Super-hydrophobic mildew-proof mineral putty powder and preparation method thereof

Through hydrophobically modified calcium oxide and magnesium oxide, as well as nano-silica, the putty powder is endowed with super-hydrophobic and micro-nano structure, which solves the harm and timeliness problems of existing putty powder antifungal agents to the human body and the environment, and achieves long-term Effective physical anti-mildew effect and good breathability.

CN118725632APending Publication Date: 2024-10-01JIANGXI FUXING ENERGY SAVING BUILDING MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410994585.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

The antifungal agents used in existing putty powder are potentially harmful to the human body and the environment, and the antifungal effect is time-sensitive and difficult to maintain for a long time.

Method used

By hydrophobically modifying calcium oxide and magnesium oxide, and adding nano-sized hydrophobic fumed silica, the putty powder is endowed with super-hydrophobic properties and a micro-nano pore structure, which physically prevents mold growth and avoids the use of chemical antifungal agents.

Benefits of technology

It achieves the long-term effective anti-mold effect of putty powder, has no potential harm to the human body and the environment, has good breathability, and reduces mold adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118725632A_ABST
    Figure CN118725632A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of putty powder processing, and discloses super-hydrophobic mildew-proof mineral putty powder and a preparation method thereof. The super-hydrophobic mildew-proof mineral putty powder is prepared from the following components in parts by weight: 22 to 35 parts of hydrophobic modified calcium oxide, 62 to 75 parts of hydrophobic modified magnesium oxide, 0 to 10 parts of hydrophobic gas-phase nano silicon dioxide, 32 to 40 parts of Portland cement, 0.1 to 0.29 part of oxypropyl methyl fiber, 0.8 to 1.0 part of inorganic rubber powder, 0.05 to 0.1 part of functional additive, 50 to 80 parts of deionized water and 5 to 10 parts of ethanol. A physical mildew-proof method is provided, calcium oxide and magnesium oxide are subjected to hydrophobic modification, the putty powder is endowed with super-hydrophobic performance, water cannot be attached to the surface of the putty powder, mildew cannot grow, meanwhile, nano-sized hydrophobic fumed silica is added into the raw materials, and the mildew-proof performance of the putty powder is improved. The surface of a wall painted by using the putty powder has abundant micro-nano structures, has good air permeability, and further prevents the growth of mould.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a super-hydrophobic and mildew-proof mineral putty powder and a preparation method thereof, and belongs to the field of putty powder processing. Background Art

[0002] Putty is a base material used for wall repair and leveling, laying a good foundation for the next step of decoration, painting and wallpapering. Putty is divided into two types: interior wall and exterior wall. Exterior wall putty must resist wind and sun, so it has strong adhesiveness, high strength, and a slightly lower environmental protection index. The comprehensive index of interior wall putty is better, healthy and environmentally friendly, so it is not used for interior walls and exterior walls. Usually putty is based on gypsum or cement, so it is easier to adhere to the rough surface. However, during construction, a layer of interface agent should be applied on the base to seal the base and improve the adhesion of the wall, so that the putty can better adhere to the base.

[0003] Putty is generally composed of base material, filler, water and additives. Base material, also known as binder, is the most critical component of putty, mainly playing various roles such as bonding. The most commonly used binders for putty are cement and organic polymers, which are divided into emulsions and latex powders. Cement is a binder with good adhesion, durability and reasonable cost performance, but its tensile strength and crack resistance are poor. Organic polymers can modify and toughen it, thereby improving the performance of putty. Fillers mainly play a filling role, and commonly used ones include calcium carbonate, talcum powder and quartz sand. Attention should be paid to the matching of filler fineness. Additives include thickeners, water retaining agents, etc. Thickeners and water retaining agents play the role of water retention, improving storage and construction performance, and generally use cellulose. Antifreeze agents mainly improve the storage stability of putty at low temperatures. Slip agents and water reducers are generally used in high-end putties to improve the construction performance of putty. Some also add fibers to play an anti-cracking role.

[0004] Traditional putty has a short service life, poor water resistance, weak adhesion, needs to be removed during secondary decoration, has poor adhesion to the wall, is easily moldy due to the influence of the wall, and has poor environmental performance. For this reason, researchers began to explore the preparation of mildew-proof and environmentally friendly putty powder.

