Production method of steel-aluminum composite anode claw
High temperature and pressure promote the diffusion of liquid aluminum atoms to realize the metallurgical bonding of the outer steel layer of the anode claw and the aluminum core. This solves the problem of balancing the electrical conductivity and mechanical properties of the anode claw, improves the casting quality and metal utilization rate of the aluminum core, and reduces the cost of the aluminum core. Resistivity and production costs.
Patent Information
- Application Number
- CN202411081817.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-15
AI Technical Summary
It is difficult to balance the improvement of electrical conductivity and mechanical properties of existing anode claws, resulting in high production costs and unstable production of electrolytic aluminum.
High temperature and pressure are used to promote the atomic diffusion of the aluminum liquid in the inner core, to achieve the metallurgical bonding of the outer steel layer and the aluminum core, to isolate the air to avoid oxidation of the aluminum liquid, and to ensure the metallurgical bonding and feeding of the aluminum liquid through induction heating and gas pressure.
The electrical conductivity and mechanical properties of the anode claw are improved, the resistivity is reduced, the casting quality of the aluminum core is enhanced, the oxidation of the aluminum liquid is avoided, and the metal utilization rate is improved.
Smart Images

Figure CN118768549A_ABST
Abstract
Description
Technical Field
[0001] The invention is applied to the field of electrolytic aluminum and relates to an anode steel claw of an aluminum electrolytic cell, specifically a method for producing a steel-aluminum composite or steel-copper composite anode claw. Background Art
[0002] Anode claws for electrolytic aluminum are crucial components connecting the guide rods and carbon blocks in the electrolytic cell. They are structurally and functionally integrated materials that require excellent electrical conductivity and mechanical properties. They must withstand the high currents flowing into the cell during aluminum electrolysis production, with the average current flowing through each steel claw reaching approximately 15,000A. Therefore, they require excellent electrical conductivity. Furthermore, the claws connect the aluminum guide rods and hold the anode carbon blocks. Because each anode weighs 700 to 1,000 kg, they require a certain level of strength and dimensional stability.
[0003] Aluminum and copper have excellent electrical conductivity, but their mechanical properties are inferior to steel. Electrical conductivity primarily affects the production cost of electrolytic aluminum, while mechanical properties directly impact its normal production. Therefore, most anode claws are currently made of steel. To improve the conductivity of anode steel claws, some patent applications address the production process or steel composition. For example, CN117340548A discloses a production process for low-resistivity, high-performance anode steel claws made from BTCY-1 hot-rolled steel. Friction welding is employed, achieving a weld fusion rate of 99% or greater and a resistivity of less than 11 μΩ·mm at 20°C. CN117626137A discloses a low-resistivity, energy-saving dual anode steel claw and its preparation method. The iron-carbon alloy is reinforced with 235B steel plates, with impurity content within the following ranges: C ≤ 0.005%, Mn ≤ 0.10%, Si ≤ 0.01%, 0.003% ≤ P ≤ 0.005%, and S ≤ 0.007%. The invention patent "A Method for Producing Anode Steel Claws" (2024105474652) applied for by the applicant earlier took process measures from multiple aspects such as alloy elements, impurities, casting defects, organization, and grain size to improve the conductive performance.
[0004] Some patent applications use steel-aluminum composite materials to reduce resistivity. For example, CN116926629A discloses an anode conductive device and its steel-aluminum connection method, a steel-aluminum connection structure, and a steel-aluminum composite sheet. The steel sheet of the steel-aluminum composite sheet includes a steel transverse joint and a steel claw joint, and the aluminum sheet includes an aluminum transverse joint and an aluminum guide rod joint. The transverse joints of the steel and aluminum are tightly combined to form a "steel-aluminum transverse joint structure" and a weld fillet accommodating notch. When the steel-aluminum composite sheet is in use, the weld fillet accommodating notch ensures that each composite sheet can be stacked and arranged tightly, not only achieving high connection strength but also greatly reducing resistance and contact voltage drop. CN203999844U discloses a steel-aluminum composite anode steel claw, which includes a channel-shaped steel frame, a steel pipe above the channel-shaped steel frame, and a round steel claw below the channel-shaped steel frame. The round steel claw is provided with a casting hole that communicates with the channel-shaped steel frame. The casting holes of the steel pipe, channel-shaped steel frame, and round steel claw are all cast with an aluminum core, forming a steel-clad aluminum composite structure. The transverse round steel and reinforcing steel in the composite steel claw groove steel frame will restrict the shrinkage of cast aluminum, which is prone to shrinkage cracks. Moreover, large current still needs to pass through the round steel claws, and the shrinkage of cast aluminum cannot form a metallurgical bond with steel, so the effect of reducing power consumption is not obvious. CN101024885B discloses a manufacturing process for an anode steel claw crossbeam of an aluminum-steel composite structure. The core of this process is to directly spot weld the casting riser to the middle and upper part of the bottom of the steel crossbeam shell, cast it into the steel shell cavity with high-temperature molten aluminum, and simultaneously perform high-temperature treatment on the steel beam shell and the molten aluminum in a high-temperature furnace or a molten aluminum pot, so that the bonding interface between the aluminum core, the steel shell and the conductive plate will produce mutual infiltration under high temperature conditions, forming a metallurgical crystal bond between the two bonding interfaces of aluminum and steel. Summary of the Invention
[0005] The technical problem solved by the present invention is to provide a production method of steel-aluminum composite anode claws, which uses high temperature and pressure to promote atomic diffusion of the inner core aluminum liquid to achieve metallurgical bonding between the outer steel layer and the aluminum core, while isolating the air to prevent oxidation of the aluminum liquid.
