High-flexibility anti-torsion watertight cable for robot mechanical arm and manufacturing process method of high-flexibility anti-torsion watertight cable
By adopting a multi-layer structure and specific manufacturing process in the robot arm cable, the problem of insufficient torsion, bending and tensile properties of existing cables in deep water environments is solved, and a highly flexible and watertight cable is achieved to meet the needs of deep water equipment. stringent requirements.
Patent Information
- Application Number
- CN202411045855.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-01
AI Technical Summary
Existing cables used in robot manipulators cannot meet the needs of deepwater equipment in working conditions, especially in terms of torsion, bending and tensile properties.
It adopts highly flexible and torsion-resistant watertight cables, including multi-strand tinned round copper wire stranded conductors injected with rubber adhesive sealant. It is composed of extruded cross-linked rubber elastomer insulation and water-swelling water-blocking aromatic fiber braiding to form a multi-layer structure to improve The cable is flexible and water-tight, and is processed through specific manufacturing process steps such as hot air drying chambers, electron beam irradiation and extruders to ensure high flexibility and durability.
It achieves high flexibility, bending resistance and torsion resistance of the cable, meets stringent torsion and bending life test requirements, and at the same time improves water tightness, can withstand high water pressure and external tension, and is suitable for deep water environments.
Smart Images

Figure CN118737550A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electric wires and cables, in particular to a highly flexible, torsion-resistant, watertight cable for a robot mechanical arm and a manufacturing process method thereof. Background Art
[0002] With the in-depth development of the ocean field, the technical requirements for various deep-water equipment are constantly increasing. As the key components of the power and control systems of underwater equipment, watertight cables are constantly increasing. With the increasing requirements for the systematic characteristics of various equipment, new requirements are also put forward for the matching functional characteristics of the matching watertight cables, such as torsion, bending, tensile and other physical characteristics. The existing cables used in robot manipulators cannot meet the needs of deep-water equipment in working conditions. Summary of the invention
[0003] The technical problem to be solved by the present invention is that the existing cables used in robot manipulators cannot meet the requirements of deep-water equipment in a working state.
[0004] The technical solution adopted by the present invention to solve its technical problems is: a highly flexible, torsion-resistant, watertight cable for a robot mechanical arm, comprising a conductor of multiple strands of tinned round copper wires twisted with rubber adhesive sealant, the conductor is insulated by extruding a cross-linked rubber elastomer to form an insulating core, water-swelling water-blocking aramid fibers are woven outside the insulation to form an insulating tensile layer I, the water-swelling water-blocking aramid rope is used as a central unit and twisted together with the insulating core wire to form a cable, when cabling, the gaps between the core wires are filled with a water-swelling two-component water-blocking adhesive to form a water-blocking sealing layer, a double-sided water-blocking tape is wrapped around the cable core, a cross-linked rubber elastomer inner sheath is extruded outside the double-sided water-blocking tape, a tensile layer II is woven outside the cross-linked rubber elastomer inner sheath with twisted water-swelling water-blocking aramid fibers, and a cross-linked rubber elastomer outer sheath is extruded as the outermost layer.
[0005] Preferably, the rubber adhesive sealant is a solvent-based chloroprene rubber adhesive prepared by a mixing method using non-sulfur-adjusted chloroprene rubber LDJ-231 as a base rubber, with a solid content of 30% to 40% and a viscosity (25° C.) of 15,000 to 20,000 mPa.s.
[0006] Preferably, the water-swellable water-blocking aramid rope is formed by twisting 60 to 100 strands of 3220dtex water-blocking aramid fiber bundles, and the bundle pitch ratio is 25 to 30.
[0007] Preferably, the main components of the water-swellable two-component water-blocking adhesive are about 75% of a two-component silicone base material, about 3% of silicone oil, 5% of a solvent xylene, 10% of an antioxidant, and 7% of cross-linked sodium polyacrylate.