[0005] Chinese patent [202011014315.3] discloses a mildew-proof and antibacterial putty powder and its preparation method and use method. Mold-proof putty powder is prepared by using methyl thiophanate as a mildew-proof agent, and is compounded with silicate cement, lime lime, talcum powder, hydrogen ethyl methyl cellulose, polyvinyl alcohol and amylase, which has good mildew-proof effect. However, methyl thiophanate has certain biological toxicity and is not conducive to environmental protection. In addition, the mildew-proof effect of methyl thiophanate has a certain timeliness. When methyl thiophanate loses its activity or its content is lost over time, the putty powder provided by the invention will lose its mildew-proof effect.

[0006] Chinese patent [202111670555.3] discloses a water-resistant and mildew-proof interior wall putty powder and its preparation method, which uses nano copper ion additives as mildew-proof agents, and 200-mesh heavy calcium powder, white cement, hydroxypropyl methylcellulose ether, latex powder, polyvinyl alcohol, mica powder, modified nano silicon dioxide, bentonite and starch ether to prepare mildew-proof putty powder, which has good mildew-proof effect. Copper ions, as a heavy metal ion, have a strong toxic effect on the human body, and using them as decorative materials for house walls may cause harm to the human body. At the same time, copper ions will slowly flow into the environment, causing pollution to the ecological environment, which is not conducive to environmental protection.

[0007] Chinese patent [202011534968.4] discloses an antibacterial and mildew-proof putty powder, which uses zinc pyrithione as a mildew-proof agent, and is mixed with modified cationic coumarins, hyperbranched organic montmorillonite, heavy calcium carbonate, zinc pyrithione, modified white cement, hyperbranched starch, and 2,6-di(oxirane-2-methyl)-1,2,3,5,6,7-hexahydropyrrolo[3,4-f]isoindole-1,3,5,7-tetraketone to prepare a mildew-proof putty powder with good mildew-proof effect. Zinc ions, as a heavy metal ion, have certain toxic effects on the human body and the environment, which is not conducive to human health and environmental protection. At the same time, its mildew-proof effect has a certain timeliness.

[0008] In summary, at present, the existing technology mainly uses chemical methods to prevent mildew, mainly by adding mildew inhibitors to putty powder, so that mold cannot grow on the surface of putty powder, and has a good mildew-proof effect. However, mildew inhibitors also have potential hazards to the human body. Long-term exposure to walls mixed with mildew inhibitors has certain toxic effects on human health. At the same time, the content of mildew inhibitors will inevitably decrease with the passage of time, which will reduce the mildew-proof effect or even lose the mildew-proof effect.

[0009] Therefore, in view of the above problems, the present invention proposes a super hydrophobic and mildew-proof mineral putty powder and a preparation method thereof by a physical mildew-proof method. The putty powder gives the wall super hydrophobicity, so that moisture cannot adhere to the wall surface, and there is no necessary condition for the growth of mold. In addition, the putty powder has a rich micro-nano pore structure and good air permeability, which can further prevent the growth of mold. Summary of the invention

[0010] In view of the shortcomings of the current use of mildew inhibitors in putty powder, which poses a potential threat to human body, is not environmentally friendly and the mildew-proof effect cannot be maintained for a long time, the present invention hydrophobically modifies calcium oxide and magnesium oxide to give the putty powder super-hydrophobic properties, so that moisture cannot adhere to its surface and mold cannot grow. At the same time, nano-sized hydrophobic fumed silica is added to the raw materials. The surface of the wall painted with the putty powder has rich micro-nano structures and good air permeability, which further prevents the growth of mold.

[0011] The invention provides a super hydrophobic and mildew-proof mineral putty powder. The super hydrophobic and mildew-proof mineral putty powder is composed of 22 to 35 parts of hydrophobically modified calcium oxide, 62 to 75 parts of hydrophobically modified magnesium oxide, 0 to 10 parts of hydrophobic fumed nano silicon dioxide, 32 to 40 parts of silicate cement, 0.1 to 0.29 parts of oxypropyl methyl fiber, 0.8 to 1.0 parts of inorganic rubber powder, 0.05 to 0.1 parts of functional additives, 50 to 80 parts of deionized water and 5 to 10 parts of ethanol in parts by weight.

