Composite absorbent and corrosion-resistant wave-absorbing coating
By using composite absorbers of modified ferroferrite magnetic nanoparticles and other materials, a coating with excellent absorbing properties and corrosion resistance is prepared, which solves the problem in the existing technology that it is difficult to balance the corrosion resistance of absorbing coatings and achieves Material development with broad application prospects.
Patent Information
- Application Number
- CN202410705383.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-03
AI Technical Summary
It is difficult for existing wave-absorbing coatings to balance corrosion resistance and wave-absorbing properties, and there is a lack of better materials.
Modified ferroferrite magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide composite absorbers are used to prepare corrosion-resistant absorbing coatings through a combination of modified epoxy resin and thickener , forming a composite material with excellent wave absorption performance and corrosion resistance.
It has achieved a minimum reflection loss of -61.53dB, an absorption bandwidth ranging from 10.1 to 14.2GHz, and significantly improved anti-corrosion and salt water resistance, making it suitable for marine environments and radar stealth materials.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of development of radar absorbing coatings, and in particular to a composite absorber and a corrosion-resistant radar absorbing coating. Background Art
[0002] Absorbing materials refer to a type of material that can absorb or significantly reduce the electromagnetic wave energy received on its surface, thereby reducing the interference of electromagnetic waves. In engineering applications, in addition to requiring absorbing materials to have a high absorption rate of electromagnetic waves in a wide frequency band, they are also required to have properties such as light weight, temperature resistance, moisture resistance, and corrosion resistance.
[0003] In modern society, with the rapid development of science and technology, various portable and wearable devices have emerged in an endless stream, which has greatly promoted economic development and improved lifestyles, but at the same time has also caused serious electromagnetic wave pollution. In the civilian field, electromagnetic wave pollution, on the one hand, interferes with precision instruments, navigation systems, and medical equipment, affecting the normal operation of electronic equipment; on the other hand, electromagnetic wave pollution can also cause human neurasthenia, induce cell pathology, and cause health problems. In the military field, radar detection technology and wireless detection technology are becoming increasingly mature, which puts higher requirements on radar stealth technology. Radar stealth technology can effectively avoid detection and attack by reducing the radar scattering and reflection area of the detected target, and improve the defense and survivability of combat equipment. However, the development of absorbing materials that are suitable for different environments is one of the main strategies to achieve radar stealth. Therefore, the study of new functional materials with strong environmental adaptability and excellent absorbing performance has scientific value and practical significance in many fields.
[0004] Chinese patent CN117106361A discloses a corrosion-resistant absorbing coating and a preparation method thereof, comprising the following components in parts by weight: 20-30 parts of resin; 20-40 parts of diluent; 5-10 parts of curing agent; 2-4 parts of filler; 1-2 parts of surfactant; 5-10 parts of porous ceramics; 3-5 parts of graphene; 1-3 parts of carbon fiber. A method for preparing a corrosion-resistant absorbing coating comprises the following steps: S1, mixing resin, diluent, surfactant, porous ceramics, graphene, carbon fiber, and filler to obtain a mixture; S2, adding curing agent to the mixture, mixing, and obtaining. The corrosion-resistant absorbing coating can be used to coat the surface of metal pipes, and has the advantages of strong corrosion resistance and strong absorbing performance; the preparation method has the advantages of simple and efficient process and easy industrial scale preparation of coatings.
[0005] Chinese patent CN117070129A discloses a highly efficient absorbing coating and a preparation method thereof, comprising the following components by weight: 45-90 parts of resin; 15-30 parts of solvent; 4-9 parts of curing agent; 3-9 parts of filler; 3-5 parts of rare earth oxide; and 20-45 parts of radiation protection composition; the raw materials for preparing the radiation protection composition include porous ceramics, adhesives, radioactive isotopes, and silane. The prepared coating has excellent corrosion resistance and wave absorption performance. The prepared coating is tested, and the reflection loss of the coating is -29.5dB and the acid resistance grade reaches level 1. The preparation method of the highly efficient absorbing coating comprises the following steps: S1, mixing resin, solvent, curing agent, and rare earth oxide to obtain a mixture; S2, adding the radiation protection composition and filler to the mixture, mixing, and obtaining. The prepared coating has strong reflection loss capacity and excellent corrosion resistance, and can be coated on the surface of metal pipes to improve performance.
