All-solid-state secondary battery

By using a negative electrode layer containing Ag and a solid electrolyte layer structure with multiple gaps in an all-solid secondary battery, the problem of the reaction layer and the expansion and contraction stress of the negative electrode during high-temperature sintering of the oxide solid electrolyte is solved, and the battery performance is improved. Cycling characteristics and stability.

CN118765453APending Publication Date: 2024-10-11TDK CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202280092637.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-09-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Oxide solid electrolytes easily react with active materials during high-temperature sintering to form a reaction layer with low ion conductivity, resulting in low cycle characteristics of all-solid secondary batteries. In addition, stress caused by expansion and contraction of the negative electrode causes cracks or peeling, deteriorating battery performance.

Method used

In an all-solid secondary battery, a phase containing Ag is used as the negative electrode layer, and multiple voids are formed in the solid electrolyte layer, especially the voids connected to Ag, to relax the stress caused by expansion and contraction, and pass through specific voids Structure and proportion enhance cyclic properties.

Benefits of technology

It effectively alleviates the stress caused by the expansion and contraction of the negative electrode, improves the cycle characteristics of the all-solid secondary battery, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118765453A_ABST
    Figure CN118765453A_ABST
Patent Text Reader

Abstract

The all-solid-state secondary battery is provided with a laminate having a positive electrode layer, a negative electrode layer, and a solid electrolyte layer positioned between the positive electrode layer and the negative electrode layer, the solid electrolyte layer containing a compound represented by formula (1), the negative electrode layer containing a phase containing Ag, and a plurality of voids formed in the negative electrode layer, at least a portion of the void is formed so as to be in contact with the Ag-containing phase. Li3 + xSixP1-xO4 (1) (Formula (1) satisfies 0 < x < 1). )
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an all-solid secondary battery.

[0002] This application claims priority based on Japanese Patent Application No. 2022-058998 filed in Japan on March 31, 2022, and the contents are incorporated herein by reference. Background Art

[0003] In recent years, the development of electronic technology has been rapid, and portable electronic devices have been made small, lightweight, thin and multifunctional. As a result, for batteries that become power sources for electronic devices, it is strongly desired to be small, lightweight, thin and reliable. In the currently commonly used lithium-ion secondary batteries, electrolytes (electrolytes) such as organic solvents have always been used as media for moving ions. However, in the battery of the above structure, there is a risk of electrolyte leakage. In addition, since the organic solvents used for the electrolyte are flammable substances, it is required to further improve the safety of the battery.

[0004] As a countermeasure to improve battery safety, it has been proposed to use a solid electrolyte instead of an electrolyte solution. In addition, development of an all-solid secondary battery using a solid electrolyte as an electrolyte and other components also consisting of solids is underway (eg, Patent Document 1).

[0005] As solid electrolytes for all-solid secondary batteries, there are mainly sulfide solid electrolytes and oxide solid electrolytes. Sulfide solid electrolytes produce hydrogen sulfide when reacting with water, so the battery needs to be made in a glove box with a controlled dew point. In addition, sulfide solid electrolytes are difficult to make into sheets, and thin solid electrolytes that can contribute to the small, lightweight, thin, and multifunctional portable electronic devices are required. In view of this situation, the application of oxide solid electrolytes is highly anticipated.

[0006] As oxide-based solid electrolytes, LSPO (Li 3+x Si x P 1-x O4) etc. (Non-Patent Document 1). It is known that LSPO is relatively stable with respect to the active material even when sintered at a high temperature for densification.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2022-25903 (A)

[0010] Non-patent literature

[0011] Non-patent document 1: Solid State Ionics 283 (2015) 109-114 Summary of the invention

[0012] The technical problem that the invention is intended to solve

[0013] Oxide solid electrolytes need to be sintered at high temperatures for densification, but at this time, they sometimes react with active materials to form a reaction layer with low ion conductivity at the interface. In order to suppress the formation of such a reaction layer, methods of using the above-mentioned LSPO as a solid electrolyte are being studied, for example, using Ag, AgPd alloys, AgPd alloys and lithium titanate (Li4Ti5O 12 ) as the negative electrode, which is expected to help realize an all-solid-state secondary battery in which a reaction layer is difficult to form.

[0014] In addition, in all-solid secondary batteries, it is required to improve the cycle characteristics. The cycle characteristics of stacked chip-type all-solid secondary batteries are deteriorated due to the expansion and contraction of active materials during charging and discharging, resulting in cracks or peeling inside the electrode or at the interface with the solid electrolyte. In order to improve the cycle characteristics, it is necessary to suppress these cracks or peeling. When LSPO is used as the solid electrolyte and a phase containing Ag, such as Ag, AgPd alloy, AgPd alloy and lithium titanate, is used in the negative electrode, there is a problem of low cycle characteristics.

[0015] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an all-solid secondary battery capable of alleviating stress caused by expansion and contraction of a negative electrode and improving cycle characteristics.

[0016] Technical solutions for solving technical problems

[0017] In order to solve the above-mentioned technical problems, the present invention provides the following means.

[0018] (1) An all-solid secondary battery of one embodiment of the present invention comprises a stacked body, wherein the stacked body has: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, wherein the solid electrolyte layer contains a compound represented by the following formula (1), the negative electrode layer contains a phase containing Ag, and a plurality of voids are formed in the negative electrode layer, and at least a portion of the voids are first voids formed by contact with the phase containing Ag.

[0019] Li 3+x Si x P 1-x O4(1)

[0020] (Equation (1) satisfies 0<x<1.)

[0021] (2) In the all-solid secondary battery of the above aspect, the diameter of the first void may be 0.01 μm or more and 3.0 μm or less.

[0022] (3) In the all-solid secondary battery of the above aspect, the volume ratio of the first voids formed in contact with the Ag-containing phase in the negative electrode layer may be 1% to 10%.

[0023] (4) In the all-solid secondary battery of the above aspect, an aspect ratio of a length of the void in the direction in which the negative electrode layer extends to a length of the first void in a stacking direction of the stack may be 3 or more.