[0008] Preferably, the insulation thickness of the extruded cross-linked rubber elastomer insulation is 0.7-1.2 mm; the sheath thickness of the extruded cross-linked rubber elastomer inner sheath is 1.2-2.0 mm; and the sheath thickness of the extruded cross-linked rubber elastomer outer sheath is 2.0-3.0 mm.
[0009] Preferably, a plurality of lateral elastic support strips arranged in a ring array are provided between the double-sided water-blocking tape and the cross-linked rubber elastic inner sheath, and limiting grooves are provided at both ends of the side walls of the lateral elastic support strips.
[0010] Preferably, the lateral elastic support strips are all disposed at the gaps between adjacent conductors and are arranged along the gaps between adjacent conductors.
[0011] Preferably, the limiting slot faces the inner sheath of the cross-linked rubber elastic body.
[0012] A manufacturing process method for a highly flexible torsion-resistant watertight cable for a robot mechanical arm, the steps of which are as follows: Step 1: twisting multiple strands of tinned round copper wires, and twisting them regularly in a "1+6+12+18" arrangement to obtain a conductor, wherein the outermost layer is twisted in the left direction, and chloroprene rubber adhesive sealant is injected during twisting, so that the adhesive sealant is twisted together with the tinned round copper wire monofilaments to fill the gaps between the tinned round copper wires, and the twisting pitch-to-diameter ratio is controlled at 10 to 12 times, and the pitch tolerance is ±2 mm. After the conductor is twisted, it is placed in a hot air circulation drying room at a temperature of 50±5°C and left to stand for 24 hours.
[0013] Step 2: After drying the cross-linked rubber elastomer insulation material at 65±5°C for 4 hours, inject it into a plastic single-screw extruder to complete the extrusion of the cross-linked rubber elastomer insulation, the extrusion thickness is 0.7-1.2mm, and an insulated wire core is obtained; a low-smoke halogen-free screw CR: 1.2-1.5 is used in the plastic single-screw extruder, and an extrusion mold is an extrusion mold; the temperature of the extruder feed port is set to 130±10°C, the temperature of the extruder head is set to 170±10°C, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to increase in a step-by-step manner; the insulated wire core is discharged from the cooling water tank, and the insulation layer on the insulated wire core is subjected to an online spark test on a power frequency spark tester with a voltage set to 6kV.
[0014] Step 3: subjecting the insulated core wire to electron beam irradiation cross-linking, with an absorbed irradiation dose of 150 to 180 kGy, controlling the elongation of the core wire insulation under load in a thermal extension test to be 30% to 50%, and the permanent deformation to be ≤5%.
[0015] Step 4: Weave a tensile layer with twisted water-swellable aramid fiber outside the insulation. The aramid fiber specification is 300-500dtex, the twist is Tm50-90, and a 16-spindle high-speed braiding machine is used. The upper and lower synchronous braiding is adopted, and the braiding coverage density is 30%-50%.
[0016] Step 5: The water-swellable water-blocking aramid fiber with a specification of 3220 dtex is bundled and twisted in a high-speed twisting machine to obtain a water-swellable water-blocking aramid rope. The aramid rope structure is 60 to 100 strands of 3220 dtex, and the bundle pitch ratio is 25 to 30.
[0017] Step 6: Mix component A and component B of the water-swellable two-component water-blocking adhesive in a ratio of 4:1. Then, when the water-swellable water-blocking aramid rope is used as the central unit and twisted with the insulated core wires into a cable, inject the mixed water-swellable two-component water-blocking adhesive into the parallel line of the cabling mold to fill the gaps between the core wires when the water-swellable two-component water-blocking adhesive is twisted. The cabling method adopts a full back-twist cable twisting with a back-twist rate of 100%, and the cabling pitch-to-pitch ratio is 9 to 11 times, which eliminates the cable twisting stress between the core wires, making the cable soft and resistant to bending, and with high overall watertight safety.