[0012] In some embodiments, the preparation of the hydrophobically modified calcium oxide comprises the following steps:

[0013] S1: preparing a hydrophobic modification solution: adding a hydrophobic modifier to an n-heptane solution, wherein the mass fraction ratio of the hydrophobic modifier to the n-heptane is 1:8-10, and reacting at 20-30° C. and a stirring speed of 200-500 rpm for 0.5-1 hour to obtain a hydrophobic modification solution;

[0014] S2 Hydrophobic modification of calcium oxide: Add calcium oxide to the prepared hydrophobic modification solution in a mass fraction ratio of calcium oxide to solution of 5 to 10:1, react at a temperature of 20 to 30°C and a stirring speed of 200 to 500 rpm for 18 to 24 hours, filter, collect the filtrate and residue separately, wash the residue with n-heptane three times, and collect the filtrate, dry the residue at 40 to 50°C and a pressure of 0.1 mbar for 12 to 18 hours to obtain hydrophobically modified calcium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0015] In some of the embodiments, the hydrophobic modifier in S1 is at least one of octadecyl fatty acid, octadecyl fatty acid methyl ester, octadecyl fatty acid ethyl ester, octadecyl fatty acid propyl ester, propyltrichlorosilane and ethyltrichlorosilane.

[0016] In some embodiments, the preparation of the hydrophobically modified magnesium oxide comprises the following steps:

[0017] S3: preparing a hydrophobic modification solution: adding a hydrophobic modifier to an n-heptane solution, wherein the mass fraction ratio of the hydrophobic modifier to the n-heptane is 1:8-10, reacting at 20-30° C. and a stirring speed of 200-500 rpm for 0.5-1 hour to obtain a hydrophobic modification solution;

[0018] S4 Hydrophobic modification of magnesium oxide: Add magnesium oxide to the prepared hydrophobic modification solution with a mass fraction ratio of calcium oxide to solution of 5 to 7:1, react at a temperature of 20 to 30°C and a stirring speed of 200 to 500 rpm for 12 to 18 hours, filter, collect the filtrate and residue separately, wash the residue with n-heptane 3 times, collect the filtrate, dry the residue at 40 to 50°C and a pressure of 0.1 mbar for 12 to 18 hours to obtain hydrophobically modified magnesium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0019] In some of the embodiments, the hydrophobic modifier in S1 is at least one of octadecyl fatty acid, octadecyl fatty acid methyl ester, octadecyl fatty acid ethyl ester, octadecyl fatty acid propyl ester, propyltrichlorosilane and ethyltrichlorosilane.

[0020] In some of the embodiments, the particle size of the hydrophobic fumed silica is 20-70 nm.

[0021] In some of the embodiments, the functional additive is at least one of an antifreeze agent, a thermal insulation agent, an electromagnetic radiation eliminator and an inorganic mineral pigment. The antifreeze agent includes the following raw materials in weight parts: 5 to 7 parts of calcium chloride, 5 to 7 parts of sodium pyrophosphate and 5 to 7 parts of sodium tripolyphosphate; the thermal insulation agent includes the following raw materials in weight parts: 6 to 8 parts of aluminum oxide and 6 to 8 parts of iron oxide; the electromagnetic radiation eliminator includes the following raw materials in weight parts: 5 to 8 parts of nano-scale silver fibers and 5 to 8 parts of conductive powder; the inorganic mineral pigment includes the following raw materials in weight parts: 8 to 10 parts of cinnabar powder and 8 to 10 parts of red clay powder.

[0022] The present invention also provides a method for preparing a super hydrophobic and mildew-proof mineral putty powder, the preparation method comprising the following steps:

[0023] S5: adding hydrophobically modified calcium oxide, hydrophobically modified magnesium oxide, silicate cement, oxypropyl methyl fiber and inorganic rubber powder into the synthesis reactor according to the formula amount, stirring at a speed of 800 to 1200 rpm and a temperature of 20 to 30° C. for 10 to 20 minutes to mix the various powders evenly to obtain a composite powder;

[0024] S6: adding a functional additive to the mixture obtained by S5, stirring at a rate of 800 to 1200 rpm and a temperature of 20 to 30° C. for 10 to 20 minutes, and standing for 5 minutes to obtain a super hydrophobic and mildew-proof mineral putty powder;

[0025] S7: The super hydrophobic and mildew-proof mineral putty powder obtained in S6 is mixed again through a 200-250 mesh sieve;

[0026] S8: Dry the super hydrophobic and mildew-proof mineral putty powder screened in S7 at a temperature of 100 to 110° C. for 3 to 6 hours, and then pack it into bags after drying, with a specification of 15 or 20 kg / bag.