[0024] (5) In the all-solid secondary battery of the above aspect, at least a portion of the voids formed in contact with the Ag-containing phase may be second voids formed at an interface between the solid electrolyte layer and the Ag-containing phase.

[0025] (6) In the all-solid secondary battery of the above aspect, the ratio of the second voids to the entire first voids may be 80 to 100%.

[0026] (7) In the all-solid secondary battery of the above aspect, the negative electrode layer may be composed of the phase containing Ag.

[0027] (8) In the above-mentioned all-solid-state secondary battery, the negative electrode layer may also have: a first phase composed of the phase containing Ag, and a second phase composed of lithium titanate and sandwiching the first phase in the stacking direction, and the negative electrode layer forms a third gap connected to the interface between the first phase and the second phase.

[0028] (9) In the all-solid secondary battery of the above aspect, the ratio of the third voids to the entire first voids may be 50 to 100%.

[0029] Effects of the Invention

[0030] The all-solid secondary battery of the above embodiment can relax the stress caused by the expansion and contraction of the negative electrode and improve the cycle characteristics. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a cross-sectional view schematically showing the all-solid secondary battery according to the present embodiment.

[0032] Figure 2 Yes Figure 1 An enlarged cross-sectional view of the negative electrode layer of an all-solid-state secondary battery.

[0033] Figure 3 Yes Figure 1An enlarged cross-sectional view of the vicinity of the negative electrode layer of the all-solid secondary battery of the modified example.

[0034] Description of Reference Numerals

[0035] 1……Positive electrode layer

[0036] 1A……Positive electrode collector

[0037] 1B……Positive electrode active material layer

[0038] 2……Negative electrode layer

[0039] 3…Solid electrolyte layer

[0040] 4...Laminated

[0041] 5…Positive terminal

[0042] 6……Negative terminal

[0043] 10……All-solid-state secondary battery

[0044] V...Void

[0045] L Vx ...the length of the gap in the direction in which the negative electrode layer extends

[0046] L Vz ...the length of the gap in the stacking direction of the stacked body

[0047] 21……Phase containing Ag (first phase)

[0048] 22… Second phase

[0049] 31……LSPO

[0050] 41...The First Gap

[0051] 41a...Second gap

[0052] 41b... The third gap

[0053] 42……Gaps not connected to the phase containing Ag DETAILED DESCRIPTION

[0054] Hereinafter, the all-solid secondary battery of the present embodiment will be described in detail with reference to the accompanying drawings as appropriate. In the drawings used in the following description, in order to make the features of the present invention easy to understand, the features are sometimes enlarged for convenience. Therefore, the size ratio of each component is sometimes different from the actual. The materials, dimensions, etc. illustrated in the following description are examples, and the present invention is not limited to these, and can be implemented by appropriate changes within the scope of not changing its purpose.

[0055] [All-solid-state secondary battery]

[0056] Figure 1 It is a cross-sectional view schematically showing the all-solid secondary battery according to the present embodiment. Figure 2 Yes Figure 1 An enlarged cross-sectional view of the negative electrode layer of the all-solid secondary battery. Figure 2 An enlarged view schematically showing the vicinity of one void is also shown.

[0057] Figure 1 and Figure 2 The all-solid secondary battery 10 shown includes a stack 4, a positive terminal 5, and a negative terminal 6. The positive terminal 5 and the negative terminal 6 are respectively in contact with the opposite surfaces of the stack 4. The positive terminal 5 and the negative terminal 6 extend in a direction intersecting (orthogonal) with the stacking surface of the stack 4. In the present embodiment, the direction in which the negative electrode layer 2 extends is sometimes referred to as the x direction, the direction in which the stack 4 is stacked is sometimes referred to as the z direction, and the direction orthogonal to the x direction and the z direction is sometimes referred to as the y direction.

[0058] The laminate 4 includes a positive electrode layer 1, a negative electrode layer 2, and a solid electrolyte layer 3 sandwiched between the positive electrode layer 1 and the negative electrode layer 2. The laminate 4 is a sintered body formed by laminating and sintering the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3. The number of layers of the positive electrode layer 1 and the negative electrode layer 2 contained in the laminate 4 may be one layer each, or may be two or more layers. Figure 1 As shown, the solid electrolyte layer 3 is not only between the positive electrode layer 1 and the negative electrode layer 2, but also between the positive electrode layer 1 and the negative electrode terminal 6, and between the negative electrode layer 2 and the positive electrode terminal 5. Figure 1 As shown, one end of the positive electrode layer 1 is connected to a positive electrode terminal 5 , and one end of the negative electrode layer 2 is connected to a negative electrode terminal 6 .

[0059] The all-solid secondary battery 10 is charged or discharged by transferring ions between the positive electrode layer 1 and the negative electrode layer 2 via the solid electrolyte layer 3. Figure 1 The laminated all-solid secondary battery 10 shown will be described as an example.

[0060] <Solid Electrolyte Layer>

[0061] The solid electrolyte layer 3 can move ions by an electric field applied from the outside. The solid electrolyte layer 3 conducts lithium ions, for example, and blocks the movement of electrons. The solid electrolyte layer 3 includes LSPO represented by the following formula (1).

[0062] Li 3+x Si x P 1-x O4(1)

[0063] (In formula (1), x is a number such that 0<x<1.)

[0064] Solid electrolyte layer 3 contains LSPO as a main component, for example, and is preferably composed of LSPO. In this embodiment, solid electrolyte layer 3 containing LSPO as a main component means that LSPO in solid electrolyte layer 3 accounts for 80 volume % or more.

[0065] <Positive Electrode Layer>

[0066] The positive electrode layer 1 includes, for example, a positive electrode current collector 1A and a positive electrode active material layer 1B. Figure 1 As shown, the positive electrode active material layer 1B may be formed on both surfaces of the positive electrode current collector 1A, or may be formed on only one surface.