[0006] Chinese patent CN117511338A discloses a light-weight absorbing coating for marine environment and its preparation method, the absorbing coating comprises a nano light-density absorber coating pre-dispersion, a nano dielectric loss type heavy-density absorber and a curing agent; and the nano light-density absorber coating pre-dispersion contains a material prepared by in-situ preparation of a highly crystalline carbon-coated single-walled carbon nanotube, the highly crystalline carbon-coated single-walled carbon nanotube has a stable structure, and not only has excellent absorbing characteristics but also has good corrosion resistance. When the absorbing coating prepared by the present invention has a coating thickness of 10 mm, within the frequency range of 2-18 GHz, the absorption bandwidth of ≤-10 dB exceeds 11.6 GHz, and at the same time, the reflectivity changes within ±5% after 1200 hours under neutral salt spray conditions, which can improve the environmental adaptability and life of the absorbing coating.
[0007] However, it can be seen from the above-mentioned prior art that the above-mentioned absorbing coating cannot achieve both corrosion resistance and absorbing performance, and there is still a lack of materials with better corrosion resistance and absorbing performance. Summary of the invention
[0008] The object of the present invention is to provide a composite absorber and a corrosion-resistant microwave-absorbing coating, which have excellent corrosion resistance and microwave-absorbing properties.
[0009] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0010] The present invention provides a composite absorbent comprising the following components:
[0011] Modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide.
[0012] Preferably, the modified ferroferric oxide magnetic nanoparticles are polyethyleneimine-modified ferroferric oxide magnetic nanoparticles.
[0013] Preferably, the weight ratio of the modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide is 8-12:8-12:8-12:4-6:1-3:1-3.
[0014] The invention also provides application of the composite absorber in preparing radar absorbing coating.
[0015] The present invention also provides a corrosion-resistant wave-absorbing coating, comprising the above-mentioned composite absorber, a coating matrix material and a coating additive.
[0016] Preferably, the corrosion-resistant radar-absorbing coating comprises the following components in parts by weight:
[0017] 50-70 parts of composite absorbent, 80-120 parts of coating base material and 0.5-5 parts of coating additive.
[0018] Preferably, the coating matrix material is modified epoxy resin.
[0019] Preferably, the modified epoxy resin is a polyurethane modified epoxy ester resin.
[0020] Preferably, the coating additive is a thickener.
[0021] The present invention also provides the use of the corrosion-resistant wave-absorbing coating in the preparation of electromagnetic wave pollution-resistant materials or radar stealth materials.
[0022] Technical effects and advantages of the present invention:
[0023] The present invention adopts modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide to compound a composite absorber. The materials can achieve complementary wave absorbing performance and can produce excellent effects when used in wave absorbing coatings, with minimum reflection loss RL min It can reach -61.53dB, and the absorption bandwidth range is 10.1-14.2GHz. The corrosion-resistant absorbing coating prepared by using the composite absorber of the present invention has significantly improved corrosion resistance and salt water resistance, and can be used in marine substrates, with broad application prospects. DETAILED DESCRIPTION
[0024] The present invention provides a composite absorbent, comprising the following components: modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide; in the present invention, the modified ferroferric oxide magnetic nanoparticles are preferably polyethyleneimine-modified ferroferric oxide magnetic nanoparticles; the weight ratio of the modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide is preferably 8-12:8-12:8-12:4-6:1-3:1-3.
[0025] The invention also provides application of the composite absorber in preparing radar absorbing coating.
[0026] The present invention also provides a corrosion-resistant absorbing coating, comprising the above-mentioned composite absorber, a coating base material and a coating additive; preferably, the corrosion-resistant absorbing coating comprises the following components in parts by weight: 50 to 70 parts of the composite absorber, 80 to 120 parts of the coating base material and 0.5 to 5 parts of the coating additive; preferably, the coating base material is a modified epoxy resin; preferably, the modified epoxy resin is a polyurethane-modified epoxy ester resin; further preferably, the coating additive is a thickener.