[0027] The present invention has the following advantages:

[0028] (1) The present invention uses calcium oxide and magnesium oxide as raw materials for putty powder, so that the putty powder has hydrophobic properties after being painted on the wall, so that moisture cannot adhere to the surface, thereby limiting the growth of mold, which belongs to physical mildew prevention and has long-term effectiveness;

[0029] (2) Using nano-sized hydrophobic fumed silica as putty powder can not only increase its hydrophobic effect, but also give the wall a micro-nanostructured pore structure, which has good air permeability and reduces the attachment of mold;

[0030] (3) The present invention does not use any chemical mildew inhibitors, and the raw materials are environmentally friendly materials that will not have any potential harmful effects on the human body or damage the environment, thus complying with the green and environmentally friendly production concept;

[0031] (4) The present invention hydrophobically modifies calcium oxide and magnesium oxide so that their surfaces have alkyl groups, which is beneficial to improving their compatibility with the inorganic rubber powder in the formula. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 From left to right are the water contact angle test graphs of unmodified calcium oxide and Examples 1 to 3;

[0033] Figure 2 From left to right are the water contact angle test graphs of unmodified magnesium oxide and Examples 4 to 6;

[0034] Figure 3 Preparation flow chart of super hydrophobic and mildew-proof mineral putty powder;

[0035] Figure 4 From left to right are the water contact angle test graphs of the super hydrophobic and mildew-proof mineral putty powder prepared in Examples 7 to 9;

[0036] Figure 5 From left to right are scanning electron microscope images of the super hydrophobic and mildew-proof mineral putty powder prepared in Examples 7 to 9. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings, technical process steps, specific implementation conditions and materials in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] A hydrophobic modifier is added to an n-heptane solution, the mass fraction ratio of octadecyl fatty acid to n-heptane is 1:8, and the reaction is carried out at 20°C and a stirring speed of 500 rpm for 0.5 hour to obtain a hydrophobically modified solution; calcium oxide is added to the prepared hydrophobically modified solution, the mass fraction ratio of calcium oxide to the solution is 5:1, and the reaction is carried out at a temperature of 20°C and a stirring speed of 500 rpm for 18 hours, and the solution is filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed 3 times with n-heptane, and the filtrate is collected, and the filter residue is dried at 40°C and a pressure of 0.1 mbar for 12 hours to obtain hydrophobically modified calcium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0040] The unmodified and hydrophobically modified calcium oxide were pressed into sheets and their water contact angles were tested. Figure 1 As shown, the contact angle is about 145.7°.

[0041] Example 2

[0042] A hydrophobic modifier is added to an n-heptane solution, the mass fraction ratio of propyltrichlorosilane to n-heptane is 1:9, and the mixture is reacted at 25°C and a stirring speed of 400 rpm for 1 hour to obtain a hydrophobically modified solution; calcium oxide is added to the prepared hydrophobically modified solution, the mass fraction ratio of calcium oxide to the solution is 8:1, and the mixture is reacted at a temperature of 25°C and a stirring speed of 400 rpm for 20 hours, filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed 3 times with n-heptane, and the filtrate is collected, and the filter residue is dried at 45°C and a pressure of 0.1 mbar for 16 hours to obtain hydrophobically modified calcium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0043] The obtained hydrophobically modified calcium oxide was pressed into a sheet and its water contact angle was tested. Figure 1 As shown, the contact angle is about 148.5°.

[0044] Example 3

[0045] A hydrophobic modifier is added to an n-heptane solution, the mass fraction ratio of octadecyl fatty acid to n-heptane is 1:10, and the mixture is reacted at 30°C and a stirring speed of 500 rpm for 1 hour to obtain a hydrophobically modified solution; calcium oxide is added to the prepared hydrophobically modified solution, the mass fraction ratio of calcium oxide to the solution is 10:1, and the mixture is reacted at a temperature of 30°C and a stirring speed of 500 rpm for 24 hours, filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed 3 times with n-heptane, and the filtrate is collected, and the filter residue is dried at 50°C and a pressure of 0.1 mbar for 18 hours to obtain hydrophobically modified calcium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0046] The obtained hydrophobically modified calcium oxide was pressed into a sheet and its water contact angle was tested. Figure 1 As shown, the contact angle is about 150.9°.

