Solid electrolytic capacitor element, solid electrolytic capacitor, and method for manufacturing solid electrolytic capacitor element
By using a resin composition with a high content of insulating resin material modified additives in the solid electrolytic capacitor to fill the pores and form an insulating area with a high glass transition temperature, the leakage current problem caused by the low filling rate of the resin material is solved, and a more stable electrolytic capacitor is achieved. Good insulation and capacitor performance.
Patent Information
- Application Number
- CN202380022774.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-25
- Filing Date
- 2023-02-20
- Publication Date
- 2024-10-01
AI Technical Summary
The filling rate of resin material in the insulation area of existing solid electrolytic capacitors is low, causing conductive materials to invade the insulation area and increase leakage current.
A resin composition containing more than 3% of insulating resin material-modifying additives is used to fill the pores of the porous part to form an insulating region of the cured product with a high glass transition temperature, thereby suppressing the intrusion of conductive materials.
Effectively reduce leakage current, ensure the insulation between the anode and cathode parts, and improve the initial capacity and electrical impedance performance of the capacitor.
Smart Images

Figure CN118742988A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a solid electrolytic capacitor element and a solid electrolytic capacitor, and a method for manufacturing the solid electrolytic capacitor element. Background Art
[0002] A solid electrolytic capacitor comprises, for example, a solid electrolytic capacitor element and an outer casing that seals the solid electrolytic capacitor element. A solid electrolytic capacitor element comprises, for example, an anode foil, a dielectric layer formed on the surface of the anode foil, and a cathode portion comprising a solid electrolyte layer covering at least a portion of the dielectric layer. From the perspective of ensuring high capacity, a porous portion having a plurality of pores is formed on the surface layer of the anode foil. The anode foil is divided into a first portion including a first end and a second portion including a second end on the opposite side of the first end, and sometimes an insulating region is provided at a predetermined position between the first end and the second end. By means of the insulating region, when the cathode portion is formed on the second portion of the anode foil through the dielectric layer, insulation between the first portion and the cathode portion can be ensured. The insulating region is formed, for example, by attaching an insulating sheet to the surface of the dielectric layer or by filling an insulating material in the pores of the porous portion.
[0003] Patent document 1 proposes a solid electrolytic capacitor having a shielding layer in a region separating an anode region and a cathode region of a solid electrolytic capacitor substrate having a porous layer on its surface, characterized in that the shielding layer is formed by a solution or dispersion of a heat-resistant resin or its precursor in which the content of a shielding layer modifying additive (excluding a silane coupling agent) is 0 to 0.1% by mass (based on the mass of the heat-resistant resin or its precursor).
[0004] Patent document 2 proposes a solid electrolytic capacitor, characterized in that the solid electrolytic capacitor has a shielding layer formed by stacking multiple layers in an area separating the anode area and the cathode area of a solid electrolytic capacitor substrate having a porous layer on the surface, and the first shielding layer directly stacked on the solid electrolytic capacitor substrate in the stacked shielding layers is formed by a solution or dispersion of a heat-resistant resin or its precursor that does not contain a shielding layer modifying additive (except a silane coupling agent) or contains the shielding layer modifying additive in an amount of 0.1% by mass or less (based on the mass of the heat-resistant resin or its precursor).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2007 / 061005
[0008] Patent Document 2: International Publication No. 2008 / 038584 Summary of the invention
[0009] Problem that the invention aims to solve
[0010] When an insulating region is formed by filling an insulating resin material (resin composition, etc.) into the pores of the porous portion and curing it, it is difficult to fill the resin material to a high degree because the pores are small. If the filling rate of the resin material in the pores of the porous portion is low, when the solid electrolyte layer is formed in the second portion, a conductive material such as a conductive polymer constituting the solid electrolyte layer invades the pores of the insulating region or invades the first portion through the pores. Therefore, it is difficult to ensure insulation between the cathode portion including the solid electrolyte layer and the first portion, and the leakage current increases.
[0011] Solutions for solving problems
[0012] A first aspect of the present disclosure relates to a solid electrolytic capacitor element comprising:
[0013] An anode foil having a porous portion on a surface layer, and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion;
[0014] a dielectric layer formed on a surface of the porous portion; and
[0015] a solid electrolyte layer covering at least a portion of the dielectric layer,
[0016] The solid electrolytic capacitor element includes an insulating region including a cured product of a resin composition between the first end and the second end of the anode foil.
[0017] In the insulating region, the solidified material fills the pores of the porous portion.
[0018] The resin composition comprises an insulating resin material and an additive for modifying the insulating resin material.
[0019] The content of the additive in the resin composition is 3% by mass or more,
[0020] The glass transition temperature of the cured product is 230° C. or higher.
[0021] A second aspect of the present disclosure relates to a solid electrolytic capacitor comprising at least one solid electrolytic capacitor element as described above.
[0022] A third aspect of the present disclosure relates to a method for manufacturing a solid electrolytic capacitor element, comprising:
[0023] The first step is to prepare an anode foil having a porous portion on a surface layer and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion;
[0024] A second step of forming a dielectric layer on the surface of the porous portion;
[0025] a third step of forming an insulating region including a cured product of a resin composition between the first end portion and the second end portion of the anode foil; and
[0026] In a fourth step, a solid electrolyte layer is formed, wherein the solid electrolyte layer covers at least a portion of the dielectric layer.
[0027] The resin composition comprises an insulating resin material and an additive for modifying the insulating resin material, the content of the additive in the resin composition is 3% by mass or more, and the glass transition temperature of the cured product is 230° C. or more.
[0028] The third step includes a sub-step of filling the pores of the porous portion with a treatment liquid containing the resin composition and a solvent and curing the resin composition.
[0029] Effects of the Invention
[0030] In a solid electrolytic capacitor having an insulating region including a cured product of an insulating resin material, leakage current can be suppressed to a low level. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 1 is a cross-sectional view schematically showing a solid electrolytic capacitor according to a first embodiment of the present disclosure.
[0032] Figure 2 It is schematically shown Figure 1 A cross-sectional view of a solid electrolytic capacitor element contained in a solid electrolytic capacitor. DETAILED DESCRIPTION
[0033] The novel features of the present invention are described in the appended claims, and the present invention relates to both structure and content. Together with other objects and features of the present invention, they can be better understood through the following detailed description with reference to the accompanying drawings.