[0018] Step 7: Wrap a layer of double-sided water-blocking tape around the cable core to form a tape layer, with an overlap rate of 15% to 30%.
[0019] Step 8: After the cable wrapping is completed, place the cable core in a hot air circulation oven at 50±5℃ for 24 hours to allow the water-swelling two-component sealant in the cable core to fully cross-link and cure, and completely release the cable stress inside the cable core to ensure the high flexibility of the cable.
[0020] Step 9: Place the lateral elastic support strips with the limiting slots facing outwards, tightly against the outside of the double-sided water-blocking tape, at the gaps on both sides of the conductor. Then, dry the cross-linked rubber elastomer insulating material at 65±5°C for 4 hours and inject it into a plastic single-screw extruder to complete the extrusion of the inner sheath of the cross-linked rubber elastomer. The extrusion thickness is 1.2-2.0 mm. A low-smoke halogen-free screw CR: 1.2-1.5 is used in the plastic single-screw extruder, and an extrusion die is used for the extrusion mold. The temperature of the extruder feed port is set to 130±10°C, and the temperature of the extruder head is set to 175±10°C. The temperature of the screw heating zone between the extruder feed port and the extruder head is set to a step-by-step increase.
[0021] Step 10: A tensile layer is braided on the outside of the inner sheath with twisted water-swellable aramid fiber. The aramid fiber specification is 1610-3220dtex, the twist is Tm50-90, and a 24-spindle high-speed braiding machine is used. The upper and lower synchronous braiding is adopted, and the braiding coverage density is 30%-50%.
[0022] Step 11: After drying the cross-linked rubber elastomer sheath material at 65±5°C for 4 hours, inject it into a plastic single-screw extruder to complete extrusion of the cross-linked rubber elastomer outer sheath, and the extrusion thickness is 2.0~3.0m; in the plastic single-screw extruder, a low-smoke halogen-free screw CR: 1.2~1.5 is used, and an extrusion mold is an extrusion mold. The temperature of the extruder feed port is set to 120±10°C, the temperature of the extruder head is set to 175±10°C, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to a step-by-step increase.
[0023] Step 12: subjecting the cable to electron beam irradiation, with an absorbed irradiation dose of 150 to 180 kGy, an elongation of the outer sheath under a thermal elongation test load of 20% to 40%, and a permanent deformation rate of 0% to 5%.
[0024] The beneficial effects of the present invention are:
[0025] (1) The cable of the present invention is highly flexible, resistant to bending and torsion: the cable conductors and the core wires are twisted and placed in a 50°C high-temperature oven for 24 hours. The high-temperature heat treatment process can fully release the torsion stress inside the conductor and the cable core during the twisting process, so that after the cable sheath is extruded, the internal cable core has no twisting stress, ensuring that the cable has higher flexibility and better torsion and bending resistance, meeting the special technical requirements of ±180° torsion life test of 10 million times and bending life test of 20 million times;
[0026] (2) By improving the common water-blocking sealing materials, the longitudinal water pressure resistance of the cable is improved. First, a new environmentally friendly solvent rubber adhesive is used in the cable conductor sealant. The non-volatile solid content of the sealing adhesive is 30% to 40%, and the viscosity (25°C / mpa.s) is 18,000, so that the filling between the conductor filaments is more dense and the water tightness of the insulated core conductor is improved; a new type of water-swelling two-component sealing filling paste is used in the cable core twisting. By improving the formula of the traditional similar water-blocking paste, the main components are improved to be about 75% of the two-component silicone base material, about 3% of silicone oil, 5% of the solvent xylene, 10% of the antioxidant, and 7% of the cross-linked sodium polyacrylate. Through the optimization, improvement and innovation of different water-blocking sealing pastes in different processes, the watertight reliability of the cable is higher. This product can withstand the underwater water pressure of 7.0MPa without leakage in the vertical and horizontal directions;
[0027] (3) The cable center unit is made of aramid rope obtained by twisting aramid fiber bundles, which has high-strength load-bearing capacity, ensuring that the cable is safe and reliable in the longitudinal load-bearing tension. After the outer sheath is extruded, the inner and outer sheaths form an integral structure. The twisted water-swellable aramid fiber braided layer between the inner and outer sheaths significantly improves the overall tensile strength of the cable. Through this process optimization, the tensile strength of the cable is also greatly improved after the assembly and vulcanization of the components, meeting the external navigation tension of the underwater vehicle during navigation. This product works normally under a tensile force of 10kN, and the breaking force is greater than 20kN. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0029] Figure 1 It is a structural schematic diagram of the present invention.
