following examples are all conventional methods unless otherwise specified. The test materials used in the following examples are all commercially available products unless otherwise specified.
[0084] In the following examples, the raw cellulose used is α-cellulose, and its particle size is 25 μm.
[0085] Example 1
[0086] (1) Preparation of carboxymethyl cellulose.
[0087] The cellulose is dispersed in an ethanol solution containing sodium hydroxide, with the mass ratio of cellulose to sodium hydroxide being 1:1, and alkalized at 55°C for 0.5h; then, chloroacetic acid is added, with the mass ratio of chloroacetic acid to cellulose being 0.6:1, and the reaction is carried out at 65°C for 3h; after the reaction is completed, ethanol is used as a precipitant, and precipitation and separation are performed to obtain carboxymethyl cellulose.
[0088] According to the analysis of NMR, the degree of substitution of carboxyl group is 0.54.
[0089] (2) Carboxymethyl cellulose grafted with gallic acid.
[0090] The carboxymethyl cellulose, gallic acid and ascorbic acid prepared in step (1) are dissolved in a four-necked flask containing pure water, nitrogen is introduced, and the mixture is stirred at 85° C. for 0.5 h, wherein the mass ratio of carboxymethyl cellulose to gallic acid is 1:0.5; thereafter, a 30% by mass hydrogen peroxide solution is added, stirred evenly, and reacted at 85° C. for 6 h. An ethanol solution is used as a precipitant, and precipitation and separation are performed to obtain carboxymethyl cellulose grafted with gallic acid (1).
[0091] Example 2
[0092] (1) Preparation of carboxymethyl cellulose.
[0093] In Example 2, carboxymethyl cellulose was prepared by the same preparation method as in Example 1.
[0094] (2) Carboxymethyl cellulose grafted with gallic acid.
[0095] The carboxymethyl cellulose prepared in step (1) is dissolved in a four-necked flask containing pure water, and nitrogen is introduced. The mixture is stirred at 85° C. for 0.5 h, and the mass ratio of carboxymethyl cellulose to gallic acid is 1:1. Thereafter, a 30% by mass hydrogen peroxide solution is added, stirred evenly, and reacted at 85° C. for 6 h. An ethanol solution is used as a precipitant, and precipitation and separation are performed to obtain carboxymethyl cellulose grafted with gallic acid (2).
[0096] Example 3
[0097] (1) Preparation of carboxymethyl cellulose.
[0098] In Example 3, carboxymethyl cellulose was prepared by the same preparation method as in Example 1.
[0099] (2) Carboxymethyl cellulose grafted with gallic acid.
[0100] The carboxymethyl cellulose prepared in step (1) is dissolved in a four-necked flask containing pure water, and nitrogen is introduced. The mixture is stirred at 85° C. for 0.5 h, and the mass ratio of carboxymethyl cellulose to gallic acid is 1:2. Thereafter, a 30% by mass hydrogen peroxide solution is added, stirred evenly, and reacted at 85° C. for 6 h. An ethanol solution is used as a precipitant, and precipitation and separation are performed to obtain carboxymethyl cellulose grafted with gallic acid (3).
[0101] In the present invention, infrared spectroscopy is performed on gallic acid, carboxymethyl cellulose, and carboxymethyl cellulose grafted with gallic acid. Figure 1As shown in Figure 2, the wave number 1593 cm appeared in the spectra of carboxymethyl cellulose and carboxymethyl cellulose grafted with gallic acid. -1 The broad peak is the characteristic absorption peak of C=O on the carboxyl group; the wave number 1729cm appears in the spectrum of carboxymethyl cellulose grafted with gallic acid -1 The absorption peak is the characteristic absorption peak of C=O on the ester group, which proves that the chloroacetic acid modifier (carboxymethyl) has been connected to the cellulose molecular chain and gallic acid has been successfully connected to the carboxymethyl cellulose molecular chain.
[0102] In the present invention, the antibacterial effect of the modified cellulose antibacterial agent prepared in the examples is described through an antibacterial test.
[0103] Antibacterial test
[0104] Escherichia coli and Staphylococcus aureus were used as test bacteria, and the plate streak method was used to test the inhibitory effect of carboxymethyl cellulose grafted with gallic acid on these two bacteria.