[0034] In the case of forming an insulating region, if the resin composition as the constituent material of the insulating region cannot be highly filled in the pores of the porous part formed on the surface layer of the anode foil and there are many gaps left, when forming the solid electrolyte layer, the conductive material such as the conductive polymer will also invade the gaps in the insulating region. In addition, sometimes the conductive material will also invade the first part (anode part) through the gaps in the insulating region. In these cases, the anode part and the cathode part including the solid electrolyte layer are connected through the conductive material invading the gaps in the insulating region or the gaps in the anode part, and the leakage current becomes large. The solid electrolyte layer is formed, for example, by in situ polymerization such as chemical polymerization or electrolytic polymerization, or by using a liquid composition containing a conductive polymer (conjugated polymer and dopant, etc.). In particular, when the solid electrolyte layer is formed by in situ polymerization, since the polymerization liquid contains relatively low molecular weight components (precursors, dopants and oxidants of conjugated polymers, etc.), it is easy to penetrate into the pores or the above-mentioned gaps. In addition, when the solid electrolyte layer is formed by electrolytic polymerization, sometimes the conductive material is pre-coated before electrolytic polymerization. The liquid dispersion (liquid composition) containing the conductive material used in the pre-coating has a low concentration and low viscosity, and is also easy to invade the gaps in the insulating region or the anode portion. Therefore, in order to reduce the invasion of these conductive materials, it is important to highly fill the pores of the porous portion with the resin composition (or its cured product) when forming the insulating region.
[0035] In order to fill the pores of the porous part highly, it is important that the dry solid content concentration of the treatment liquid containing the resin composition for forming the insulating region is high. However, when the dry solid content concentration of the treatment liquid is high, there is a tendency for the viscosity to increase. In particular, when the glass transition temperature (Tg) of the solidified material is high, the viscosity tends to increase significantly. When the viscosity of the treatment liquid is high, the filling property into the pores of the porous part decreases. When a solvent is used to reduce the viscosity of the treatment liquid, the dry solid content concentration of the treatment liquid becomes low. Since the pores of the porous part are fine, even if a treatment liquid with a low dry solid content concentration is repeatedly applied to the porous part, the opening part of the pores is easily clogged in the initial stage, making it difficult to fill in deep. Therefore, it is also difficult to improve the filling property of the resin composition into the pores in this case.
[0036] In view of the above, (1) the solid electrolytic capacitor element disclosed in the present invention includes: an anode foil having a porous portion on the surface layer, and having a first portion including a first end and a second portion including a second end on the opposite side of the first end; a dielectric layer formed on the surface of the porous portion; and a solid electrolyte layer covering at least a portion of the dielectric layer. The solid electrolytic capacitor element has an insulating region containing a cured product of a resin composition between the first end and the second end of the anode foil. In the insulating region, the cured product is filled in the pores of the porous portion. The resin composition contains an insulating resin material and an additive that modifies the insulating resin material. The content of the additive in the resin composition is 3% by mass or more. The glass transition temperature of the cured product is 230° C. or more.
[0037] Thus, in the solid electrolytic capacitor element of the present disclosure, an insulating region is formed using a resin composition containing an insulating resin material and an additive that modifies the insulating resin material. The insulating region contains a cured product of such a resin composition. Here, the content of the additive in the resin composition is 3% by mass or more, and the Tg of the cured product is 230°C or more. In the solid electrolytic capacitor element, in the insulating region, the cured product of such a resin composition is filled in the pores of the porous portion. In the case where the Tg of the cured product is in a high range of 230°C or more, the viscosity of the treatment liquid containing the resin composition for forming the insulating region tends to increase, but by using an additive that modifies the insulating resin material at 3% by mass or more, the viscosity can be suppressed to a low level while maintaining a high dry solid content concentration of the treatment liquid, and the filling property of the resin composition into the pores of the porous portion can be improved. In the insulating region, since the insulating cured product is highly filled in the pores of the porous portion, the intrusion of the conductive material into the voids of the insulating region is suppressed when the solid electrolyte layer is formed. Therefore, the insulation between the first part (anode part) and the cathode part including the solid electrolyte layer can be more reliably ensured. As a result, the leakage current can be reduced. In addition, in the present disclosure, the initial high capacity can be ensured, and the initial tanδ and equivalent series resistance (ESR) can be suppressed to a low level, and excellent capacitor performance can also be ensured.
[0038] (2) In the above (1), the viscosity of a γ-butyrolactone solution of the resin composition containing the resin composition at a concentration of 30% by mass at 25° C. may be 1,000 mPa·s or more and 10,000 mPa·s or less.
[0039] (3) In the above (1) or (2), the content of the additive in the resin composition may be 60% by mass or less.
[0040] (4) In any one of the above (1) to (3), the additive may interact or react with the insulating resin material.
[0041] (5) In any one of the above (1) to (4), the additive may include a polymer of an epoxy compound.
[0042] (6) In any one of the above (1) to (5), the insulating resin material may include a polyimide-based resin.
[0043] (7) With regard to any one of (1) to (6) above, in the cross section of the solid electrolytic capacitor element in the insulating region, the area of the solidified material filling the pores may account for 80% or more of the total area of the pores.
[0044] (8) With respect to any one of the above (1) to (7), in the insulating region, the solidified material may be formed on the main surface of the anode foil via the dielectric layer. In the main surface of the anode foil, the maximum thickness of the solidified material formed on the dielectric layer on one main surface side of the anode foil is t c , the thickness of the anode foil is t f At this time, the maximum thickness of the solidified material is c Relative to the thickness t of the anode foil f The ratio (=t c / t f ) can be less than 0.12.
[0045] The present disclosure also includes (9) a solid electrolytic capacitor comprising at least one of the above-mentioned solid electrolytic capacitor elements.
[0046] (10) In the above (9), the solid electrolytic capacitor may include an outer casing that seals the solid electrolytic capacitor element.
[0047] The present disclosure also includes a method for manufacturing a solid electrolytic capacitor element. The solid electrolytic capacitor element can be formed by, for example, the following manufacturing method, which includes:
[0048] The first step is to prepare an anode foil having a porous portion on a surface layer and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion;
[0049] A second step of forming a dielectric layer on the surface of the porous portion;
[0050] A third step of forming an insulating region including a cured product of the resin composition between the first end portion and the second end portion of the anode foil; and
[0051] In the fourth step, a solid electrolyte layer is formed, the solid electrolyte layer covering at least a portion of the dielectric layer.
[0052] More specifically, (11) the method for manufacturing a solid electrolytic capacitor element of the present disclosure includes:
[0053] The first step is to prepare an anode foil having a porous portion on a surface layer and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion;
[0054] A second step of forming a dielectric layer on the surface of the porous portion;
[0055] a third step of forming an insulating region including a cured product of a resin composition between the first end portion and the second end portion of the anode foil; and
[0056] In a fourth step, a solid electrolyte layer is formed, the solid electrolyte layer covering at least a portion of the dielectric layer.
[0057] The resin composition includes an insulating resin material and an additive for modifying the insulating resin material. The content of the additive in the resin composition is 3% by mass or more. The glass transition temperature of the cured product is 230° C. or more.
[0058] The third step includes a sub-step of filling the pores of the porous portion with a treatment liquid containing the resin composition and a solvent and curing the resin composition.
[0059] (12) In the above (11), the dry solid content of the treatment liquid may be 30% by mass or more, and the viscosity at 25° C. may be 1,000 mPa·s or more and 50,000 mPa·s or less.
[0060] (13) In the above (11) or (12), the fourth step may include the following second sub-step, which forms at least a portion of the solid electrolyte layer by in-situ polymerizing a precursor of a conjugated polymer in the presence of a dopant.