[0030] Figure 2 It is an internal cross-sectional view of the present invention.
[0031] Figure 3 It is a structural schematic diagram of the lateral elastic support strip in the present invention.
[0032] Numbers in the figure: 1. Conductor, 2. Cross-linked rubber elastomer insulation, 3. Water-swellable water-blocking aramid fiber, 4. Water-swellable water-blocking aramid rope, 5. Gap forming water-blocking sealing layer, 6. Double-sided water-blocking tape, 7. Cross-linked rubber elastomer inner sheath, 8. Twisted water-swellable water-blocking aramid fiber braiding, 9. Cross-linked rubber elastomer outer sheath, 10. Lateral elastic support strip, 11. Limiting slot. DETAILED DESCRIPTION
[0033] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, which only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0034] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0035] like Figure 1 , Figure 2 and Figure 3As shown, the structure of the highly flexible and torsion-resistant watertight cable for the robot mechanical arm of this embodiment is set as follows: a conductor 1 of multiple strands of tinned round copper wires injected with rubber adhesive sealant, a cross-linked rubber elastomer insulation 2 is extruded on the conductor 1 to form an insulating wire core, and a water-swelling water-blocking aramid fiber 3 is woven outside the insulation to form an insulating tensile layer I, a water-swelling water-blocking aramid rope 4 is used as a central unit and twisted together with the insulating core wire to form a cable, and when cabling, the gaps between the core wires are filled with a water-swelling two-component water-blocking adhesive to form a water-blocking sealing layer 5, a double-sided water-blocking tape 6 is wrapped around the cable core, a cross-linked rubber elastomer inner sheath 7 is extruded outside the double-sided water-blocking tape 6, and a twisted water-swelling water-blocking aramid fiber is woven outside the cross-linked rubber elastomer inner sheath 7 to form a tensile layer II, and a cross-linked rubber elastomer outer sheath 8 is extruded as the outermost layer to form a final finished cable.
[0036] In a specific implementation, the conductor 1 of multiple strands of tinned round copper wires injected with rubber adhesive sealant is made of 37 strands of tinned soft copper wires, which are regularly twisted in the arrangement of "1+6+12+18", and the outermost layer is twisted to the left. During the twisting, chloroprene rubber adhesive sealant is injected to make the adhesive sealant and the tinned round copper wire monofilaments twisted together to fill the gaps between the tinned round copper wires. The twisting pitch-to-diameter ratio is controlled at 10 to 12 times. After the conductor is twisted, it is placed in a hot air circulation drying room at a temperature of 50±5°C and left to stand for 24 hours. A cross-linked rubber elastomer is used for extruded insulation 2, and the thickness of the extrusion is 0.7 to 1.2 mm. A twisted water-swelling aramid fiber is used to weave a tensile layer 3 outside the insulation 2, and the weaving coverage density is 30% to 50%. The water-swellable water-blocking aramid fiber with a specification of 3220dtex is bundled and twisted in a high-speed stranding machine to obtain a water-swellable water-blocking aramid rope 4, the aramid rope structure is 60 to 100 strands of 3220dtex, and the bundle pitch ratio is 25 to 30. When the water-swellable water-blocking aramid rope 4 is used as a central unit and twisted with an insulating core wire to form a cable, a water-swellable two-component water-blocking adhesive 5 after mixing and proportioning is injected at the paralleling point of the cable forming mold to fill the gap between the core wires, and a double-sided water-blocking tape 6 is overlapped and wrapped outside the cable core to form a tape layer, and the wrapping coverage rate is 15% to 30%; after the cable wrapping is completed, the cable core is placed in a hot air circulation drying room at a temperature of 50±5℃ and left to stand for 24 hours; a cross-linked rubber elastic body is used to extrude an inner sheath 7, and the extrusion thickness is 1.2 to 2.0mm; a tensile layer is woven with twisted water-swellable aramid fiber 8 outside the cross-linked rubber elastic body extruded inner sheath 7, and the weaving coverage density is 30% to 50%. The outer sheath 9 is extruded by a cross-linked rubber elastic body with a thickness of 2.0-3.0 mm. The cable is irradiated with an electron beam with an absorbed radiation dose of 150-180 kGy. The outer sheath has an elongation of 20%-40% under a thermal extension test load and a permanent deformation rate of 0%-5%.