[0047] Example 4

[0048] A hydrophobic modifier is added to an n-heptane solution, the mass fraction ratio of octadecyl fatty acid methyl ester to n-heptane is 1:8, and the reaction is carried out at 20°C and a stirring speed of 500 rpm for 1 hour to obtain a hydrophobically modified solution; magnesium oxide is added to the prepared hydrophobically modified solution, the mass fraction ratio of calcium oxide to the solution is 5:1, and the reaction is carried out at a temperature of 20°C and a stirring speed of 500 rpm for 12 hours, and the solution is filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed with n-heptane for 3 times, and the filtrate is collected, and the filter residue is dried at 40°C and a pressure of 0.1 mbar for 18 hours to obtain hydrophobically modified magnesium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0049] Unmodified and hydrophobically modified calcium oxide were pressed into sheets and their water contact angles were tested. Figure 2 As shown, the contact angle is about 152.1°.

[0050] Example 5

[0051] A hydrophobic modifier is added to an n-heptane solution, with the mass fraction ratio of octadecyl fatty acid to n-heptane being 1:9, and the mixture is reacted at 25°C and a stirring speed of 400 rpm for 1 hour to obtain a hydrophobically modified solution; magnesium oxide is added to the prepared hydrophobically modified solution, with the mass fraction ratio of calcium oxide to the solution being 6:1, and the mixture is reacted at a temperature of 25°C and a stirring speed of 400 rpm for 16 hours, and the mixture is filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed 3 times with n-heptane, and the filtrate is collected, and the filter residue is dried at 45°C and a pressure of 0.1 mbar for 16 hours to obtain hydrophobically modified magnesium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0052] The obtained hydrophobically modified calcium oxide was pressed into a sheet and its water contact angle was tested. Figure 2As shown, the contact angle is about 153.6°.

[0053] Example 6

[0054] A hydrophobic modifier is added to an n-heptane solution, the mass fraction ratio of ethyltrichlorosilane to n-heptane is 1:10, and the mixture is reacted at 30°C and a stirring speed of 500 rpm for 1 hour to obtain a hydrophobically modified solution; magnesium oxide is added to the prepared hydrophobically modified solution, the mass fraction ratio of calcium oxide to the solution is 7:1, and the mixture is reacted at a temperature of 30°C and a stirring speed of 500 rpm for 18 hours, filtered, and the filtrate and filter residue are collected respectively, the filter residue is washed 3 times with n-heptane, and the filtrate is collected, and the filter residue is dried at 50°C and a pressure of 0.1 mbar for 12 hours to obtain hydrophobically modified magnesium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

[0055] The obtained hydrophobically modified calcium oxide was pressed into a sheet and its water contact angle was tested. Figure 2 As shown, the contact angle is about 148.9°.

[0056] Example 7

[0057] The preparation process of super hydrophobic and mildew-proof mineral putty powder is as follows: Figure 3 As shown, hydrophobically modified calcium oxide, hydrophobically modified magnesium oxide, silicate cement, oxypropyl methyl fiber and inorganic rubber powder are added to the synthesis kettle according to the formula amount, and the various powders are mixed evenly at a stirring speed of 800 rpm and a temperature of 20°C for 20 minutes to obtain a composite powder; functional additives are added to the obtained mixture, and the stirring time is 20 minutes at a stirring rate of 800 rpm and a temperature of 2°C, and the mixture is allowed to stand for 5 minutes to obtain a super hydrophobic and mildew-proof mineral putty powder; the obtained super hydrophobic and mildew-proof mineral putty powder is passed through a 200-mesh sieve and mixed again; the screened super hydrophobic and mildew-proof mineral putty powder is dried at a temperature of 110°C for 3 hours, and then bagged after drying, with a specification of 15kg / bag.

[0058] Table 1 Material formula used in Example 7

[0059]

[0060]

[0061] In the table, the hydrophobically modified calcium oxide is prepared in Example 1, the hydrophobically modified magnesium oxide is prepared in Example 4, and the functional additives are antifreeze agent and thermal insulation agent. The antifreeze agent includes the following raw materials in parts by weight: 5 parts of calcium chloride, 5 parts of sodium pyrophosphate and 5 parts of sodium tripolyphosphate; the thermal insulation agent includes the following raw materials in parts by weight: 6 parts of aluminum oxide and 7 parts of iron oxide.

[0062] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and a water contact angle test was performed after drying. The results are as follows: Figure 4 As shown, the water contact angle is about 154.5°.

[0063] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and the surface was characterized by scanning electron microscopy. The results are as follows: Figure 5 As shown, the surface is relatively smooth and has less pore structure.

[0064] The super hydrophobic and mildew-proof mineral putty powder prepared in this example was subjected to an air permeability test, and the experimental result was 1026 g m -2 day -1 .