[0061] (14) In the above (13), the fourth step may include, before the second sub-step, a first sub-step of pre-coating the surface of the dielectric layer with a liquid composition containing a conductive material.
[0062] It should be noted that the dry solid content concentration of the treatment liquid or the dry solid content content of the treatment liquid refers to the total content of components other than the solvent in the mass of the treatment liquid.
[0063] The following describes in more detail the solid electrolytic capacitor element and solid electrolytic capacitor, and the method for manufacturing the solid electrolytic capacitor element, including the above (1) to (14). At least one of the above (1) to (14) is combined with at least one of the elements described below within the scope of no technical contradiction.
[0064] [Solid electrolytic capacitors]
[0065] The solid electrolytic capacitor element contained in the solid electrolytic capacitor includes: an anode body, a dielectric layer formed on the surface of the anode body, and a cathode portion covering at least a portion of the dielectric layer. The cathode portion includes a solid electrolyte layer covering at least a portion of the dielectric layer. Hereinafter, the solid electrolytic capacitor element is sometimes referred to as a capacitor element.
[0066] (Capacitor Components)
[0067] (Anode Foil)
[0068] The anode foil may include a valve metal, an alloy containing a valve metal, a compound containing a valve metal, etc. The anode foil may include one of the above materials, or a combination of two or more. As the valve metal, aluminum, tantalum, niobium, and titanium are preferred.
[0069] The anode foil has a porous portion at least on the surface. The anode foil has a plurality of fine pores in the porous portion. Through this porous portion, the anode body has a fine concave-convex shape at least on the surface. The anode foil having a porous portion on the surface is obtained, for example, by roughening the surface of a substrate (metal foil, etc.) containing a valve-acting metal. Surface roughening can also be performed, for example, by etching treatment (electrolytic etching, chemical etching, etc.). This anode foil, for example, has a substrate portion (core portion), and a porous portion formed integrally with the core portion on both sides of the core portion.
[0070] The anode foil is divided into a second part in which a cathode portion is formed via a dielectric layer, and a first part other than the second part. The second part is sometimes referred to as a cathode forming part, and the first part is referred to as an anode lead-out part (or anode part). The anode foil has a first end and a second end on the opposite side of the first end. The first end and the second end correspond to the two ends in the length direction of the anode foil. The first part includes the first end, and the second part includes the second end. An insulating region is formed between the first end and the second end. It should be noted that the length direction of the anode foil refers to the direction connecting the center of the end face of the first end and the center of the end face of the second end when the anode foil is in an extended state (unbent state).
[0071] The porous portion may be formed in the second portion and the portion forming the insulating region, or may be formed on both surfaces of the anode foil as a whole (specifically, the second portion and the first portion). The first portion is used to electrically connect to the external electrode on the anode side. For example, one end of the anode lead is electrically connected to the first portion, and the other end of the anode lead is led out from the outer casing and electrically connected to the external electrode.
[0072] The thickness of the anode foil (t f ) may be 50 μm or more and 200 μm or less, or 70 μm or more and 150 μm or less. The thickness t of the anode foil f The thickness of the anode foil is determined by measuring the thickness of the anode foil at a plurality of locations (eg, five locations) using a sample for determining the filling rate of the cured product described later and averaging the measured values.
[0073] (Dielectric layer)
[0074] The dielectric layer is formed, for example, in a manner covering at least a portion of the surface of the anode foil. The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer is formed by anodizing the valve metal on the surface of the anode foil using a chemical conversion treatment or the like. The dielectric layer is formed on the porous surface of the anode foil, so the surface of the dielectric layer has a fine concavo-convex shape corresponding to the shape of the porous portion of the anode foil.
[0075] The dielectric layer includes an oxide of a valve metal. For example, when tantalum is used as the valve metal, the dielectric layer includes Ta2O5, and when aluminum is used as the valve metal, the dielectric layer includes Al2O3. It should be noted that the dielectric layer is not limited to these examples, as long as it functions as a dielectric.
[0076] (Insulation area)
[0077] The insulating region is provided at a portion of the anode foil between the first end and the second end where the porous portion is formed with a predetermined width. The insulating region may be formed, for example, at the end of the first portion on the second portion side. In this case, the cathode portion is sometimes formed at the end of the second end side of the surface of the insulating region. In other words, the insulating region is sometimes provided from the end of the first portion on the second portion side to the end of the second portion on the first portion side. From the perspective of more reliably ensuring the insulation between the first portion and the cathode portion, it is preferred that the insulating region is not provided in the second portion.
[0078] The insulating region contains a cured product of a resin composition. In the insulating region, the cured product is filled in the pores of the porous portion. The Tg of the cured product is above 230°C and can be above 250°C. When the Tg of the cured product is so high, the viscosity of the treatment liquid containing the resin composition for forming the insulating region tends to increase, and the filling property of the resin composition into the pores of the porous portion tends to decrease. In addition, even if the treatment liquid is diluted with a solvent, the filling property of the resin composition into the pores tends to decrease due to the decrease in the dry solid content of the treatment liquid. In the present disclosure, the resin composition contains an insulating resin material and an additive (hereinafter sometimes referred to as the first additive) for modifying the insulating resin material, and the content of the additive in the resin composition is set to 3% by mass or more. Therefore, although the Tg of the cured product of the resin composition is high as described above and the viscosity of the treatment liquid containing the resin composition tends to increase, the resin composition (or its cured product) can still be highly filled in the pores. Therefore, since the insulation between the cathode portion and the first portion (anode portion) is easily ensured by the insulating region, the leakage current can be reduced.
[0079] The content of the first additive in the resin composition is 3% by mass or more, and may be 5% by mass or more, 10% by mass or more, or 13% by mass or more. When the resin composition contains the first additive at such a content, it is possible to maintain a high dry solid content in the treatment liquid for forming the insulating region and suppress the viscosity of the treatment liquid to a lower level, and to improve the filling property of the resin composition (or its cured product) into the pores. The content of the first additive in the resin composition is, for example, 60% by mass or less, and may be 55% by mass or less or 50% by mass or less. When the content of the first additive is in such a range, it is easy to ensure a high Tg of the cured product. These lower limits and upper limits can be combined arbitrarily. The content of the first additive in the resin composition may be, for example, 3% by mass or more (or 5% by mass or more) and 60% by mass or less, 10% by mass or more (or 13% by mass or more) and 60% by mass or less. The upper limit may be changed to the above value within these ranges.
[0080] The viscosity of a γ-butyrolactone solution containing a resin composition at a concentration of 30% by mass at 25°C may be 10,000 mPa·s or less, 8,000 mPa·s or less, or 6,000 mPa·s or less. It should be noted that the concentration of the resin composition in the solution is the content (mass %) of the dry solid component in the solution. Since the Tg of the cured product is high as described above, the viscosity of the solution containing the resin composition having such a high content of dry solid components tends to increase. However, in the present disclosure, since the first additive is used at the content rate described above, the viscosity of the solution can be suppressed to a low level. From the perspective of easily maintaining the processing liquid for forming the insulating region at a predetermined position to form the insulating region, the viscosity of the above-mentioned solution at 25°C is, for example, 1,000 mPa·s or more, and may be 2,000 mPa·s or more. These lower limits and upper limits can be combined arbitrarily.