[0037] The manufacturing process of the highly flexible anti-torsion watertight cable for the robot mechanical arm in this embodiment is carried out in the following steps:
[0038] Step 1: Use multiple strands of tinned round copper wires to twist, and twist them in a regular manner according to the arrangement of "1+6+12+18" to obtain a conductor. The outermost layer is twisted to the left. During the twisting, inject chloroprene rubber adhesive sealant to make the adhesive sealant twisted together with the tinned round copper wire monofilaments to fill the gaps between the tinned round copper wires. The twisting pitch-to-diameter ratio is controlled at 10 to 12 times, and the pitch tolerance is ±2mm. After the conductor is twisted, place it in a hot air circulation oven at 50±5℃ for 24 hours.
[0039] Step 2: After drying the cross-linked rubber elastomer insulation material at 65±5℃ for 4 hours, inject it into a plastic single-screw extruder to complete the extrusion of the cross-linked rubber elastomer insulation 2, with an extrusion thickness of 0.7-1.2mm, to obtain an insulated wire core; a low-smoke halogen-free screw CR: 1.2-1.5 is used in the plastic single-screw extruder, and an extrusion mold is an extrusion mold; the temperature of the extruder feed port is set to 130±10℃, the temperature of the extruder head is set to 170±10℃, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to increase in a step-by-step manner; the insulated wire core is discharged from the cooling water tank, and the insulation layer on the insulated wire core is subjected to an online spark test on a power frequency spark tester with a voltage set to 6kV.
[0040] Step 3: subjecting the insulated core wire to electron beam irradiation cross-linking, with an absorbed irradiation dose of 150 to 180 kGy, controlling the elongation of the core wire insulation under load in a thermal extension test to be 30% to 50%, and the permanent deformation to be ≤5%.
[0041] Step 4: Weave a tensile layer with twisted water-swellable aramid fiber 3 outside the insulation. The aramid fiber specification is 300-500dtex, the twist is Tm50-90, and a 16-spindle high-speed braiding machine is used. The upper and lower synchronous braiding is adopted, and the braiding coverage density is 30%-50%.
[0042] Step 5: The water-swellable water-blocking aramid fiber with a specification of 3220 dtex is bundled and twisted in a high-speed twisting machine to obtain a water-swellable water-blocking aramid rope. The aramid rope structure is 60 to 100 strands of 3220 dtex, and the bundle pitch ratio is 25 to 30.
[0043] Step 6: Mix component A and component B of the water-swellable two-component water-blocking adhesive in a ratio of 4:1. Then, when the water-swellable water-blocking aramid rope 4 is used as the central unit and twisted with the insulated core wires into a cable, inject the mixed water-swellable two-component water-blocking adhesive at the paralleling point of the cabling mold to fill the gaps between the core wires when the water-swellable two-component water-blocking adhesive is twisted. The cabling method adopts a full back-twist cable twisting with a back-twist rate of 100%, and the cabling pitch-to-pitch ratio is 9 to 11 times, which eliminates the cable twisting stress between the core wires, making the cable soft and resistant to bending, and having high overall watertight safety.