[0065] According to JG / T 157-2009, the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface to test the degree of cracking, and the result was 0.18.

[0066] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment is mixed with water and ethanol and stirred evenly, the mass ratio of the three is 1:0.3:0.05, the mixture is used to apply to the wall surface, and after a period of time after the application, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is sprinkled with water. After the watering treatment is completed, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is placed in an airy place for 3 days. After 3 days of ventilation, the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder is measured.

[0067] The test results of the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment are shown in Table 2.

[0068] Table 2 Anti-mildew test results of super hydrophobic anti-mildew mineral putty powder prepared in Example 7

[0069] Rhizopus content Aspergillus niger content Penicillium content Trichoderma content 0.03% 0.02% 0.01% 0.007%

[0070] Example 8

[0071] The preparation process of super hydrophobic and mildew-proof mineral putty powder is as follows: Figure 3As shown, hydrophobically modified calcium oxide, hydrophobically modified magnesium oxide, silicate cement, oxypropyl methyl fiber and inorganic rubber powder are added to the synthesis kettle according to the formula, and the various powders are evenly mixed at a stirring speed of 1000 rpm and a temperature of 25°C for 15 minutes to obtain a composite powder; functional additives are added to the obtained mixture, and the stirring time is 15 minutes at a stirring rate of 1000 rpm and a temperature of 25°C. The mixture is allowed to stand for 5 minutes to obtain a super hydrophobic and mildew-proof mineral putty powder; the obtained super hydrophobic and mildew-proof mineral putty powder is mixed again through a 250-mesh sieve; the screened super hydrophobic and mildew-proof mineral putty powder is dried at a temperature of 105°C for 5 hours, and then bagged after drying, with a specification of 20kg / bag.

[0072] Table 3 Material formula used in Example 8

[0073] Hydrophobically modified calcium oxide 29 servings Hydrophobically modified magnesium oxide 68 servings Hydrophobic fumed nanosilica 5 servings Portland cement 36 servings Oxypropyl Methyl Fiber 0.2 parts Inorganic rubber powder 0.9 parts Functional additives 0.08 Deionized water 65 servings Ethanol 8 servings

[0074] In the table, the hydrophobically modified calcium oxide is prepared in Example 2, the hydrophobically modified magnesium oxide is prepared in Example 5, and the functional additives are antifreeze agents and inorganic mineral pigments. The antifreeze agent includes the following raw materials in parts by weight: 6 parts of calcium chloride, 6 parts of sodium pyrophosphate and 6 parts of sodium tripolyphosphate; the inorganic mineral pigment includes the following raw materials in parts by weight: 9 parts of cinnabar powder and 9 parts of red clay powder.

[0075] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and a water contact angle test was performed. The results are as follows: Figure 4 As shown, the water contact angle is about 157.2°.

[0076] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and the surface was characterized by scanning electron microscopy. The results are as follows: Figure 5 As shown, the surface has a certain micro-nano composite rough structure and a relatively rich pore structure, which is conducive to air permeability.

[0077] The super hydrophobic and mildew-proof mineral putty powder prepared in this example was subjected to an air permeability test, and the experimental result was 1183 g m ~2 day ~1 .

[0078] According to JG / T 157-2009, the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface to test the degree of cracking, and the result was 0.29.

[0079] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment is mixed with water and ethanol and stirred evenly, the mass ratio of the three is 1:0.3:0.05, the mixture is used to apply to the wall surface, and after a period of time after the application, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is sprinkled with water. After the watering treatment is completed, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is placed in an airy place for 3 days. After 3 days of ventilation, the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder is measured.

[0080] The test results of the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment are shown in Table 4.

[0081] Table 4 Anti-mildew test results of super hydrophobic anti-mildew mineral putty powder prepared in Example 8

[0082] Rhizopus content Aspergillus niger content Penicillium content Trichoderma content 0.02% 0.012% 0.009% 0.005%

[0083] Example 9

[0084] The preparation process of super hydrophobic and mildew-proof mineral putty powder is as follows: Figure 3 As shown, hydrophobically modified calcium oxide, hydrophobically modified magnesium oxide, silicate cement, oxypropyl methyl fiber and inorganic rubber powder are added to the synthesis kettle according to the formula amount, and the mixture is stirred at a stirring speed of 1200 rpm and a temperature of 30°C for 10 hours to mix the various powders evenly to obtain a composite powder; functional additives are added to the obtained mixture, and the mixture is stirred at a stirring rate of 1200 rpm and a temperature of 30°C for 10 minutes, and the mixture is allowed to stand for 5 minutes to obtain a super hydrophobic and mildew-proof mineral putty powder; the obtained super hydrophobic and mildew-proof mineral putty powder is passed through a 250-mesh sieve and mixed again; the screened super hydrophobic and mildew-proof mineral putty powder is dried at a temperature of 100°C for 6 hours, and then bagged after drying, with a specification of 15kg / bag.