[0081] The viscosity of the solution can be measured using a cone and plate viscometer at a rotation speed of 60 rpm.
[0082] As the insulating resin material, a resin material whose Tg of a cured product of a resin composition is in the above range can be cited. As the insulating resin material, a curable resin can be cited, but a thermoplastic resin can also be used. When a thermoplastic resin is used as the insulating resin material, a cured product of the resin composition is formed, for example, by a reaction between the first additive and the thermoplastic resin. When the insulating resin material is a curable resin, it is preferred that the Tg of the cured product of the curable resin itself is also high. The Tg of the cured product of the curable resin can be above 230°C, or above 250°C.
[0083] As insulating resin materials, curable resins (polyimide resins, silicone resins, phenolic resins, urea resins, melamine resins, unsaturated polyesters, furan resins, polyurethanes, silicone resins (siloxanes), curable acrylic resins, epoxy resins, etc.), photoresists, thermoplastic resins (such as polyamide, polyamideimide, thermoplastic polyimide, polyphenylene sulfone resins, polyethersulfone resins, cyanate resins, fluororesins), etc. are listed. From the perspective of obtaining a high Tg of the cured product and easily ensuring high heat resistance, polyimide resins (among which, curable polyimide resins) are preferred. Curable polyimide resins include, for example, curable polyamideimide and curable polyimide. The insulating resin material may contain one of these resins, or may contain two or more in combination. It should be noted that the insulating resin material, in addition to the resin as a polymer, also contains a precursor of the resin (monomer, oligomer, or prepolymer, etc.), depending on the type of the resin. The curable resin may be a one-component curing type or a two-component curing type. In addition to the insulating resin material and the first additive, the resin composition may further include at least one selected from the group consisting of a curing agent, a curing accelerator, a polymerization initiator, and a catalyst.
[0084] The Tg of the cured product of the resin composition can be determined, for example, by dynamic viscoelasticity measurement (DMA) under the conditions of a temperature increase rate of 2° C. / min and a frequency of 1 Hz.
[0085] The first additive is a component that modifies the insulating resin material. The first additive preferably contains a component that interacts or reacts with the insulating resin material. Examples of the first additive include silane coupling agents, surface tension modifiers, epoxy compounds or polymers thereof. Among them, as the first additive, a component different from the insulating resin material is used. The resin composition may contain one first additive, or may contain a combination of two or more. It is believed that by including the first additive in the resin composition at a relatively high content of 3% by mass or more, the first additive enters between the molecular chains of the insulating resin material, thereby improving fluidity and increasing the permeability of the resin composition into the pores of the porous portion.
[0086] Examples of the silane coupling agent include tetraalkoxysilane (tetramethoxysilane, etc.), alkoxysilane having a hydrocarbon group (methyltrimethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, phenyltrimethoxysilane, etc.), alkoxysilane having a functional group [3-(trimethoxysilyl)propylamine, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-(trimethoxysilyl)propylmethacrylate, 3-glycidoxypropyltrimethoxysilane, etc.], etc. The content of the silane coupling agent in the resin composition may be low, and the resin composition may not contain the silane coupling agent.
[0087] Surface tension adjusters include defoamers, silicon-based and non-silicon-based surface tension adjusters, etc. Examples of silicon-based surface tension adjusters include silicone oil, silicon-based surfactants, and silicon-based synthetic lubricating oils. Examples of non-silicon-based surface tension adjusters include lower alcohols, mineral oils, oleic acid, polypropylene glycol, glycerol higher fatty acid esters, higher alcohol boric acid esters, and fluorine-containing surfactants.
[0088] Examples of epoxy compounds include glycidyl ethers, glycidyl esters, alicyclic epoxy compounds, and the like. Examples of epoxy compounds include bisphenol epoxy compounds (bisphenol A epoxy compounds, bisphenol F epoxy compounds, and the like), condensed ring aromatic epoxy compounds (naphthalene epoxy compounds, and the like), and novolac epoxy compounds, and the like. Examples of epoxy compound polymers include reactants of epoxy compounds and active hydrogen-containing compounds (amines, hydroxyl compounds, phenol compounds, acid anhydrides, and the like). Epoxy compounds and their polymers are preferably components that are liquid (have fluidity) at 25°C. In addition to having the effect of reducing the viscosity of the treatment liquid, such epoxy compounds or their polymers react with insulating resin materials such as polyimide resins and are incorporated into the cured product, and are therefore particularly excellent in improving the filling properties of the cured product in the pores of the porous portion.
[0089] The resin composition may contain a known additive (second additive) for forming an insulating region of a capacitor element in addition to the first additive as required. Examples of the second additive include flame retardants, fillers, colorants, release agents, and inorganic ion scavengers.
[0090] In the present disclosure, in the insulating region, the resin composition (or its cured product) containing the insulating resin material can be highly filled in the pores of the porous portion. In the cross section of the solid electrolytic capacitor element in the insulating region (more specifically, the cross section of the portion including the insulating region and the anode foil), the ratio of the area of the cured product filled in the pores to the total area of the pores (the filling rate of the cured product) is, for example, 80% or more.
[0091] The filling rate of the solidified material can be obtained using the anode foil with the insulating region formed before the solid electrolyte layer is formed (before pre-coating). More specifically, the anode foil with the insulating region is buried in a curable resin to cure the curable resin. The solidified material is subjected to grinding or cross-sectional polishing to expose a cross section parallel to the thickness direction of the insulating region and parallel to the length direction of the anode foil. The cross section is a cross section passing through the center of the width of the insulating region (in other words, the length in the direction parallel to the width direction of the anode foil). In this way, a sample for measurement can be obtained. In addition, the cross section of the sample is subjected to image processing and divided into the metal portion (including the dielectric layer portion) constituting the anode foil, the void portion, and the portion occupied by the solidified material, and the proportion (%) of the area of the portion occupied by the solidified material in the total area of the void portion and the portion occupied by the solidified material is obtained as the filling rate of the solidified material. Each area is calculated as follows: in an image in which the entire cross-section in the thickness direction of the anode foil including the entire portion where the insulating region is formed can be observed, the length direction is calculated for a portion of a length of 0.5L centered on the center of the length L of the insulating region, and the thickness direction is calculated for the entire porous portion (two porous portions when porous portions are formed on two surface layers).
[0092] In the insulating region, the solidified material may be formed not only in the pores but also on the main surface of the anode foil via the dielectric layer. In addition, a sheet-like insulating material such as an insulating tape may be attached to the main surface of the anode foil as required.
[0093] When the solidified material is formed on the main surface of the anode foil via the dielectric layer, the maximum thickness t of the solidified material formed on the dielectric layer on the main surface of the anode foil is c It can be less than 20 μm or less than 15 μm. c When the thickness is within this range, the leakage current is further reduced, and the short circuit rate can be suppressed to a low level. In addition, when stacking capacitor elements, the stress of the bent lead frame can be suppressed to a low level. c It can be 0 μm or more. The maximum thickness t c It is the maximum value of the thickness of the cured product on one main surface side of the anode foil. The thickness of the cured product is measured using a sample of the cross section used to measure the above filling rate.