[0067] (Positive electrode collector)

[0068] The positive electrode collector 1A is made of a material with high conductivity. The positive electrode collector 1A includes, for example, metals such as silver, palladium, gold, platinum, aluminum, copper, nickel, stainless steel, iron, and their alloys, conductive resins, and other conductive materials. The positive electrode collector 1A may also contain, for example, positive electrode active materials such as lithium cobalt oxide (LiCoO2), lithium vanadium compounds (LiV2O5, Li3V2(PO4)3, LiVOPO4), etc. The positive electrode collector 1A may also be in the form of powder, foil, stamped product, and extended product.

[0069] (Positive Electrode Active Material Layer)

[0070] The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive auxiliary agent or a solid electrolyte.

[0071] (Positive electrode active material)

[0072] The positive electrode active material is not particularly limited as long as it can reversibly release and adsorb lithium ions, and detach and insert lithium ions. For example, a positive electrode active material used in a known lithium ion secondary battery can be used.

[0073] The positive electrode active material is preferably one or two or more selected from, for example, composite transition metal oxides and transition metal composite oxides.

[0074] Examples of the positive electrode active material include lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese spinel (LiMn2O4), and a material having the general formula: LiNi x Co y Mn z M a O2 (x+y+z+a=1, 0≤x≤1, 0≤y≤1, 0≤z≤1, 0≤a≤1, M represents one or more elements selected from Al, Mg, Nb, Ti, Cu, Zn, Cr) represented by a composite metal oxide, lithium titanate (Li4Ti5O12 )wait.

[0075] As the positive electrode active material, a positive electrode active material that does not contain lithium can also be used. The positive electrode active material that does not contain lithium can be used by pre-arranging a negative electrode active material doped with metallic lithium and / or lithium ions in the negative electrode layer 2, and the all-solid secondary battery 10 is used from the start of discharge. As the positive electrode active material that does not contain lithium, for example, metal oxides (MnO2, V2O5, etc.) can be cited.

[0076] (Conductive additive)

[0077] The conductive aid is not particularly limited as long as it makes the electron conductivity in the positive electrode active material layer 1B good, and a known conductive aid can be used. The conductive aid can include, for example, carbon materials such as graphite, carbon black, graphene, and carbon nanotubes, metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron, conductive oxides such as ITO (indium tin oxide), or mixtures thereof. The conductive aid can also be in the form of powder or fiber.

[0078] The solid electrolyte contained in the positive electrode active material layer 1B makes the ion conductivity in the positive electrode active material layer 1B good. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. From the viewpoint of improving the adhesion between the solid electrolyte layer 3 and the positive electrode layer 1, it is preferred that the solid electrolyte use the same compound as the compound constituting the above-mentioned solid electrolyte layer 3.

[0079] <Negative Electrode Layer>

[0080] Figure 1 and Figure 2 The negative electrode layer 2 shown in the figure serves as both a negative electrode current collector and a negative electrode active material layer. The negative electrode layer 2 includes a phase 21 containing Ag, which is either Ag or an AgPd alloy, and may also contain lithium titanate (Li4Ti5O 12 The negative electrode layer 2 is composed of a base material having a lower potential than the positive electrode active material. The negative electrode layer 2 has a void V in contact with the phase 21 containing Ag.

[0081] The negative electrode layer 2 has, for example, a plurality of voids V. The plurality of voids V are classified into a first void 41 that is in contact with the phase 21 containing Ag and a void 42 that is not in contact with the phase 21 containing Ag. The first void 41 is further classified into a second void 41a and a third void 41b. The second void 41a is a void in contact with the interface between the solid electrolyte layer 3 and the phase 21 containing Ag. The third void 41b is a void in contact with the interface between the first phase 21 (phase 21 containing Ag) and the second phase 22 composed of lithium titanate.

[0082] The relationship between the second gap 41a and the third gap 41b is substantially mutually exclusive.

[0083] Each of the plurality of voids V is formed, for example, at a portion of the interface between the phase 21 containing Ag and the solid electrolyte of the solid electrolyte layer 3, and all of the voids V may also be formed, respectively, at a portion of the interface between the phase containing Ag and the solid electrolyte. That is, each of the plurality of voids V exists, for example, in contact with a portion of the interface between the phase 21 containing LSPO31 and Ag, and preferably, all of the voids V are in contact with a portion of the interface between the phase 21 containing LSPO31 and Ag. In addition, when the negative electrode layer 2 contains lithium titanate, each of the plurality of voids V may also be formed, for example, at a portion of the interface between the phase containing Ag and lithium titanate.

[0084] The volume ratio (void ratio) of the voids V in the negative electrode layer 2 is, for example, 0.1% to 20%, preferably 1% to 10%, and more preferably 1% to 5%.

[0085] The volume ratio of the first voids 41 in the negative electrode layer 2 may be 1% to 10%, or 1% to 5%.

[0086] The ratio of the second voids to the entire first voids may be 80% or more and 100% or less.

[0087] The ratio of the third voids to the entire first voids may be 50% to 100%, or 80% to 100%.

[0088] The volume ratio of the voids V in the negative electrode layer 2 was calculated based on the electron microscope image. Specifically, the region of the voids V in the negative electrode layer 2 was defined in the following procedure, and the volume ratio was calculated.

[0089] First, a scanning electron microscope image of a cross section parallel to the stacking direction of the stacked body 4 is obtained, and the region of the negative electrode layer 2 is delimited based on the scanning electron microscope image. The negative electrode layer 2 is considered to be the region located between the two solid electrolyte layers in the above scanning electron microscope image, and is delimited by image analysis. The area of ​​the negative electrode layer 2 is calculated by image analysis.