[0105] Dissolve 10 g of peptone, 5 g of sodium chloride, 3 g of beef powder and 15 g of agar in 1000 mL of pure water to prepare a nutrient agar medium. Add the nutrient agar medium into 6 conical flasks, which are marked as 1-6. Conical flask No. 1 is used as a control group without any additional treatment; gallic acid, carboxymethyl cellulose and carboxymethyl cellulose grafted gallic acid (1)-(3) obtained in Examples 1-3 are added into conical flasks 2-6, respectively.
[0106] After high temperature sterilization, pour the culture medium into the plate and inoculate the strain into the solid culture medium by plate streak method. Incubate in a 37℃ constant temperature incubator for 18 hours and observe the growth of bacteria. The results are as follows: Figure 2-3 shown.
[0107] in, Figure 2 (a)- Figure 2 The bacteria inoculated in the medium shown in (f) is Escherichia coli, Figure 3 (g)- Figure 3 (l) The bacteria inoculated in the culture medium shown is Staphylococcus aureus.
[0108] See also Figure 2 (b) and Figure 3 As shown in (h), when the dosage of gallic acid was 5 mg / mL, the growth of Escherichia coli and Staphylococcus aureus was significantly restricted.
[0109] See also Figure 2 (c) and Figure 3 As shown in (i), the addition amount of carboxymethyl cellulose was 15 mg / mL, which had no obvious inhibitory effect on the growth of both bacteria. Figure 2 (d)- Figure 2 (f) and Figure 3 (j)- Figure 3 As can be seen from (l), when the dosage of the carboxymethyl cellulose grafted gallic acid (1)-(3) obtained in Examples 1-3 was 15 mg / mL, the growth and reproduction of the two bacteria were significantly inhibited.
[0110] At the same time, the present invention also conducted a comparative test on the antibacterial performance of the carboxymethyl cellulose grafted with gallic acid (1) prepared in Example 1 and the existing carboxymethyl cellulose grafted with protocatechuic acid. The comparative test process and condition parameters are all referred to the above antibacterial test, and the test results are referred to Figure 4 shown.
[0111] like Figure 4 As shown, under the premise of the same dosage, the modified cellulose antibacterial agent prepared in the present invention has a better antibacterial effect than the modified cellulose scale inhibitor, i.e., carboxymethyl cellulose grafted with protocatechuic acid. The antibacterial rate of carboxymethyl cellulose grafted with gallic acid (1) against Escherichia coli is 93.4%, and the antibacterial rate against Staphylococcus aureus is 99.1%, while the antibacterial rate of carboxymethyl cellulose grafted with protocatechuic acid against Escherichia coli is 38.8%, and the antibacterial rate against Staphylococcus aureus is 87.2%. This also shows that the phenolic hydroxyl group in carboxymethyl cellulose grafted with gallic acid is more likely to bind to the cell membrane, changing the membrane structure and membrane potential, resulting in increased membrane permeability, and ultimately limiting the growth of bacteria.
[0112] In addition, the present invention also illustrates the scale inhibition effect of the modified cellulose antibacterial agent through a static scale inhibition test.
[0113] Static scale inhibition test
[0114] The carboxymethyl cellulose grafted gallic acid (1)-(3) prepared in Examples 1-3 were used as water treatment agents, and calcium chloride and sodium sulfate solutions were used as simulated salt water samples. Static scale inhibition experiments were conducted to determine the scale inhibition performance of the carboxymethyl cellulose grafted gallic acid (1)-(3) in the above water bodies.
[0115] Prepare 100 mL of a simulated solution with a pH value of 8, which contains 3000 mg / L of calcium ions and sulfate ions, and one of the carboxymethyl cellulose grafted gallic acid (1)-(3). Then, cool the solution to room temperature and filter it with a 20 μm filter paper. Titrate with a standard solution of disodium ethylenediaminetetraacetic acid (EDTA) to determine the concentration of calcium ions in the filtrate. The calculation formula (1) for the scale inhibition efficiency of carboxymethyl cellulose grafted gallic acid on calcium sulfate is as follows:
[0116]
[0117] V0 (mL) represents the consumption of EDTA solution when no scale inhibitor is added and no heating is performed; V1 (mL) represents the consumption of EDTA solution when no scale inhibitor is added and heating is performed; V2 (mL) represents the consumption of EDTA solution when no scale inhibitor is added and heating is performed.
[0118] See also Figure 5 As shown, the scale inhibition efficiency of carboxymethyl cellulose grafted with gallic acid (1)-(3) is significantly better than that of carboxymethyl cellulose. When the dosage is 15 mg / L, the scale inhibition efficiency reaches 98.8%, which significantly inhibits the formation of calcium sulfate scale.