[0027] The present invention also provides the use of the above-mentioned corrosion-resistant wave-absorbing coating in the preparation of anti-electromagnetic wave pollution materials or radar stealth materials, and the coating thickness is preferably above 1.5 mm.
[0028] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0029] The Chinese name of PEI@Fe3O4 used in the embodiment is polyethyleneimine-modified ferroferric oxide magnetic nanoparticles, purchased from Shanghai Buwei Applied Materials Technology Co., Ltd., CAS: 1317-61-9;
[0030] The modified epoxy resin was purchased from Wuhan Shiquanxing New Materials Technology Co., Ltd., the trade name is polyurethane modified epoxy ester resin, the product number is SZ-2360;
[0031] The thickener was purchased from Wuhan Runxingyuan Technology Co., Ltd. with the product number of QSC-935.
[0032] Example 1
[0033] Prepare absorbent:
[0034] Mix all the ingredients in the following weight ratio:
[0035] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 10:10:10:5:3:2.
[0036] Formulating corrosion-resistant and radar-absorbing coatings:
[0037] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0038] Wave absorption performance test:
[0039] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0040] The results show that the minimum reflection loss RL of the experimental sample is min It is -61.53dB, and the absorption bandwidth range is 10.1~14.2GHz, with excellent absorption performance.
[0041] Anti-corrosion performance test:
[0042] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0043] The results showed that the anti-corrosion performance of the experimental samples was level 1 and the coating was almost not damaged.
[0044] Salt water resistance test:
[0045] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0046] The results showed that the salt water resistance of the experimental samples was level 1 and the coating was almost not damaged.
[0047] Example 2
[0048] Prepare absorbent:
[0049] Mix all the ingredients in the following weight ratio:
[0050] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 10:10:8:5:3:2.
[0051] Formulating corrosion-resistant and radar-absorbing coatings:
[0052] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0053] Wave absorption performance test:
[0054] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0055] The results show that the minimum reflection loss RL of the experimental sample is min It is -59.55dB, and the absorption bandwidth ranges from 10.1 to 14.1GHz, with excellent absorption performance.
[0056] Anti-corrosion performance test:
[0057] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0058] The results showed that the anti-corrosion performance of the experimental samples was level 1 and the coating was almost not damaged.
[0059] Salt water resistance test:
[0060] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0061] The results showed that the salt water resistance of the experimental samples was level 1 and the coating was almost not damaged.
[0062] Example 3
[0063] Prepare absorbent:
[0064] Mix all the ingredients in the following weight ratio:
[0065] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 10:10:12:5:3:2.
[0066] Formulating corrosion-resistant and radar-absorbing coatings:
[0067] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0068] Wave absorption performance test:
[0069] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0070] The results show that the minimum reflection loss RL of the experimental sample is min It is -59.67dB, and the absorption bandwidth range is 10.1~14.1GHz, with excellent absorption performance.
[0071] Anti-corrosion performance test:
[0072] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0073] The results showed that the anti-corrosion performance of the experimental samples was level 1 and the coating was almost not damaged.
[0074] Salt water resistance test:
[0075] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0076] The results showed that the salt water resistance of the experimental samples was level 1 and the coating was almost not damaged.
[0077] Example 4
[0078] Prepare absorbent:
[0079] Mix all the ingredients in the following weight ratio:
[0080] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 10:10:10:5:3:2.
[0081] Formulating corrosion-resistant and radar-absorbing coatings:
[0082] 100 parts of modified epoxy resin, 55 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0083] Wave absorption performance test:
[0084] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0085] The results show that the minimum reflection loss RL of the experimental sample is min It is -59.39dB, and the absorption bandwidth range is 10.1~14.0GHz, with excellent absorption performance.
[0086] Anti-corrosion performance test:
[0087] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0088] The results showed that the anti-corrosion performance of the experimental samples was level 1 and the coating was almost not damaged.
[0089] Salt water resistance test:
[0090] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0091] The results showed that the salt water resistance of the experimental samples was level 1 and the coating was almost not damaged.
[0092] Example 5
[0093] Prepare absorbent:
[0094] Mix all the ingredients in the following weight ratio:
[0095] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 10:10:10:5:3:2.