[0090] Next, by binarizing the above-mentioned scanning electron microscope image with brightness, the phase corresponding to the gap is separated from the phase corresponding to other areas. The binarization of the scanning electron microscope image is performed as follows: a concentration histogram is prepared by a pattern method, and the concentration domain of the valley corresponding to the boundary between the target phase and the other phases is used as a threshold. That is, the "dark part" and the "bright part" are distinguished by the threshold and binarization is performed. In addition, in the concentration histogram, more than two valleys are sometimes generated, but the above-mentioned gap is an area with low brightness in the scanning electron microscope image. It is only necessary to select the valley between the peak with the lowest brightness and the peak with low brightness after the peak as the valley equivalent to the boundary, and use the concentration value of the valley as the threshold.

[0091] The darkest area is considered to be a void. The total area of ​​the voids in the negative electrode layer 2 that are in contact with alloys such as AgPd or metals such as Ag can be calculated by image analysis. Here, the total area of ​​the voids and the negative electrode layer is obtained, for example, from the same scanning electron microscope image at a magnification of 1000 to 5000 times. In this way, the area of ​​the negative electrode layer 2 and the area of ​​the void V are calculated, and the volume ratio (void ratio) of the void V in the negative electrode layer 2 can be calculated by dividing the area of ​​the void V by the area of ​​the negative electrode layer 2.

[0092] In the present embodiment, the diameter of the void V is estimated as the diameter of the void V by assuming a circle having the same area as the region judged to be a void whose brightness is less than a predetermined value through the binarization process.

[0093] The length L of the gap in the direction in which the negative electrode layer 2 extends is Vx The length L of the gap V in the stacking direction of the stacked body 4 is Vz The aspect ratio (L Vx / L Vz ) is, for example, 1 or more, preferably 3 or more. The aspect ratio of each void V is calculated by performing image analysis on an electron microscope image binarized in the same manner as in the above step. That is, by performing image analysis on the void V defined by binarizing the electron microscope image, the length L in the direction in which the negative electrode layer 2 extends is calculated. Vx and the length L in the stacking direction Vz Next, the length L of each gap V Vz Divide by the length L Vzx , and calculate the aspect ratio of each void V. In this embodiment, the aspect ratios of the voids V are calculated for any 10 voids V in the electron microscope image, and their arithmetic average is taken as the length L of the voids V in the direction in which the negative electrode layer 2 extends. Vx The length L of the gap V in the stacking direction of the stacked body 4 is Vz aspect ratio to handle.

[0094] The voids V in the negative electrode layer 2 preferably have an axial direction in the direction in which the negative electrode layer 2 extends. For example, it is preferred that the aspect ratio (L Vx / L Vz ) is a value greater than 1, and the extension direction of the gap is roughly parallel to the extension direction of the negative electrode layer 2.

[0095] The plurality of voids V in the negative electrode layer 2 are preferably connected to each other to form a network structure. In addition, the voids V in the negative electrode layer 2 preferably have the above-mentioned network structure and are connected to the AgPd alloy particles in the x direction and the z direction. The voids having such a structure can easily relax stress in various directions.

[0096] The negative electrode layer 2 may contain a conductive additive, a solid electrolyte, and the like in addition to at least one of the metal particles and the alloy particles described above.

[0097] (Conductive additive)

[0098] The conductive auxiliary agent improves the electron conductivity of the negative electrode layer 2. As the conductive auxiliary agent, the same material as that of the positive electrode active material layer 1B can be used.

[0099] (Solid Electrolyte)

[0100] The solid electrolyte contained in the negative electrode layer 2 improves the ion conductivity in the negative electrode layer 2. As the solid electrolyte, one or a mixture of two or more known solid electrolytes can be used. As the solid electrolyte, the same compound as the compound forming the above-mentioned solid electrolyte layer 3 can also be contained.

[0101] [Method for manufacturing all-solid-state secondary battery]

[0102] Next, an example of a method for producing the all-solid secondary battery 10 will be described.

[0103] First, the laminate 4 is produced. The laminate 4 can be produced, for example, by firing, or by any of a simultaneous firing method and a sequential firing method. The simultaneous firing method is a method of producing the laminate 4 by stacking the materials forming each layer and then firing them all at once. The sequential firing method is a method of performing firing each time each layer is formed. The simultaneous firing method can produce the laminate 4 with fewer operating steps than the sequential firing method. In addition, the laminate 4 produced by the simultaneous firing method is denser than the laminate 4 produced by the sequential firing method. The following is a description of a method for producing the laminate 4 when the simultaneous firing method is used to produce the laminate 4.

[0104] First, the materials constituting the positive electrode current collector 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3 and the negative electrode layer 2 of the laminate 4 are made into pastes to prepare pastes corresponding to the materials of each layer.

[0105] In the manufacturing method of the all-solid secondary battery of the present embodiment, in order to form a plurality of voids in contact with the phase containing Ag in the negative electrode layer 2 and control the amount, shape, and size thereof, the following method is used, for example. In order to control the amount of voids V in the negative electrode layer 2, for example, an organic filler is added to the negative electrode active material to change its amount. In order to control the shape of the voids in the negative electrode layer 2, for example, the flatness of the organic filler is changed, and an organic filler with high flatness is used to obtain a void with a high aspect ratio. In addition, in order to control the direction of the voids in the negative electrode, for example, the organic filler can be arranged in the in-plane direction during coating to control it. Specifically, a scraper method is used to control the degree of orientation by the coating speed and coating thickness. In order to control the size of the voids in the negative electrode layer, for example, the size of the added organic filler is controlled, and by using a large filler, the size of the voids also becomes larger.

[0106] The method for making each material for manufacturing the laminate 4 into a paste is not particularly limited, and for example, a method of mixing the powders of each material in a carrier to obtain a paste can be used. Here, the carrier is a general term for a medium in a liquid phase. The carrier in this embodiment includes, for example, a solvent, a binder, and a plasticizer. As a solvent, for example, dihydroterpineol can be used. As a binder, for example, ethyl cellulose can be used.

[0107] Next, green sheets corresponding to the layers constituting the laminate 4 are prepared. The green sheets are obtained, for example, by applying pastes prepared from the materials constituting the layers of the laminate 4 onto a substrate such as a PET (polyethylene terephthalate) film, drying the pastes as needed, and then peeling the pastes off the substrate.