[0085] Table 5 Material formula used in Example 9

[0086]

[0087]

[0088] In the table, the hydrophobically modified calcium oxide is prepared in Example 3, the hydrophobically modified magnesium oxide is prepared in Example 6, and the functional additives include an antifreeze agent and an electromagnetic radiation eliminator. The antifreeze agent includes the following raw materials in parts by weight: 7 parts of calcium chloride, 7 parts of sodium pyrophosphate and 7 parts of sodium tripolyphosphate; the electromagnetic radiation eliminator includes the following raw materials in parts by weight: 6 parts of nano-scale silver fibers and 7 parts of conductive powder.

[0089] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and a water contact angle test was performed. The results are as follows: Figure 4 As shown, the water contact angle is about 158.4°.

[0090] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was applied to the wall surface, and the surface was characterized by scanning electron microscopy. The results are as follows: Figure 5 As shown, the surface has a large number of micro-nano composite rough structures and a very rich pore structure, which is conducive to air permeability.

[0091] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment was mixed with water and ethanol and stirred evenly, the mass ratio of the three being 1:0.3:0.05, and then the mixture was subjected to an air permeability test, and the experimental result was 1277 g m -2 day -1 .

[0092] The degree of cracking when the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment is applied on the wall surface is tested according to JG / T 157-2009, and the result is 0.57.

[0093] The super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment is mixed with water and ethanol and stirred evenly, the mass ratio of the three is 1:0.3:0.05, the mixture is used to apply to the wall surface, and after a period of time after the application, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is sprinkled with water. After the watering treatment is completed, the wall coated with the super hydrophobic and mildew-proof mineral putty powder is placed in an airy place for 3 days. After 3 days of ventilation, the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder is measured.

[0094] The test results of the mold content on the wall coated with the super hydrophobic and mildew-proof mineral putty powder prepared in this embodiment are shown in Table 4.

[0095] Table 6 Anti-mildew test results of super hydrophobic anti-mildew mineral putty powder prepared in Example 9

[0096]

[0097]

[0098] Technical personnel should note that although the present invention has been described according to the above specific implementation methods, the inventive concept of the present invention is not limited to this invention, and any modification using the inventive concept will be included in the scope of protection of this patent.

Claims

1. A super hydrophobic and mildew-proof mineral putty powder, characterized in that: The composition of the super hydrophobic and mildew-proof mineral putty powder is, by weight: 22 to 35 parts of hydrophobically modified calcium oxide, 62 to 75 parts of hydrophobically modified magnesium oxide, 0 to 10 parts of hydrophobic fumed nano-silica, 32 to 40 parts of silicate cement, 0.1 to 0.29 parts of oxypropyl methyl fiber, 0.8 to 1.0 parts of inorganic rubber powder, and 0.05 to 0.1 parts of functional additives.

2. A super hydrophobic and mildew-proof mineral putty powder as claimed in claim 1, characterized in that: The preparation of the hydrophobically modified calcium oxide comprises the following steps: S1. preparing a hydrophobic modification solution: adding a hydrophobic modifier to an n-heptane solution, wherein the mass fraction ratio of the hydrophobic modifier to the n-heptane is 1:8-10, and reacting at 20-30° C. and a stirring speed of 200-500 rpm for 0.5-1 hour to obtain a hydrophobic modification solution; S2 Hydrophobic modification of calcium oxide: Add calcium oxide to the prepared hydrophobic modification solution in a mass fraction ratio of calcium oxide to solution of 5 to 10:

1. React at a temperature of 20 to 30°C and a stirring speed of 200 to 500 rpm for 18 to 24 hours. Filter, collect the filtrate and residue separately, wash the residue with n-heptane three times, and collect the filtrate. Dry the residue at 40 to 50°C and a pressure of 0.1 mbar for 12 to 18 hours to obtain hydrophobically modified calcium oxide. The filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

3. A super hydrophobic mildew-proof mineral putty powder as claimed in claim 2, characterized in that, The hydrophobic modifier in S1 is at least one of octadecyl fatty acid, octadecyl fatty acid methyl ester, octadecyl fatty acid ethyl ester, octadecyl fatty acid propyl ester, propyltrichlorosilane and ethyltrichlorosilane.