[0044] Step 7: Wrap a layer of double-sided water-blocking tape around the cable core to form a tape layer, with an overlap rate of 15% to 30%.
[0045] Step 8: After the cable wrapping is completed, place the cable core in a hot air circulation oven at 50±5℃ for 24 hours to allow the water-swelling two-component sealant in the cable core to fully cross-link and cure, and completely release the cable stress inside the cable core to ensure the high flexibility of the cable.
[0046] Step 9: Place the lateral elastic support strip 10 with the limiting slot 11 facing outward, close to the outside of the double-sided water-blocking tape 6, located in the gap position on both sides of the conductor 1, and then dry the cross-linked rubber elastomer insulating material at 65±5°C for 4 hours and inject it into the plastic single-screw extruder to complete the extrusion of the cross-linked rubber elastomer inner sheath 7, with an extrusion thickness of 1.2 to 2.0 mm; a low-smoke halogen-free screw CR: 1.2 to 1.5 is used in the plastic single-screw extruder, and an extrusion die is used for the extrusion mold; the temperature of the extruder feed port is set to 130±10°C, the temperature of the extruder head is set to 175±10°C, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to a step-by-step increase.
[0047] Step 10: Weave a tensile layer with twisted water-swellable aramid fiber 8 outside the cross-linked rubber elastomer inner sheath 7, the aramid fiber specification is 1610-3220dtex, the twist is Tm50-90, a 24-spindle high-speed braiding machine is used, upper and lower synchronous braiding is adopted, and the braiding coverage density is 30%-50%.
[0048] Step 11: After drying the cross-linked rubber elastomer sheath material at 65±5°C for 4 hours, inject it into a plastic single-screw extruder to complete extrusion of the cross-linked rubber elastomer outer sheath 9, and the extrusion thickness is 2.0-3.0 mm; in the plastic single-screw extruder, a low-smoke halogen-free screw CR: 1.2-1.5 is used, an extrusion mold is an extrusion mold, the extruder feed port temperature is set to 130±10°C, the extruder head temperature is set to 175±10°C, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to a step-by-step increase.
[0049] Step 12: The cable is subjected to electron beam irradiation, the irradiation absorbed dose is 150-180 kGy, the elongation of the cross-linked rubber elastic outer sheath 9 under the heat extension test load is 20%-40%, and the permanent deformation rate is 0%-5%.
[0050] The structure and performance indicators of the highly flexible anti-torsion watertight cable for the robot mechanical arm of the present invention are listed in Table 1:
[0051]
[0052] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A highly flexible, torsion-resistant, watertight cable for a robot manipulator, comprising a conductor (1) of multiple strands of tinned round copper wires twisted together and injected with a rubber adhesive sealant, characterized in that: The conductor (1) is formed by extruding a cross-linked rubber elastic insulation (2) to form an insulating wire core, and a water-swelling water-blocking aramid fiber (3) is braided outside the insulation to form an insulating tensile layer I. The water-swelling water-blocking aramid rope (4) is used as a central unit and twisted together with the insulating core wire to form a cable. When forming the cable, the gaps between the core wires are filled with a water-swelling two-component water-blocking adhesive to form a water-blocking sealing layer (5). A double-sided water-blocking tape (6) is wrapped around the cable core, and a cross-linked rubber elastic inner sheath (7) is extruded outside the double-sided water-blocking tape (6). The cross-linked rubber elastic inner sheath (7) is braided with twisted water-swelling water-blocking aramid fiber (8) to form a tensile layer II. The outermost layer is extruded as a cross-linked rubber elastic outer sheath (9).