[0094] The maximum thickness of the above solidified material is t c Relative to the thickness of the anode foil t f The ratio (=t c / t f ) may be less than 0.12, less than 0.11, or less than 0.10. c / t fWhen the ratio is within this range, the leakage current is further reduced, and the short circuit occurrence rate can be suppressed to a low level. c / t f The ratio may be 0.01 or more.
[0095] The insulating region can be formed, for example, by a step (third step) including the sub-steps of filling the pores of the porous portion with a treatment liquid containing a resin composition and a solvent and curing the resin composition.
[0096] The content of the dry solid content of the treatment liquid (concentration of the resin composition) is, for example, 30% by mass or more, and may be 30% by mass or more and 50% by mass or less. In addition, the viscosity of the treatment liquid at 25°C may be 1,000 mPa·s or more and 50,000 mPa·s or less, 2,000 mPa·s or more and 35,000 mPa·s or more, or 2,500 mPa·s or more and 30,000 mPa·s or less. In the present disclosure, by combining a resin composition having a high Tg of the cured product as described above and a first additive having a specific content, the viscosity of the treatment liquid can be kept within such a low range even if the content of the dry solid content of the treatment liquid for forming the insulating region is as high as described above. Therefore, the resin composition (or its cured product) can be highly filled in the pores of the porous portion, and the intrusion of the conductive material into the remaining voids in the insulating region can be reduced, thereby reducing the leakage current. It should be noted that the viscosity of the treatment liquid can be measured using a cone and plate viscometer at a rotation speed of 60 rpm.
[0097] In the method for manufacturing a capacitor element, before the third step of forming an insulating region, the following steps are performed: a first step of preparing an anode foil having a porous portion on a surface layer, and having a first portion including a first end portion and a second portion including a second end portion on the opposite side of the first end portion; and a second step of forming a dielectric layer on the surface of the porous portion. For each step, reference can be made to the description of the anode foil and the dielectric layer.
[0098] (Cathode)
[0099] The cathode portion is formed in a manner covering at least a portion of the dielectric layer formed on the surface of the anode body. The cathode portion includes at least a solid electrolyte layer. The cathode portion may include, for example: a solid electrolyte layer covering at least a portion of the dielectric layer and a cathode lead layer covering at least a portion of the solid electrolyte layer. The layers constituting the cathode portion may be formed using a known method according to the layer structure of the cathode portion.
[0100] Hereinafter, constituent elements of the cathode portion will be described.
[0101] (Solid electrolyte layer)
[0102] The solid electrolyte layer contains, for example, a conductive polymer (a conjugated polymer, a dopant, etc.) The solid electrolyte layer may contain a manganese compound, an additive, and the like.
[0103] As conjugated polymers, for example, well-known conjugated polymers such as π-conjugated polymers used in solid electrolytic capacitors can be listed. As conjugated polymers, for example, polymers with polypyrrole, polythiophene, polyaniline, polyfuran, polyacetylene, polyphenylene, polyphenylene vinylene, polybenzone and polythiophene vinylene as basic skeletons can be listed. The polymer only needs to contain at least one monomer unit constituting the basic skeleton. The monomer unit also includes a monomer unit with a substituent. The above-mentioned polymer includes, for example, a homopolymer and a copolymer of two or more monomers. For example, polythiophene includes poly (3,4-ethylenedioxythiophene) and the like. The solid electrolyte layer can contain one conjugated polymer, or it can contain a combination of two or more.
[0104] As a dopant, a polymer anion such as polystyrene sulfonic acid (PSS) can be used. In addition, as a dopant, a compound that can generate anions (such as aromatic sulfonic acids such as naphthalenesulfonic acid and toluenesulfonic acid) can also be used. However, the dopant is not limited to these.
[0105] The solid electrolyte layer is formed so as to cover at least a portion of the dielectric layer (the fourth step). From the perspective of ensuring insulation from the first portion, the solid electrolyte layer is formed after the insulating region is formed (after the third step).
[0106] The solid electrolyte layer can be formed, for example, by in situ polymerization (more specifically, polymerization on the dielectric layer) of a conjugated polymer precursor (monomer, oligomer, etc.) in the presence of a dopant. As dopants, aromatic sulfonic acids and the like can be listed. As in situ polymerization, at least one of chemical polymerization and electrolytic polymerization can be used. Alternatively, the solid electrolyte layer can also be formed by attaching a treatment liquid (solution or dispersion) containing a conductive polymer (conjugated polymer and dopant, etc.) to the dielectric layer and drying it. As a dispersion medium (solvent), for example, water, an organic solvent or a mixture thereof can be listed. The solid electrolyte layer can be formed by combining a method using in situ polymerization and a method using a treatment liquid containing a conductive polymer. For example, after a portion of the solid electrolyte layer is formed by in situ polymerization, the remaining portion of the solid electrolyte layer can be formed using a treatment liquid containing a conductive polymer.
[0107] In the electrolytic polymerization, the surface of the dielectric layer may also be pre-coated before polymerization. The pre-coating is performed, for example, using a liquid composition (liquid dispersion, etc.) containing a conductive material. More specifically, the pre-coating can be performed using a liquid dispersion containing a conductive polymer (a conjugated polymer and a dopant, etc.). The conductive polymer in the liquid dispersion used in the pre-coating has a small particle size and a low concentration. For example, the average primary particle size of the conductive polymer particles contained in the pre-coating liquid dispersion is, for example, less than 100 nm.
[0108] The polymerizing liquid used in the in-situ polymerization easily penetrates into the fine recesses of the dielectric layer, and therefore, the method utilizing in-situ polymerization is at least suitable for forming a solid electrolyte in the fine recesses of the dielectric layer. Therefore, the process (the 4th process) forming the solid electrolyte layer may include a sub-step (the 2nd sub-step) of forming at least a portion of the solid electrolyte layer by in-situ polymerization of the precursor of the conjugated polymer in the presence of a dopant. In addition, before the 2nd sub-step, a sub-step (the 1st sub-step) of pre-coating with a liquid composition containing a conductive material on the surface of the dielectric layer may be performed. The pre-coating liquid composition also easily penetrates into the fine recesses of the dielectric layer. In the present disclosure, since the filling property of the cured product of the resin composition in the porous portion of the insulating region can be improved, even in the case of forming at least a portion of the solid electrolyte layer by in-situ polymerization or in the case of pre-coating, the polymerizing liquid or the pre-coating liquid composition can be effectively suppressed from invading the gap in the insulating region or the 1st part. Therefore, even in this case, the leakage current can be reduced.