4. A super hydrophobic mildew-proof mineral putty powder as claimed in claim 1, characterized in that, The preparation of the hydrophobically modified magnesium oxide comprises the following steps: S3: preparing a hydrophobic modification solution: adding a hydrophobic modifier to an n-heptane solution, wherein the mass fraction ratio of the hydrophobic modifier to n-heptane is 1:8-10, and reacting at 20-30° C. and a stirring speed of 200-500 rpm for 0.5-1 hour to obtain a hydrophobic modification solution; S4 Hydrophobic modification of magnesium oxide: Add magnesium oxide to the prepared hydrophobic modification solution in a mass fraction ratio of calcium oxide to solution of 5 to 7:1, react at a temperature of 20 to 30°C and a stirring speed of 200 to 500 rpm for 12 to 18 hours, filter, collect the filtrate and residue separately, wash the residue with n-heptane three times, and collect the filtrate, dry the residue at 40 to 50°C and a pressure of 0.1 mbar for 12 to 18 hours to obtain hydrophobically modified magnesium oxide, and the filtrates collected twice can be mixed and reused as a hydrophobically modified solution.

5. A super hydrophobic mildew-proof mineral putty powder as claimed in claim 4, characterized in that, The hydrophobic modifier in S1 is at least one of octadecyl fatty acid, octadecyl fatty acid methyl ester, octadecyl fatty acid ethyl ester, octadecyl fatty acid propyl ester, propyltrichlorosilane and ethyltrichlorosilane.

6. A super hydrophobic mildew-proof mineral putty powder as claimed in claim 1, characterized in that: The particle size of the hydrophobic fumed silica is 20 to 70 nm.

7. The inorganic mildew-proof mineral putty powder according to claim 1, characterized in that: The functional additive is at least one of an antifreeze agent, a thermal insulation agent, an electromagnetic radiation eliminator and an inorganic mineral pigment. The antifreeze agent includes the following raw materials in parts by weight: 5 to 7 parts of calcium chloride, 5 to 7 parts of sodium pyrophosphate and 5 to 7 parts of sodium tripolyphosphate; the thermal insulation agent includes the following raw materials in parts by weight: 6 to 8 parts of aluminum oxide and 6 to 8 parts of iron oxide; the electromagnetic radiation eliminator includes the following raw materials in parts by weight: 5 to 8 parts of nano-scale silver fibers and 5 to 8 parts of conductive powder; the inorganic mineral pigment includes the following raw materials in parts by weight: 8 to 10 parts of cinnabar powder and 8 to 10 parts of red clay powder.

8. A method for preparing a super hydrophobic and mildew-proof mineral putty powder as claimed in any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: S5: adding hydrophobically modified calcium oxide, hydrophobically modified magnesium oxide, silicate cement, oxypropyl methyl fiber and inorganic rubber powder into the synthesis reactor according to the formula amount, stirring at a speed of 800 to 1200 rpm and a temperature of 20 to 30° C. for 10 to 20 minutes to mix the various powders evenly to obtain a composite powder; S6: adding a functional additive to the mixture obtained by S5, stirring at a rate of 800 to 1200 rpm and a temperature of 20 to 30° C. for 10 to 20 minutes, and standing for 5 minutes to obtain a super hydrophobic and mildew-proof mineral putty powder; S7: The super hydrophobic and mildew-proof mineral putty powder obtained in S6 is mixed again through a 200-250 mesh sieve; S8: Dry the super hydrophobic and mildew-proof mineral putty powder screened in S7 at a temperature of 100 to 110° C. for 3 to 6 hours, and then pack it into bags after drying, with a specification of 15 or 20 kg / bag.

Citation Information

Patent Citations

  • Hydrophobic self-cleaning coating for foam cement insulation board for exterior wall and preparation method thereof

    CN103351768A

  • Preparation method for surface-hydrophobic modified calcium oxide

    CN104893362A

  • Preparation method, application and use method of super-hydrophobic calcium carbonate coating assistant

    CN104962126A

  • Exterior wall water-resistant putty and preparation method thereof

    CN111423759A

  • Inorganic mildew-proof mineral putty

    CN115975427A