2. The highly flexible, torsion-resistant, watertight cable for a robot manipulator according to claim 1 is characterized by: The rubber adhesive sealant is a solvent-type chloroprene rubber adhesive prepared by a mixing method using non-sulfur-adjusted chloroprene rubber LDJ-231 as a base rubber, with a solid content of 30% to 40% and a viscosity (25° C.) of 15000 to 20000 mpa.s.
3. The highly flexible anti-torsion watertight cable for a robot manipulator according to claim 1 is characterized by: The water-swellable water-blocking aramid rope is formed by twisting 60 to 100 strands of 3220dtex water-blocking aramid fiber bundles, and the bundle pitch-to-diameter ratio is 25 to 30.
4. The highly flexible anti-torsion watertight cable for a robot manipulator according to claim 1 is characterized by: The main components of the water-swellable two-component water-blocking adhesive are about 75% of a two-component silicone base material, about 3% of silicone oil, 5% of a solvent xylene, 10% of an antioxidant, and 7% of cross-linked sodium polyacrylate.
5. The highly flexible anti-torsion watertight cable for a robot manipulator according to claim 1 is characterized by: The insulation thickness of the extruded cross-linked rubber elastic body insulation (2) is 0.7-1.2 mm; the sheath thickness of the extruded cross-linked rubber elastic body inner sheath (7) is 1.2-2.0 mm; and the sheath thickness of the extruded cross-linked rubber elastic body outer sheath (9) is 2.0-3.0 mm.
6. The highly flexible anti-torsion watertight cable for a robot manipulator according to claim 1 is characterized by: A plurality of lateral elastic support strips (10) arranged in a ring array are provided between the double-sided water-blocking tape (6) and the cross-linked rubber elastic inner sheath (7), and both ends of the side walls of the lateral elastic support strips (10) are provided with limit slots (11).
7. A highly flexible, torsion-resistant, watertight cable for a robot manipulator according to claim 6, characterized in that: The lateral elastic support strips (10) are all arranged at the gaps between adjacent conductors and are arranged along the gaps between adjacent conductors.
8. The highly flexible anti-torsion watertight cable for a robot manipulator according to claim 6 is characterized by: The limiting groove (11) faces the inner sheath (7) of the cross-linked rubber elastic body.
9. A manufacturing process for a highly flexible torsion-resistant watertight cable for a robot manipulator, characterized in that: The steps are as follows: Step 1: Use multiple strands of tinned round copper wires to twist them in a regular manner according to the arrangement of "1+6+12+18" to obtain a conductor (1), wherein the outermost layer is twisted in the left direction. During the twisting process, chloroprene rubber adhesive sealant is injected to allow the adhesive sealant to be twisted together with the tinned round copper wire monofilaments to fill the gaps between the tinned round copper wires. The twisting pitch-to-diameter ratio is controlled to be 10 to 12 times, and the pitch tolerance is ±2 mm. After the conductor is twisted, it is placed in a hot air circulation drying room at a temperature of 50±5°C and left to stand for 24 hours. Step 2: drying the cross-linked rubber elastic insulation material at 65±5°C for 4 hours and then injecting it into a plastic single-screw extruder to complete the extrusion of the cross-linked rubber elastic insulation (2), the extrusion thickness of which is 0.7 to 1.2 mm, to obtain an insulated wire core; using a low-smoke halogen-free screw CR in the plastic single-screw extruder: 1.2~1.5, the extrusion die adopts an extrusion die; the temperature of the extruder discharge port is set to 130±10℃, the temperature of the extruder head is set to 170±10℃, and the temperature of the screw heating zone between the extruder discharge port and the extruder head is set to increase in a step-by-step manner; the insulated wire core is discharged from the cooling water tank and passed through an industrial frequency spark tester with a voltage set to 6kV to conduct an online spark test on the insulation layer on the insulated wire core. Step 3: subjecting the insulated core wire (2) to electron beam irradiation cross-linking, with an absorbed irradiation dose of 150 to 180 kGy, and controlling the elongation of the core wire insulation under load in a thermal extension test to be 30% to 50%, and the permanent deformation to be ≤5%. Step 4: Weave a tensile layer with twisted water-swellable aramid fiber (3) outside the insulation (2), the aramid fiber specification is 300-500 dtex, the twist Tm is 50-90, a 16-spindle high-speed braiding machine is used, upper and lower synchronous braiding is adopted, and the braiding coverage density is 30%-50%. Step 5: The water-swellable water-blocking aramid fiber with a specification of 3220 dtex is bundled and twisted in a high-speed twisting machine to obtain a water-swellable water-blocking aramid rope (4). The aramid rope structure is 60 to 100 strands of 3220 dtex, and the bundle pitch ratio is 25 to 30. Step 6: Mix component A and component B of the water-swellable two-component water-blocking adhesive in a ratio of 4:
1. Then, when the water-swellable water-blocking aramid rope is used as a central unit and twisted with the insulated core wires to form a cable, inject the mixed water-swellable two-component water-blocking adhesive (5) at the paralleling point of the cabling mold, so that the water-swellable two-component water-blocking adhesive (5) fills the gaps between the core wires when twisting. The cabling method adopts a full back-twist cable twisting with a back-twist rate of 100%, and the cabling pitch-to-pitch ratio is 9 to 11 times, so as to eliminate the cable twisting stress between the core wires, so that the cable has good flexibility, bending resistance, and high overall watertight safety. Step 7: wrap a layer of double-sided water-blocking tape (6) around the cable core to form a tape layer, with an overlap rate of 15% to 30%. Step 8: After the cable wrapping is completed, place the cable core in a hot air circulation oven at 50±5℃ for 24 hours to allow the water-swelling two-component sealant in the cable core to fully cross-link and cure, and completely release the cable stress inside the cable core to ensure the high flexibility of the cable. Step 9: The lateral elastic support strip (10) is then arranged closely on the outside of the double-sided water-blocking tape (6) with the limiting groove (11) facing outward, located in the gap position on both sides of the conductor (1), and then the cross-linked rubber elastomer insulating material is dried at 65±5°C for 4 hours and injected into a plastic single-screw extruder to complete the extrusion of the cross-linked rubber elastomer inner sheath (7), and the extrusion thickness is 1.2-2.0 mm; a low-smoke halogen-free screw CR: 1.2-1.5 is used in the plastic single-screw extruder, and an extrusion die is used; the temperature of the extruder feed port is set to 130±10°C, the temperature of the extruder head is set to 175±10°C, and the temperature of the screw heating zone between the extruder feed port and the extruder head is set to increase in a step-by-step manner. Step 10: Weaving a tensile layer with twisted water-swellable aramid fiber (8) outside the cross-linked rubber elastic body sheath (7), the aramid fiber specification is 1610-3220dtex, the twist is Tm50-90, using a 24-spindle high-speed braiding machine, upper and lower synchronous braiding, and the braiding coverage density is 30%-50%. Step 11: After drying the cross-linked rubber elastomer sheath material at 65±5°C for 4 hours, inject it into a plastic single-screw extruder to complete extrusion of the cross-linked rubber elastomer outer sheath (9), and the extrusion thickness is 2.0~3.0m; in the plastic single-screw extruder, a low-smoke halogen-free screw CR: 1.2~1.5 is used, and an extrusion die is an extrusion die. The extruder feed port temperature is set to 120±10°C, the extruder head temperature is set to 175±10°C, and the screw heating zone between the extruder feed port and the extruder head is set to a step-by-step increase in temperature. Step 12: subjecting the cable to electron beam irradiation, with an absorbed irradiation dose of 150 to 180 kGy, an elongation of the outer sheath under a thermal elongation test load of 20% to 40%, and a permanent deformation rate of 0% to 5%.