[0109] (Cathode extraction layer)
[0110] The cathode lead layer only needs to have at least a first layer that contacts the solid electrolyte layer and covers at least a portion of the solid electrolyte layer, and may also have a first layer and a second layer that covers the first layer. As the first layer, for example, a layer containing conductive particles, a metal foil, etc. can be listed. As the conductive particles, for example, at least one selected from conductive carbon and metal powder can be listed. For example, the cathode lead layer can be composed of a layer containing conductive carbon as the first layer (also referred to as a carbon layer) and a layer containing metal powder or a metal foil as the second layer. In the case of using a metal foil as the first layer, the cathode lead layer can also be composed of the metal foil.
[0111] Examples of the conductive carbon include graphite (artificial graphite, natural graphite, etc.).
[0112] The layer containing metal powder as the second layer can be formed, for example, by laminating a composition containing metal powder on the surface of the first layer. As such a second layer, for example, a metal paste layer (silver paste layer, etc.) formed using a composition containing metal powder such as silver particles and a resin (binder resin) can be cited. As the resin, a thermoplastic resin can also be used, but a thermosetting resin such as an imide resin and an epoxy resin is preferably used.
[0113] When a metal foil is used as the first layer, the type of metal is not particularly limited, and preferably a valve metal such as aluminum, tantalum, niobium, or an alloy containing a valve metal is used. The surface of the metal foil may be roughened as required. A chemical conversion coating may be provided on the surface of the metal foil, or a coating of a metal (dissimilar metal) or a non-metallic film different from the metal constituting the metal foil may be provided. Examples of the dissimilar metal or non-metal include metals such as titanium and non-metals such as carbon (conductive carbon, etc.).
[0114] The coating of the above-mentioned different metal or non-metal (for example, conductive carbon) may be used as the first layer, and the above-mentioned metal foil may be used as the second layer.
[0115] The method for manufacturing a capacitor element may further include a step of forming a cathode lead layer (fifth step).
[0116] (Separator)
[0117] When a metal foil is used for the cathode lead-out layer, a separator may be disposed between the metal foil and the anode foil. The separator is not particularly limited, and for example, a nonwoven fabric containing fibers of cellulose, polyethylene terephthalate, vinylon, or polyamide (e.g., aliphatic polyamide, aromatic polyamide such as aramid) may be used.
[0118] (other)
[0119] The solid electrolytic capacitor includes, for example, at least one capacitor element and an outer casing that seals the capacitor element. The solid electrolytic capacitor may include more than two capacitor elements. The solid electrolytic capacitor may be a wound type, or may be a chip type or a stacked type. For example, the solid electrolytic capacitor may have more than two wound capacitor elements, or may have more than two stacked capacitor elements. The structure of the capacitor element may be selected according to the type of the solid electrolytic capacitor.
[0120] In the capacitor element, the cathode lead layer is electrically connected to one end of the cathode lead. The anode body is electrically connected to one end of the anode lead. The other end of the anode lead and the other end of the cathode lead are respectively led out from the resin outer casing or the shell. The other end of each lead exposed from the resin outer casing or the shell is used for welding with a substrate to be mounted with a solid electrolytic capacitor, etc. As each lead, a lead wire or a lead frame can be used.
[0121] A solid electrolytic capacitor can be obtained, for example, by a manufacturing method including a process of forming a capacitor element and a process of sealing at least one solid electrolytic capacitor element with an outer casing. The capacitor element is formed, for example, by the above-mentioned manufacturing method (for example, a manufacturing method including the first to fifth processes, etc.). For example, when manufacturing a solid electrolytic capacitor including two or more stacked capacitor elements, the manufacturing method further includes a process of stacking two or more capacitor elements before the sealing process. Furthermore, in the sealing process, the stacked two or more capacitor elements are sealed with an outer casing.
[0122] The outer casing also includes a shell. The outer casing may include a resin. For example, the capacitor element and the material resin of the outer casing (for example, uncured thermosetting resin and filler) may be housed in a mold, and the capacitor element may be sealed with a resin outer casing by transfer molding, compression molding, etc. At this time, the portion of the other end side of the anode lead and the portion of the other end side of the cathode lead that are led out from the capacitor element are exposed from the mold respectively. In addition, the capacitor element may be housed in a bottomed shell in a manner such that the portion of the other end side of the anode lead and the portion of the other end side of the cathode lead are located on the opening side of the bottomed shell, and the opening of the bottomed shell is closed by a sealing body, thereby forming a solid electrolytic capacitor.
[0123] The solid electrolytic capacitor may further include a shell disposed outside the resin outer casing as required. As the resin material constituting the shell, thermoplastic resins or compositions containing thermoplastic resins may be listed. As the metal material constituting the shell, for example, metals such as aluminum, copper, and iron or their alloys (including stainless steel, brass, etc.) may be listed.
[0124] Figure 1 It is a cross-sectional view schematically showing the structure of the solid electrolytic capacitor according to the first embodiment of the present disclosure. Figure 2 It is schematically shown Figure 1 FIG. 1 is an enlarged cross-sectional view of capacitor element 2 included in a solid electrolytic capacitor.
[0125] The solid electrolytic capacitor 1 includes a capacitor element 2, an outer casing 3 sealing the capacitor element 2, and an anode lead terminal 4 and a cathode lead terminal 5, each of which has at least a portion exposed to the outside of the outer casing 3. The outer casing 3 has a substantially rectangular parallelepiped shape, and the solid electrolytic capacitor 1 also has a substantially rectangular parallelepiped shape.
[0126] Capacitor element 2 includes anode foil 6 , a dielectric layer (not shown) covering the surface of anode foil 6 , and cathode portion 8 covering the dielectric layer. The dielectric layer may be formed on at least a portion of the surface of anode foil 6 .
[0127] The cathode portion 8 includes a solid electrolyte layer 9 and a cathode lead layer 10. The solid electrolyte layer 9 is formed so as to cover at least a portion of the dielectric layer. The cathode lead layer 10 is formed so as to cover at least a portion of the solid electrolyte layer 9. The cathode lead layer 10 includes a first layer 11 as a carbon layer and a second layer 12 as a metal paste layer. The cathode lead terminal 5 is electrically connected to the cathode portion 8 via an adhesive layer 14 formed of a conductive adhesive.
[0128] The anode foil 6 includes a substrate portion (core portion) 6a and a porous portion 6b formed on the surface of the substrate portion 6a. The anode foil 6 includes a second portion II as a cathode forming portion where a solid electrolyte layer 9 (or cathode portion 8) is formed, and a first portion I other than the second portion II. The first portion I includes at least the anode portion ia. The anode lead terminal 4 is electrically connected to the anode portion ia of the anode foil 6 by welding. The anode foil 6 has a first end portion Ie on the side connected to the anode lead terminal 4 and a second end portion IIe on the opposite side to the first end portion Ie.
[0129] An insulating region 13 is provided between the first end Ie and the second end IIe of the anode foil 6. The insulating region 13 may be provided at the end of the first portion I on the second portion II side. The insulating region 13 includes at least a cured product of the resin composition filled in the pores of the porous portion 6b.