[0119] In the present invention, the scale body after the test is also subjected to microscope analysis, see Figure 6 As shown in Figure 2, compared with carboxymethyl cellulose, after adding carboxymethyl cellulose grafted with gallic acid, the calcium sulfate crystals are destroyed, their surfaces become rough, and the scale volume formed is larger (see Figure 6 (b)), which directly proves that the carboxymethyl cellulose grafted with gallic acid prepared by the present invention can act as a scale inhibitor while inhibiting bacteria, and effectively alleviate the scaling problem in the water treatment process.
[0120] In addition, the present invention also conducted a comparative test on the scale inhibition of the carboxymethyl cellulose grafted with gallic acid (1) prepared in Example 1 and the existing scale inhibitor carboxymethyl cellulose grafted with protocatechuic acid. The comparative test process and condition parameters were all referred to the above static scale inhibition test.
[0121] The test results show that the scale inhibition efficiency of the carboxymethyl cellulose grafted with gallic acid (1) in the present invention is 97.3%, which is better than the scale inhibition efficiency of the existing carboxymethyl cellulose grafted with protocatechuic acid (86.7%), and has a better scale inhibition effect.
[0122] Meanwhile, the present invention further investigates the dispersibility of carboxymethyl cellulose grafted with gallic acid on iron oxide.
[0123] like Figure 7 As shown, under the tested concentration, when the sample concentration is greater than 20 mg / L, carboxymethyl cellulose grafted with gallic acid (1)-(3) has better dispersibility and can stably disperse the iron oxide particles in the solution, thereby showing a lower solution transmittance.
[0124] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention, and they should all be included in the scope of the claims and specification of the present invention. In particular, as long as there is no structural conflict, the various technical features mentioned in each embodiment can be combined in any way. The present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A modified cellulose antibacterial agent, characterized in that: The modified cellulose antibacterial agent is carboxymethyl cellulose grafted with gallic acid. The carboxymethyl cellulose grafted with gallic acid has carboxymethyl cellulose as the main chain, and the carboxyl groups in the gallic acid molecules react with the hydroxyl groups in the carboxymethyl cellulose to be grafted onto the main chain.
2. The modified cellulose antibacterial agent according to claim 1, characterized in that The mass proportion of the carboxymethyl group in the carboxymethyl cellulose grafted gallic acid is 10-40%.
3. The modified cellulose antibacterial agent according to claim 1, characterized in that The gallic acid accounts for 10-15% of the mass of the carboxymethyl cellulose grafted with gallic acid.
4. A method for preparing the modified cellulose antibacterial agent according to any one of claims 1 to 3, characterized in that: The following steps are involved: dissolving carboxymethyl cellulose and gallic acid in water to obtain an aqueous solution; After nitrogen is introduced into the aqueous solution, a hydrogen peroxide solution is added to obtain the carboxymethyl cellulose grafted with gallic acid through free radical grafting.
5. The preparation method according to claim 4, characterized in that: Ascorbic acid is also added to the aqueous solution; Preferably, the mass ratio of the ascorbic acid to the gallic acid is (0.15-0.4):
1.
6. The preparation method according to claim 4, characterized in that: The mass ratio of the gallic acid to the carboxymethyl cellulose is (0.5-2):
1.
7. The preparation method according to claim 4, characterized in that: The reaction temperature of the free radical grafting is 70-85° C., and the reaction time is 0.5-6 hours.
8. The preparation method according to claim 4, characterized in that: The hydrogen peroxide solution is a hydrogen peroxide solution with a mass fraction of 30%; Preferably, the volume ratio of the added amount of the hydrogen peroxide solution to the carboxymethyl cellulose solution is 5-10%.
9. The preparation method according to claim 4, characterized in that: The carboxymethyl cellulose is prepared by etherifying cellulose and chloroacetic acid; Preferably, the mass ratio of the chloroacetic acid to the cellulose is (0.5-2):1; Preferably, the degree of substitution of carboxyl groups in the carboxymethyl cellulose is 0.45 to 1.
55.
10. Use of the modified cellulose antibacterial agent according to any one of claims 1 to 3 or the modified cellulose antibacterial agent prepared by the preparation method according to any one of claims 4 to 9 in inhibiting the growth of Escherichia coli and Staphylococcus aureus.
Citation Information
Cited By