[0108] The method for applying the paste onto the substrate is not particularly limited, and for example, a known method such as screen printing, coating, transfer, and doctor blade method can be used.

[0109] Next, the raw sheets corresponding to the layers constituting the laminate 4 are stacked in a desired order and number of stackings to produce a laminated sheet material for the laminate 4. When stacking the raw sheets, alignment and cutting are performed as needed. For example, as a fully solid secondary battery 10, when a parallel type or a series-parallel type battery is produced, the raw sheets corresponding to the layers are stacked by aligning the end face of the positive electrode collector 1A and the end face of the negative electrode layer 2 in a manner that is inconsistent.

[0110] The green sheets used as the laminated sheets may be the positive electrode units and negative electrode units produced in advance.

[0111] The positive electrode unit is a green sheet in which the solid electrolyte layer 3 , a sheet to be the positive electrode active material layer 1B, a sheet to be the positive electrode current collector 1A, and a sheet to be the positive electrode active material layer 1B are sequentially stacked.

[0112] The structure of the negative electrode unit can be changed according to the desired negative electrode layer. For example, it is a raw sheet formed by stacking in sequence a second negative electrode paste which will become a second phase containing lithium titanate as the main component, a first negative electrode paste which will become a first phase containing a phase containing Ag as the main component, and a second negative electrode paste which will become a second phase containing lithium titanate as the main component.

[0113] When a positive electrode unit is used, a laminated sheet to be the laminated body 4 can be produced by laminating a positive electrode unit and a negative electrode unit to be the negative electrode layer 2 via a solid electrolyte green sheet.

[0114] Next, the produced laminated sheets are pressurized together to improve the adhesion of each layer and form a laminate. Pressing can be performed, for example, using a molding machine, a warm isostatic press (WIP), a cold isostatic press (CIP), an isostatic press, etc. Pressing is preferably performed while heating. The heating temperature during pressurization can be set to 40 to 95° C., for example. Next, the laminated body obtained after pressurization is cut using a cutting device to form a laminated chip. Then, the obtained laminated chip is sintered. Thus, a laminated body 4 consisting of a sintered body can be obtained.

[0115] The debinding and firing process can be performed, for example, by placing the laminate on a ceramic table. The debinding and firing process can be performed, for example, by heating to 550° C. to 1100° C. in an air atmosphere. The heating time (firing time) can be, for example, 0.1 hour to 10 hours. The heating temperature and firing time in the debinding and firing process can be appropriately determined according to the composition of each layer constituting the laminate 4, etc.

[0116] The sintered laminate 4 (sintered body) may also be placed in a cylindrical container together with an abrasive such as alumina and ground by a drum grinding method. Thus, the corners of the laminate 4 can be chamfered. The grinding of the laminate 4 may also be performed by sandblasting. Sandblasting is preferred because it can only remove a specific portion of the surface of the laminate 4.

[0117] Next, a positive electrode terminal 5 and a negative electrode terminal 6 are formed on the mutually opposing sides of the produced laminate 4. The positive electrode terminal 5 and the negative electrode terminal 6 are formed by methods such as sputtering, dipping, screen printing, spraying, etc. The all-solid secondary battery 10 is manufactured through the above steps.

[0118] According to the all-solid secondary battery 10 of the present embodiment, as described above, by forming a solid electrolyte layer 3 containing LSPO, a negative electrode layer 2 containing a phase 21 containing Ag, and a gap V in which the negative electrode layer 2 and the phase 21 containing Ag are connected, the gap V can be used to alleviate the stress of expansion and contraction of the phase 21 containing Ag in the negative electrode layer 2 during charging and discharging, thereby suppressing the formation of a reaction layer, and suppressing the generation of cracks in the solid electrolyte layer 3 or peeling between layers, thereby obtaining excellent cycle characteristics.

[0119] Although one embodiment of the present invention has been described in detail above, each structure and combination thereof in each embodiment are merely examples, and addition, omission, substitution, and other changes of structures may be made without departing from the gist of the present invention.

[0120] For example, in Figure 1 In the figure, a fully solid secondary battery 10 is shown in which the negative electrode layer 2 serves as both a negative electrode current collector and a negative electrode active material layer, but a fully solid secondary battery in which the negative electrode layer has a separate negative electrode current collector and a negative electrode active material can also be used. For such a fully solid secondary battery, for example, a fully solid secondary battery in which a negative electrode active material layer is provided on both sides of the main surface of the negative electrode current collector can also be made.

[0121] In addition, for example, the all-solid secondary battery of the above embodiment may also be a structure in which the negative electrode layer 2 has a stacked structure of a negative electrode active material layer and a negative electrode collector. In the case where the negative electrode layer 2 is a stacked structure of a negative electrode active material layer and a negative electrode collector, for example, the phase 21 containing Ag is contained in the negative electrode active material layer, and a gap V is formed in a manner that is in contact with the phase 21 containing Ag. In this case, the phase 21 containing Ag may also be contained in the negative electrode collector, and the gap V may be formed in a manner that is in contact with a portion of the phase 21 containing Ag in the negative electrode collector.

[0122] Alternatively, for example, the first phase 21 may include the phase 21 containing Ag and the second phase 22 may include lithium titanate. Figure 3 A cross-sectional view of an all-solid secondary battery satisfying the above structure, that is, an all-solid secondary battery after the negative electrode layer is enlarged. In this case, the negative electrode layer is, for example, a structure in which a phase 21 containing Ag as a first phase is clamped by a second phase 22 such as lithium titanate in the z direction, and is in contact with the interface between the phase 21 containing Ag as the first phase and the second phase 22 to form a gap V. In addition, the first phase and the second phase may exist adjacent to each other in layers, and a portion of the first phase may be located outside the second phase in the z direction so that a portion of the first phase becomes closer to the solid electrolyte layer 3 than the second phase, or may be in contact with the interface between the first phase and the second phase to form a gap, or may be a structure formed by combining them.