[0130] Outer casing 3 covers capacitor element 2 and a portion of lead terminals 4 and 5. From the viewpoint of suppressing the intrusion of air into outer casing 3, capacitor element 2 and a portion of lead terminals 4 and 5 are preferably sealed by outer casing 3. Figure 1 Although the case where outer casing 3 is a resin outer casing is shown, the present invention is not limited to this case and outer casing 3 may be a case or the like capable of accommodating capacitor element 2. The resin outer casing is formed by sealing capacitor element 2 and part of lead terminals 4 and 5 with a resin material.
[0131] One end of lead terminals 4 and 5 is electrically connected to capacitor element 2 , and the other end is led out of outer casing 3 . In solid electrolytic capacitor 1 , one end of lead terminals 4 and 5 is covered by outer casing 3 together with capacitor element 2 .
[0132] [Example]
[0133] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited only to the following Examples.
[0134] 《Examples 1 and 2 and Comparative Example 1》
[0135] (1) Preparation of anode foil with dielectric layer
[0136] An aluminum foil (thickness 100 μm) was prepared as a substrate, and both surfaces of the aluminum foil were etched to obtain an anode foil having a porous portion on the surface layer (thickness 35 μm on one main surface side of the aluminum foil and thickness 35 μm on the other main surface side).
[0137] The anode foil is immersed in a chemical conversion solution and a direct current voltage is applied to form a dielectric layer containing aluminum oxide on the surface of the anode foil.
[0138] (2) Formation of insulation area
[0139] At a predetermined position between the first end and the second end of the anode foil formed with a dielectric layer, a treatment liquid containing a resin composition is impregnated in a strip shape along the width direction of the anode foil on both surfaces of the anode foil, and heated at 200°C for 30 minutes to cure the resin composition. The resin composition cures while filling the pores of the porous portion. In this way, an insulating region containing a cured product is formed. As the treatment liquid, a liquid composition containing a curable polyamide-imide resin (precursor), γ-butyrolactone as a solvent, and a bisphenol A type liquid epoxy resin (polymer) as a first additive is used. The content (mass %) of the dry solid content of the liquid composition, the content (mass %) of the first additive in the resin composition (dry solid content of the liquid composition), the viscosity (mPa·s) of the liquid composition at 25°C, and the Tg (°C) of the cured product of the resin composition are shown in Table 1.
[0140] (3) Formation of solid electrolyte layer
[0141] Pre-coating is performed by immersing the second portion of the second end portion of the anode foil having the insulating region obtained in (2) above in a liquid composition containing a conductive material, taking it out and drying it. A power supply tape is attached to the surface of the insulating region.
[0142] Prepare a polymerization solution (liquid composition) containing pyrrole (monomer of conjugated polymer), naphthalenesulfonic acid (dopant) and water. Immerse the pre-coated anode foil and counter electrode in the obtained polymerization solution. Apply voltage to the power supply belt in a manner that the potential of the power supply belt is 2.0V (= polymerization voltage) and perform electrolytic polymerization at 25°C to form a solid electrolyte layer. The polymerization voltage is the potential of the power supply body relative to the reference electrode (silver / silver chloride reference electrode).
[0143] (4) Formation of cathode lead layer
[0144] The anode foil having the solid electrolyte layer obtained in (3) above is immersed in a dispersion in which graphite particles are dispersed in water, taken out of the dispersion and dried, thereby forming a carbon layer (first layer) at least on the surface of the solid electrolyte layer. The drying is performed at 150° C. for 30 minutes.
[0145] A silver paste containing silver particles and a binder resin (epoxy resin) was applied to the surface of the carbon layer, and the binder resin was cured by heating at 150°C for 30 minutes to form a silver paste layer (second layer). In this way, a cathode lead layer consisting of the carbon layer and the silver paste layer was formed, and the cathode portion consisting of the solid electrolyte layer and the cathode lead layer was completed.
[0146] (5) Assembly of solid electrolytic capacitors
[0147] The cathode portion of the capacitor element obtained in (4) above and one end of the cathode lead terminal are bonded via an adhesive layer of a conductive adhesive. One end of the anode lead terminal is bonded to the first end side surface of the first portion of the anode foil protruding from the capacitor element by laser welding.
[0148] Next, a resin outer casing made of insulating resin was formed around the capacitor element by molding. At this time, the other end of the anode lead terminal and the other end of the cathode lead terminal were set to be led out of the resin outer casing. In this way, a total of 20 solid electrolytic capacitors were completed.
[0149] (6) Evaluation
[0150] The following evaluations were performed using a liquid composition or a solid electrolytic capacitor containing the resin composition.
[0151] (a) Viscosity of the treatment liquid (liquid composition) and a solution having a concentration of 30% by mass
[0152] The viscosity of the treatment liquid at 25° C. was measured in the above-mentioned procedure. The treatment liquid was diluted with γ-butyrolactone so that the concentration of the resin composition in the treatment liquid was 30% by mass, and the viscosity of the obtained solution at 25° C. was measured.
[0153] (b) Tg of cured product of resin composition
[0154] A cured product of the resin composition was prepared using the treatment liquid, and the Tg of the cured product was measured according to the above-mentioned procedure.
[0155] (c) Initial electrostatic capacitance, tanδ and ESR (equivalent series resistance)
[0156] In an environment of 20°C, a 4-terminal LCR meter was used to measure the initial capacitance (μF) and initial tanδ of each solid electrolytic capacitor at a frequency of 120Hz, and the initial ESR (mΩ) at a frequency of 100kHz was measured. Then, the average value of the 20 solid electrolytic capacitors was calculated. The results of each example are expressed as relative values when the results of Comparative Example 1 are set to 100.
[0157] (d) Leakage current (LC)
[0158] A 1 kΩ resistor was connected in series with the solid electrolytic capacitor, and the leakage current (μA) was measured after applying a rated voltage of 25 V using a DC power supply for 1 minute, and the average value of 20 solid electrolytic capacitors was obtained. The results of each example are expressed as relative values when the result of Comparative Example 1 is set to 100.
[0159] The evaluation results are shown in Table 1. In Table 1, E1 and E2 are Examples 1 and 2, and C1 is Comparative Example 1.
[0160] [Table 1]
[0161]
[0162] As shown in Table 1, compared with Comparative Example 1 in which the content of the first additive in the resin composition is 0.1% by mass, in the embodiment, the leakage current is significantly reduced. Polyimide resins such as polyamide-imide resins have a tendency to have a high Tg and a high viscosity of the treatment liquid. Since the dry solid content of the treatment liquid decreases when such a resin is diluted with a solvent, it is difficult to fill it into the pores of the porous portion at a high filling rate. As in Comparative Example 1, even if the first additive is added, if a certain degree of dry solid content is maintained when the content of the first additive is low, the viscosity of the treatment liquid increases, and it is difficult to fill the resin composition highly in the pores of the porous portion. In contrast, in the embodiment, the resin composition contains more first additives than Comparative Example 1, so although a polyimide resin or the like is used to provide an insulating resin material with a high Tg, the viscosity of the treatment liquid containing the resin composition can still be reduced while maintaining a relatively high dry solid content. Therefore, the resin composition can be highly filled in the pores of the porous part, and the pre-coating liquid composition or the solid electrolyte layer forming polymer solution can be inhibited from invading the pores of the porous part in the insulating region or invading the first part side through the pores. Therefore, in the embodiment, since the insulation of the insulating region becomes higher, the insulation between the cathode part and the first part can be ensured, so the leakage current is significantly reduced. It should be noted that in the embodiment, the filling rate of the cured product in the insulating region obtained according to the above steps is 80% or more.