[0096] Formulating corrosion-resistant and radar-absorbing coatings:
[0097] 100 parts of modified epoxy resin, 65 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0098] Wave absorption performance test:
[0099] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0100] The results show that the minimum reflection loss RL of the experimental sample is min It is -60.57dB, and the absorption bandwidth range is 10.1~14.3GHz, with excellent absorption performance.
[0101] Anti-corrosion performance test:
[0102] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0103] The results showed that the anti-corrosion performance of the experimental samples was level 1 and the coating was almost not damaged.
[0104] Salt water resistance test:
[0105] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0106] The results showed that the salt water resistance of the experimental samples was level 1 and the coating was almost not damaged.
[0107] Comparative Example 1
[0108] Prepare absorbent:
[0109] Mix all the ingredients in the following weight ratio:
[0110] SiC powder: graphene: polydopamine: aluminum oxide: titanium oxide = 15:5:5:3:2.
[0111] Formulating corrosion-resistant and radar-absorbing coatings:
[0112] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0113] Wave absorption performance test:
[0114] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0115] The results show that the minimum reflection loss RL of the experimental sample is min It is -35.73dB, and the absorption bandwidth ranges from 11.2 to 12.8GHz.
[0116] Anti-corrosion performance test:
[0117] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0118] The results show that the corrosion resistance of the experimental samples is level 3.
[0119] Salt water resistance test:
[0120] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0121] The results show that the salt water resistance of the experimental samples is level 1.
[0122] Comparative Example 2
[0123] Prepare absorbent:
[0124] Mix all the ingredients in the following weight ratio:
[0125] SiC powder:graphene:PEI@Fe3O4:alumina=10:10:10:5.
[0126] Formulating corrosion-resistant and radar-absorbing coatings:
[0127] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0128] Wave absorption performance test:
[0129] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0130] The results show that the minimum reflection loss RL of the experimental sample is min It is -41.96dB, and the absorption bandwidth ranges from 10.6 to 12.4GHz.
[0131] Anti-corrosion performance test:
[0132] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0133] The results show that the corrosion resistance of the experimental samples is level 3.
[0134] Salt water resistance test:
[0135] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0136] The results show that the salt water resistance of the experimental samples is level 2.
[0137] Comparative Example 3
[0138] Prepare absorbent:
[0139] Mix all the ingredients in the following weight ratio:
[0140] SiC powder: graphene: PEI@Fe3O4: alumina: titanium oxide = 15:5:10:3:2.
[0141] Formulating corrosion-resistant and radar-absorbing coatings:
[0142] 100 parts of modified epoxy resin, 65 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a radar absorbing coating.
[0143] Wave absorption performance test:
[0144] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0145] The results show that the minimum reflection loss RL of the experimental sample is min It is -46.91dB, and the absorption bandwidth ranges from 10.6 to 13.1GHz.
[0146] Anti-corrosion performance test:
[0147] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0148] The results show that the corrosion resistance of the experimental samples is level 4.
[0149] Salt water resistance test:
[0150] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0151] The results show that the salt water resistance of the experimental samples is level 3.
[0152] Comparative Example 4
[0153] Prepare absorbent:
[0154] Mix all the ingredients in the following weight ratio:
[0155] SiC powder: graphene: PEI@Fe3O4: polydopamine: alumina: titanium oxide = 5:5:15:15:2:3.
[0156] Formulating corrosion-resistant and radar-absorbing coatings:
[0157] 100 parts of modified epoxy resin, 60 parts of absorbent and 0.5 parts of thickener were weighed, mixed in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0158] Wave absorption performance test:
[0159] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0160] The results show that the minimum reflection loss RL of the experimental sample is min It is -38.89dB, and the absorption bandwidth ranges from 11.0 to 13.3GHz.
[0161] Anti-corrosion performance test:
[0162] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0163] The results show that the corrosion resistance of the experimental samples is level 2.
[0164] Salt water resistance test:
[0165] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0166] The results show that the salt water resistance of the experimental samples is level 2.