[0123] In such a modification, the amount and structure of the voids may be the same as those of the all-solid secondary battery 10 of the above embodiment. In addition, the proportion of voids in contact with the AgPd alloy among the plurality of voids included in the stacked body 4 is preferably 50% or more.

[0124] The voids V preferably exist at the boundary between the Ag-containing phase 21 and lithium titanate, or at the boundary between the Ag-containing phase 21 and the solid electrolyte layer 3. If voids exist at other locations, stress caused by expansion and contraction of the negative electrode cannot be relieved, and improvement in cycle characteristics is not seen.

[0125] Example

[0126] Hereinafter, examples of the present invention will be described. However, the present invention is not limited to the following examples.

[0127] [Example 1]

[0128] (1) Preparation of solid electrolyte paste

[0129] First, prepare the solid electrolyte paste according to the following procedure. 3+x Si x P 1-x Particles composed of O4 (x in formula (1) is 0.5), ethyl cellulose and dihydroterpineol were added to a ball mill and wet mixed to obtain a solid electrolyte paste.

[0130] (2) Preparation of positive electrode collector paste

[0131] A powder of an AgPd alloy with a ratio of Ag:Pd=8:2, ethyl cellulose, and dihydroterpineol were added to a ball mill and wet mixed to prepare a positive electrode current collector paste of Example 1.

[0132] (3) Preparation of positive electrode active material paste

[0133] Lithium cobalt oxide (LiCoO2) powder, ethyl cellulose and dihydroterpineol were added to a ball mill and wet mixed to prepare the positive electrode active material paste of Example 1.

[0134] (4) Preparation of negative electrode paste

[0135] AgPd powder, polymer particles, ethyl cellulose and dihydroterpineol, which are composed of an AgPd alloy with a ratio of Ag:Pd=8:2, were added to a ball mill for wet mixing to prepare a first negative electrode paste. The volume ratio of AgPd powder to polymer particles was set to 95:5, and as polymer particles, particles with an aspect ratio of 1:3 and a particle size of 0.5 μm when the same volume is converted into a true sphere were used.

[0136] Separately, lithium titanate powder, ethyl cellulose, and dihydroterpineol were added to a ball mill and wet-mixed to prepare a second negative electrode paste.

[0137] (5) Fabrication of positive electrode unit to become positive electrode layer

[0138] On a substrate composed of a PET (polyethylene terephthalate) film, a positive electrode active material layer paste with a thickness of 5 μm was applied by screen printing, and dried at 80°C for 5 minutes. On the dried positive electrode active material layer paste, a positive electrode collector paste with a thickness of 5 μm was applied by screen printing, and dried at 80°C for 5 minutes. On the dried positive electrode collector paste, a positive electrode active material layer paste with a thickness of 5 μm was applied by screen printing, and dried at 80°C for 5 minutes, and then peeled off from the substrate. Thus, a positive electrode unit in which a positive electrode active material layer, a positive electrode collector layer, and a positive electrode active material layer are stacked in sequence is obtained.

[0139] (6) Preparation of solid electrolyte green sheets

[0140] The solid electrolyte paste was applied to a substrate composed of a PET (polyethylene terephthalate) film to a thickness of 20 μm by screen printing, dried at 80° C. for 10 minutes, and then peeled from the substrate. Thus, a solid electrolyte green sheet serving as a solid electrolyte layer was obtained.

[0141] (7) Preparation of Negative Electrode Unit to Become Negative Electrode Layer

[0142] On a substrate composed of a PET (polyethylene terephthalate) film, a second negative electrode paste with a thickness of 5 μm was applied by screen printing and dried at 80°C for 5 minutes. On the dried second negative electrode paste, a first negative electrode paste with a thickness of 5 μm was applied by screen printing and dried at 80°C for 5 minutes. On the dried second negative electrode paste, a second negative electrode paste with a thickness of 5 μm was applied by screen printing, dried at 80°C for 5 minutes, and then peeled off from the substrate. Thus, a negative electrode unit in which the second negative electrode layer, the first negative electrode layer, and the second negative electrode layer are stacked in sequence is obtained.

[0143] (8) Formation of Laminated Body

[0144] 25 positive electrode units and 25 negative electrode units are alternately stacked in a manner of sandwiching solid electrolyte green sheets to obtain a laminated sheet material that becomes a laminate. In addition, the top and bottom of the laminated sheet material are stacked in a manner of forming a solid electrolyte unit. In addition, the top and bottom of the laminated sheet material are stacked in a manner of forming a solid electrolyte green sheet. In addition, the positive electrode unit is stacked in a staggered manner so that only one end face of the laminated sheet material is extended, and the negative electrode unit is extended only on the end face of the opposite side.

[0145] Next, the green sheets were pressed together and cut using a cutting device to produce a laminated chip. Then, the laminated chip was debonded and fired to obtain a laminated body of Example 1 consisting of a sintered body. The debonding treatment was performed by heating the laminated body at 500° C. for 10 hours in an atmospheric atmosphere. The firing was performed at 900° C. for 1 hour in an atmospheric atmosphere. The debonding and firing can be performed in a single process.

[0146] Next, a positive terminal and a negative terminal were formed on a pair of opposite sides of the produced laminate by Au sputtering, thereby obtaining the all-solid secondary battery of Example 1. Here, the positive terminal and the negative terminal were formed in such a way that the positive terminal was joined to the positive electrode unit, and the negative terminal was joined to the negative electrode unit.

[0147] [Example 2]

[0148] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 0.005 μm.

[0149] [Example 3]

[0150] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 0.05 μm.

[0151] [Example 4]

[0152] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 1 μm.

[0153] [Example 5]

[0154] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 5 μm.

[0155] [Example 6]

[0156] An all-solid secondary battery was produced in the same manner as in Example 1, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 99.9:0.1.