[0163] In addition, in the example, while ensuring the same high initial electrostatic capacitance as the comparative example, tanδ and ESR can be significantly reduced compared to the comparative example. Thus, in the example, while ensuring the initial excellent capacitor performance, the leakage current can be reduced as described above.
[0164] 《Examples 3 to 6》
[0165] In Example 1 (2), the dry solid content (mass %) of the liquid composition and the viscosity of the liquid composition at 25° C. were adjusted so that the ratio t c / t f The values shown in Table 2 were achieved. A solid electrolytic capacitor was produced in the same manner as in Example 1 except for the above.
[0166] Evaluate the leakage current (LC) according to the above step (d), find the ratio (%) of the number of solid electrolytic capacitors with a leakage current exceeding 0.068 mA in 20, and use this ratio as the LC defect rate. At this time, find the ratio (%) of the number of solid electrolytic capacitors with a leakage current exceeding 1 mA in 20. Use this ratio as the short circuit defect rate.
[0167] The results are shown in Table 2. In Table 2, E3 to E6 are Examples 3 to 6.
[0168] [Table 2]
[0169] E3 E4 E5 E6 <![CDATA[t c / t f ]]> 0.05 0.09 0.14 0.19 Short circuit failure rate (%) 0.1 0.2 0.9 0.3 LC defect rate (%) 6.7 8.4 32.5 37.4
[0170] As shown in Table 2, from the perspective of ensuring a lower LC defect rate, the t c / t f It is preferably 0.12 or less, and more preferably 0.11 or less or 0.10 or less. c / t f When it is within such a range, the short-circuit defect rate can also be suppressed to be low.
[0171] The present invention has been described by the currently preferred embodiments, but such disclosure is not to be construed in a limiting sense. Various modifications and changes will undoubtedly be apparent to those skilled in the art in the art to which the present invention belongs by reading the above disclosure. Therefore, the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.
[0172] Industrial Applicability
[0173] In the solid electrolytic capacitor of the present disclosure, leakage current is reduced and excellent capacitor performance can be obtained. Therefore, the solid electrolytic capacitor can be used for various applications requiring high reliability, for example.
[0174] Description of Reference Numerals
[0175] 1: Solid electrolytic capacitor
[0176] 2: Capacitor element
[0177] 3: Exterior body
[0178] 4: Anode lead terminal
[0179] 5: Cathode lead terminal
[0180] 6: Anode foil
[0181] 6a: Base material (core)
[0182] 6b: Porous part
[0183] 8: Cathode
[0184] 9: Solid electrolyte layer
[0185] 10: Cathode lead layer
[0186] 11: Carbon layer (1st layer)
[0187] 12: Silver paste layer (2nd layer)
[0188] 13: Insulation area
[0189] 14: Adhesive layer
[0190] I: Part 1
[0191] II: Part 2
[0192] Ie: 1st end
[0193] IIe: 2nd end
[0194] ia: Anode
Claims
1. A solid electrolytic capacitor element, comprising: An anode foil having a porous portion on a surface layer, and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion; a dielectric layer formed on a surface of the porous portion; as well as a solid electrolyte layer covering at least a portion of the dielectric layer, The solid electrolytic capacitor element includes an insulating region including a cured product of a resin composition between the first end and the second end of the anode foil. In the insulating region, the solidified material fills the pores of the porous portion. The resin composition comprises an insulating resin material and an additive for modifying the insulating resin material. The content of the additive in the resin composition is 3% by mass or more, The glass transition temperature of the cured product is 230° C. or higher.
2. The solid electrolytic capacitor element according to claim 1, wherein The viscosity of a γ-butyrolactone solution of the resin composition at a concentration of 30% by mass at 25° C. is 1,000 mPa·s or more and 10,000 mPa·s or less.
3. The solid electrolytic capacitor element according to claim 1 or 2, wherein: The content of the additive in the resin composition is 60% by mass or less.
4. The solid electrolytic capacitor element according to any one of claims 1 to 3, wherein The additive interacts or reacts with the insulating resin material.
5. The solid electrolytic capacitor element according to any one of claims 1 to 4, wherein The additive comprises a polymer of an epoxy compound.
6. The solid electrolytic capacitor element according to any one of claims 1 to 5, wherein The insulating resin material includes a polyimide-based resin.
7. The solid electrolytic capacitor element according to any one of claims 1 to 6, wherein In the cross section of the solid electrolytic capacitor element in the insulating region, a ratio of the area of the solidified material filled in the pores to the total area of the pores is 80% or more.
8. The solid electrolytic capacitor element according to any one of claims 1 to 7, wherein In the insulating region, the solidified material is also formed on the main surface of the anode foil via the dielectric layer. In the main surface of the anode foil, the maximum thickness of the solidified material formed on the dielectric layer on one main surface side of the anode foil is t c , the thickness of the anode foil is t f , The maximum thickness of the solidified material is t c Relative to the thickness t of the anode foil f The ratio (=t c / t f ) is less than 0.
12. 9 . A solid electrolytic capacitor comprising at least one solid electrolytic capacitor element according to claim 1 . 10 . The solid electrolytic capacitor according to claim 9 , comprising an outer casing that seals the solid electrolytic capacitor element.
11. A method for manufacturing a solid electrolytic capacitor element, comprising: The first step is to prepare an anode foil having a porous portion on a surface layer and having a first portion including a first end portion and a second portion including a second end portion on the opposite side to the first end portion; A second step of forming a dielectric layer on the surface of the porous portion; a third step of forming an insulating region including a cured product of a resin composition between the first end portion and the second end portion of the anode foil; and In a fourth step, a solid electrolyte layer is formed, wherein the solid electrolyte layer covers at least a portion of the dielectric layer. The resin composition comprises an insulating resin material and an additive for modifying the insulating resin material, the content of the additive in the resin composition is 3% by mass or more, and the glass transition temperature of the cured product is 230° C. or more. The third step includes a sub-step of filling the pores of the porous portion with a treatment liquid containing the resin composition and a solvent and curing the resin composition.
12. The method for manufacturing a solid electrolytic capacitor element according to claim 11, wherein: The treatment liquid has a dry solid content of 30% by mass or more and a viscosity at 25° C. of 1,000 mPa·s or more and 50,000 mPa·s or less.
13. The method for manufacturing a solid electrolytic capacitor element according to claim 11 or 12, wherein: The fourth step includes a second sub-step of forming at least a portion of the solid electrolyte layer by in-situ polymerizing a precursor of a conjugated polymer in the presence of a dopant.
14. The method for manufacturing a solid electrolytic capacitor element according to claim 13, wherein: The fourth step includes, before the second sub-step, a first sub-step of pre-coating the surface of the dielectric layer with a liquid composition containing a conductive material.