[0167] Comparative Example 5
[0168] Prepare absorbent:
[0169] Mix all the ingredients in the following weight ratio:
[0170] Graphene:PEI@Fe3O4:alumina:titanium oxide=15:15:5:5.
[0171] Formulating corrosion-resistant and radar-absorbing coatings:
[0172] Weigh 100 parts of common epoxy resin, 50 parts of absorbent, and 0.5 parts of thickener, mix them in an ultracentrifuge at 35° C. for 30 minutes to obtain a corrosion-resistant radar-absorbing coating.
[0173] Wave absorption performance test:
[0174] The above coating was used as a sample, and aluminum alloy was used as the coating substrate for the experiment. The coating thickness was 2 mm. The wave absorption performance of the material was tested by the coaxial probe method using a vector network analyzer:
[0175] The results show that the minimum reflection loss RL of the experimental sample is min It is -33.20dB, and the absorption bandwidth ranges from 10.7 to 11.9GHz.
[0176] Anti-corrosion performance test:
[0177] The coated substrate was immersed in a 30% sulfuric acid solution. After two weeks, the corrosion of the coating was observed and recorded. The corrosion degree was evaluated according to levels 1 to 5, where level 5 showed that the coating was almost completely destroyed and lost its protective ability, indicating that the coating had the worst corrosion resistance.
[0178] The results show that the corrosion resistance of the experimental samples is level 5.
[0179] Salt water resistance test:
[0180] The coated substrate was immersed in a 3% sodium chloride solution and heated to 40°C. After two weeks, the corrosion of the coating was observed and recorded. The degree of corrosion was evaluated on a scale of 1 to 5, with 5 indicating that the coating was almost completely corroded and had the worst salt water resistance.
[0181] The results show that the salt water resistance of the experimental samples is level 5.
[0182] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite absorbent, characterized in that: Includes the following components: Modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide.
2. The composite absorbent according to claim 1, characterized in that: The modified ferroferric oxide magnetic nanoparticles are ferroferric oxide magnetic nanoparticles modified by polyethyleneimine.
3. The composite absorbent according to claim 1 or 2, characterized in that: The weight ratio of the modified ferroferric oxide magnetic nanoparticles, silicon carbide, graphene, polydopamine, aluminum oxide and titanium oxide is 8-12:8-12:8-12:4-6:1-3:1-3.
4. Use of the composite absorber according to any one of claims 1 to 3 in the preparation of radar absorbing coatings.
5. A corrosion-resistant radar absorbing coating, characterized in that: The invention comprises the composite absorbent as claimed in any one of claims 1 to 3, a coating matrix material and a coating additive.
6. The corrosion-resistant radar absorbing coating according to claim 5, characterized in that: The corrosion-resistant radar-absorbing coating comprises the following components in parts by weight: 50-70 parts of composite absorbent, 80-120 parts of coating base material and 0.5-5 parts of coating additive.
7. The corrosion-resistant radar absorbing coating according to claim 5 or 6, characterized in that: The coating matrix material is modified epoxy resin.
8. The corrosion-resistant radar absorbing coating according to claim 7, characterized in that: The modified epoxy resin is polyurethane modified epoxy ester resin.
9. The corrosion-resistant radar absorbing coating according to claim 5 or 6, characterized in that: The coating additive is a thickener.
10. Use of the corrosion-resistant and radar-absorbing coating according to any one of claims 5 to 9 in the preparation of electromagnetic wave pollution-resistant materials or radar stealth materials.
Citation Information
Patent Citations
Polymine-coated ferroferric oxide magnetic nanoparticle and synthesis method thereof
CN101819871A
Preparation method of porous sponge with electromagnetic shielding performance, wave absorption performance and sound absorption performance
CN109265728A
High-temperature-resistant electromagnetic wave absorbing paint, coating and preparation method and application thereof
CN111205743A
Preparation method and application of modified ferroferric oxide
CN116986637A
Electromagnetic wave absorbing material with high thermal conductivity
CN117939865A
Cited By
Low-VOC (volatile organic compound) epoxy resin coating based on nano modification technology and preparation method thereof
CN119161785A
A CNT-based corrosion-resistant electromagnetic wave absorbing composite material and a preparation method thereof
CN122917489A