[0157] [Example 7]

[0158] An all-solid secondary battery was produced in the same manner as in Example 1, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 99:1.

[0159] [Example 8]

[0160] An all-solid secondary battery was produced in the same manner as in Example 1, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 90:10.

[0161] [Example 9]

[0162] An all-solid secondary battery was produced in the same manner as in Example 1, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 80:20.

[0163] [Example 10]

[0164] An all-solid secondary battery was produced in the same manner as in Example 1 except that the aspect ratio of the polymer particles in the first negative electrode paste was changed to 1:1.

[0165] [Example 11]

[0166] An all-solid secondary battery was produced in the same manner as in Example 1, except that the aspect ratio of the polymer particles in the first negative electrode paste was changed to 1:10.

[0167] [Example 12]

[0168] A fully solid secondary battery was produced by the same method as in Example 1 except that the negative electrode layer was formed without using the second negative electrode paste. With this change, the negative electrode layer was substantially composed of AgPd alloy and lithium titanate in Examples 1 to 11, but was substantially changed to a structure composed of AgPd alloy.

[0169] [Example 13]

[0170] A fully solid secondary battery was produced in the same manner as in Example 12 except that the aspect ratio of the polymer particles in the first negative electrode paste was changed to 1:10. Example 13 was the same as in Example 12, except that the negative electrode layer was substantially composed of an AgPd alloy.

[0171] [Example 14]

[0172] An all-solid secondary battery was produced in the same manner as in Example 1, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 89:11.

[0173] [Example 15]

[0174] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 0.01 μm.

[0175] [Example 16]

[0176] An all-solid secondary battery was produced in the same manner as in Example 1 except that the particle size of the polymer particles in the first negative electrode paste was changed to 3 μm.

[0177] [Example 17]

[0178] An all-solid secondary battery was produced in the same manner as in Example 1 except that the aspect ratio of the polymer particles in the first negative electrode paste was changed to 1:5.

[0179] [Example 18]

[0180] An all-solid secondary battery was produced in the same manner as in Example 12, except that the volume ratio of the AgPd powder to the polymer particles in the first negative electrode paste was changed to 99:1.

[0181] [Example 19]

[0182] An all-solid secondary battery was produced in the same manner as in Example 12, except that the volume ratio of the AgPd powder and the polymer particles in the first negative electrode paste was changed to 90:10.

[0183] [Example 20]

[0184] An all-solid secondary battery was produced in the same manner as in Example 12 except that the particle size of the polymer particles in the first negative electrode paste was changed to 0.01 μm.

[0185] [Example 21]

[0186] An all-solid secondary battery was produced in the same manner as in Example 12 except that the particle size of the polymer particles in the first negative electrode paste was changed to 3 μm.

[0187] [Comparative Example 1]

[0188] An all-solid secondary battery was produced in the same manner as in Example 1, except that the polymer particles were not added to the first negative electrode paste.

[0189] [Comparative Example 2]

[0190] In addition to the use of Li 1.3 Al 0.3 Ti 1.7An all-solid secondary battery was produced in the same manner as in Example 1 except that solid electrolyte particles composed of (PO4)3, ethyl cellulose and dihydroterpineol were added to a ball mill and wet mixed to produce a solid electrolyte paste.

[0191] [Comparative Example 3]

[0192] An all-solid secondary battery was produced in the same manner as in Example 12, except that the polymer particles were not added to the first negative electrode paste.

[0193] [Comparative Example 4]

[0194] In addition to the use of Li 1.3 Al 0.3 Ti 1.7 An all-solid secondary battery was produced in the same manner as in Example 12 except that (PO4)3-constituting solid electrolyte particles, ethyl cellulose and dihydroterpineol were added to a ball mill and wet mixed to produce a solid electrolyte paste.

[0195] <Analysis of all-solid-state secondary batteries>

[0196] The all-solid secondary battery produced by the above method was analyzed according to the following procedures.

[0197] (Cyclic test)

[0198] Cycle tests of the all-solid secondary batteries 10 of Examples 1 to 20 and Comparative Examples 1 to 4 were performed using an electrochemical tester (manufactured by Hokuto Denko Co., Ltd.) by the method described below.

[0199] In an environment of 60°C, constant current charging (CC charging) is performed at a constant current of 100μA until the battery voltage reaches 3.9V, and then constant current discharging (CC discharging) is performed at a constant current of 100μA until the battery voltage reaches 0V. This process is set as one cycle, and the cycle process is repeated 10 times. The discharge capacitance (μAh) of the 10th cycle is set as the initial capacitance Q1.

[0200] The all-solid secondary battery with the initial capacitance Q1 obtained was charged again at 60°C with a constant current of 100μA (CC charging) until the battery voltage reached 3.9V, and discharged with a constant current of 100μA (CC discharging) until the battery voltage reached 0V. The above charge and discharge were counted as one cycle, and 1000 cycles of charge and discharge were performed. Then, the discharge capacitance Q2 after 1000 cycles of charge and discharge was obtained.

[0201] From the discharge capacities Q1 and Q2 thus obtained, the capacitance retention rate E after 1000 cycles was obtained using the following formula. Table 1 shows the results.

[0202] E(%)=(Q2 / Q1)×100

[0203] (Structural Analysis)

[0204] The structures of the all-solid secondary batteries of Examples 1 to 13 and Comparative Example 1 before charge and discharge were analyzed using a scanning electron microscope (manufactured by Hitachi High-Tech Corporation, model: S-4800). Specifically, first, for the all-solid secondary batteries of Examples 1 to 13 and Comparative Example 1, scanning electron microscope images of the cross sections parallel to the stacking direction were obtained. The observation conditions under the scanning electron microscope were set to an acceleration voltage of 10 kV. In Examples 1 to 11, a battery having Figure 3 The negative electrode structure of the all-solid secondary battery is shown. Figure 3 For the convenience of explanation, the Figure 1 The symbols corresponding to the structures described in . Figure 3 In Example 1, a negative electrode layer is made of a material containing a mixture of an AgPd alloy and lithium titanate as a main component, and a negative electrode layer 2 having a first phase of an AgPd alloy as a phase 21 containing Ag is sandwiched by a second phase 22 containing lithium titanate, thereby forming a structure sandwiched by a solid electrolyte layer 3. In Examples 12 and 13, a negative electrode layer is made of a material containing an AgPd alloy as a main component, thereby forming a structure having Figure 1 and Figure 2 The all-solid secondary battery of the structure shown is an all-solid secondary battery in which the negative electrode layer 2 is composed of a phase 21 containing Ag.

[0205] By binarizing these scanning electron microscope images with brightness using a pattern method, the area where the voids are formed is delineated. Then, the area sandwiched by the solid electrolyte layer is used as the negative electrode layer. In Examples 1 to 13, most of the voids are in contact with AgPd. In Comparative Example 1, no voids were confirmed. In addition, in Examples 1 to 11, a portion of the interface between the first phase and the second phase is in contact with the voids, and in Examples 12 and 13, a portion of the interface between the phase containing Ag and the solid electrolyte is in contact with the voids.

[0206] Next, based on the scanning electron microscope image obtained by binarization, the area of ​​the negative electrode layer and the area of ​​the voids in the same scanning electron microscope image (magnification: 5000 times) are calculated by image analysis, and the area of ​​the voids is divided by the area of ​​the negative electrode layer to calculate the void ratio occupied by the voids in the negative electrode layer, which is regarded as the volume ratio of the voids in the negative electrode layer. In addition, the arithmetic mean of the areas of all voids in the scanning electron microscope image is calculated, and the diameter of a circle with the same area as the arithmetic mean is calculated. In addition, the length of the voids in the stacking direction of the stack and the length of the voids in the direction in which the negative electrode layer extends are measured, and the length of the voids in the direction in which the negative electrode layer extends is divided by the length of the voids in the stacking direction of the stack, thereby calculating the aspect ratio (L Vx / L Vz ).

[0207] Table 1 summarizes the measurement results of Examples 1 to 13 and Comparative Example 1.

[0208] [Table 1]

[0209]

[0210] According to Table 1, it can be confirmed that Examples 1 to 13 of the all-solid secondary battery in which the solid electrolyte layer contains LSPO, the negative electrode layer contains Ag or Ag alloy, and the negative electrode layer has voids formed at a portion of the interface between LSPO and the phase containing Ag, can significantly improve the cycle characteristics compared to the all-solid secondary battery of Comparative Example 1 in which no voids are formed at a portion of the interface between LSPO and the phase containing Ag.

[0211] In addition, it can be confirmed that Examples 1, 7, and 8, in which the void ratio in the negative electrode layer is 1% or more and 10% or less, can obtain higher cycle characteristics compared with Example 6, in which the void ratio in the negative electrode layer is 0.05%, and Example 9, in which the void ratio in the negative electrode layer is 20%. This indicates that if the void ratio in the negative electrode layer is small, the stress caused by the expansion and contraction caused by the charge and discharge of the negative electrode is not sufficiently relieved, and if there are many voids, the voids may be connected to each other due to stress.

[0212] In the all-solid secondary batteries of Examples 1 to 9 and 11 to 13, the aspect ratio of the void is greater than 1, and it can be confirmed from its electron microscope image that a plurality of voids have an axial direction in a direction substantially parallel to the direction in which the negative electrode layer extends. By configuring such a void in contact with the AgPd alloy, the expansion and contraction of the void can be effectively mitigated and the cycle characteristics can be improved compared to the void having an axis in the stacking direction. This effect is confirmed by the following: Compared with Example 10 having an aspect ratio of 1, Example 1 having an aspect ratio of 3 can obtain higher cycle characteristics.

[0213] Industrial Applicability

[0214] Compared with existing technologies, it can provide all-solid-state batteries with high safety and excellent characteristics.

Claims

1. An all-solid secondary battery, wherein: A laminated body is provided, the laminated body comprising: a positive electrode layer, a negative electrode layer, and a solid electrolyte layer located between the positive electrode layer and the negative electrode layer, The solid electrolyte layer contains a compound represented by the following formula (1): The negative electrode layer comprises a phase containing Ag, A plurality of gaps are formed in the negative electrode layer, At least a portion of the voids is a first void formed by contact with the Ag-containing phase, Li 3+x Yes x P 1-x O4(1) Formula (1) satisfies 0<x<1.

2. The all-solid secondary battery according to claim 1, wherein: The diameter of the first voids is not less than 0.01 μm and not more than 3.0 μm.

3. The all-solid secondary battery according to claim 1 or 2, wherein: The volume ratio of the first voids formed in the negative electrode layer and in contact with the phase containing Ag is 1% to 10%.

4. The all-solid secondary battery according to claim 1 or 2, wherein: An aspect ratio of a length of the void in a direction in which the negative electrode layer extends to a length of the first void in a stacking direction of the stacked body is 3 or more.

5. The all-solid secondary battery according to claim 1 or 2, wherein: At least a portion of the voids formed in contact with the phase containing Ag are second voids formed at the interface between the solid electrolyte layer and the phase containing Ag.

6. The all-solid secondary battery according to claim 1 or 2, wherein: The proportion of the second gap to the entire first gap is 80 to 100%.

7. The all-solid secondary battery according to claim 1 or 2, wherein: The negative electrode layer is composed of the phase containing Ag.

8. The all-solid secondary battery according to claim 1 or 2, wherein: The negative electrode layer includes a first phase composed of the phase containing Ag and a second phase composed of lithium titanate and sandwiching the first phase in a stacking direction. The negative electrode layer has a third gap formed therein that is in contact with an interface between the first phase and the second phase.

9. The all-solid secondary battery according to claim 7, wherein: The proportion of the third gap to the entire first gap is 50 to 100%.

Citation Information

Patent Citations

  • All-solid battery

    JP2022025903A