[0006] The technical solution adopted by the present invention is: the production method of the steel-aluminum composite anode claw comprises the following steps: 1) Production of outer steel layer: The connecting pipe, crossbeam pipe and clamping pipe of the outer steel layer are cast or welded into one piece. The inner surface is clean and there must be no debris or obstruction that hinders atomic diffusion.
[0007] 2) Molding: The connecting pipe is sealed with refractory bricks placed at the bottom thereof, the crossbeam pipe is fixed with molding sand, and the upper end of the clamping pipe is sealed and placed with a thermal insulation riser; an induction coil is set outside the circumference of the clamping pipe, and the distance between the induction coil and the outer wall of the clamping pipe is consistent, so that the induction heating is uniform.
[0008] 3) Pouring: Before pouring, the clamping tube is induction heated to 200°C-300°C to minimize the temperature drop of the molten aluminum during pouring. After pouring, the clamping tube is induction heated to 650°C-720°C, preferably 650°C-680°C, which is approximately the melting point of the molten aluminum. Insulating agent is sprinkled on the surface of the molten aluminum in the insulated riser to prevent heat dissipation from the molten aluminum. Quickly seal the insulated riser with a sealing cap. Pressurized gas is introduced into the riser through the air inlet on the sealing cap. The pressure of the pressurized gas should be 0.2-0.4 MPa. After the induction coil is heated at high temperature for 2-5 minutes, the power is turned off and the aluminum is cooled. After the molten aluminum solidifies, the pressurized gas is removed.
[0009] 4) Cleaning: Remove the pouring spout and clean.
[0010] Preferably, in order to ensure the stability of the insulation riser, the insulation riser is placed in a steel bucket and supported by the steel bucket, and refractory mud sealing paste is filled between the two.
[0011] Preferably, in order to facilitate the placement and removal of the induction coil, the induction coil is in the shape of a semicircular groove, the groove opening of which bends inwards when placed and opens outwards when unpacked and removed.
[0012] Preferably, to prevent deformation of the clamping tube due to insufficient thermal strength to withstand the gas pressure during high-temperature heating by the induction coil, the clamping tube is supported by vacuum sand. Vacuum sand refers to binderless sand that is dense when evacuated. At high temperatures, the sand maintains sufficient strength to prevent deformation of the clamping tube, and exhibits good fluidity after the vacuum is removed.
[0013] Preferably, to facilitate production planning and organization, the outer steel layer is heated to 100-200° C., and boric acid is sprinkled on the inner surface to protect the inner surface from oxidation by utilizing the liquefied diffusion of the boric acid.
[0014] The present invention utilizes high temperature and high pressure to promote the diffusion of aluminum atoms, creating a metallurgical bond at the aluminum-steel interface. The aluminum core of the anode claw is fully supported and protected by the outer steel layer. The gas pressure also facilitates shrinkage feeding of the aluminum, improving the casting quality of the aluminum core. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a schematic diagram of the modeling of Example 1; Figure 2 Schematic diagram of the induction coil structure; Figure 3 This is a schematic diagram of the modeling of Example 2; In the figure: 1-outer steel layer, 2-molten aluminum, 3-induction coil, 4-insulation riser, 5-steel bucket, 6-sealing cover, 7-air inlet, 8-insulation agent, 9-sealing paste, 10-support plate, 11-refractory brick, 12-molding sand, 13-plastic film; 101-connecting tube, 102-crossbeam tube, 103-clamping tube. DETAILED DESCRIPTION
[0016] The following embodiments use a three-prong anode claw as an example, but are not limited to this type of claw. The anode claw produced by this invention structurally comprises an outer steel layer and an inner aluminum core. The aluminum core is located within the outer steel layer and emerges at the conductive end of the anode claw. The outer steel layer ensures the mechanical properties of the anode claw, while the aluminum core ensures its excellent electrical conductivity. The outer steel layer and the aluminum core are seamlessly metallurgically bonded together through atomic diffusion.
[0017] The high temperature mentioned below refers to the temperature of the induction coil after casting, which is 650℃-720℃. Example 1
[0018] This embodiment is applicable to the outer steel layer of cast steel. The production method of the steel-aluminum composite anode claw includes the following steps: 1. Make the outer steel layer The outer steel layer 1 can be made by casting or welding, and its inner surface can be cleaned by shot blasting or grinding, and no debris that affects atomic diffusion can be attached. Figure 1 As shown, it includes a connecting tube 101, a crossbeam tube 102 and a clamping tube 103. The connecting tube 101 and the clamping tube 103 are usually round, and the crossbeam tube 102 is usually square. The connecting tube 101 is used to connect the guide rod, and the clamping tube 103 is used to connect the carbon block.
[0019] If the outer steel layer 1 is cast as an integral structure, the composition of the cast steel can be designed according to the size of the anode claw and the application conditions. The composition can be adjusted in the smelting furnace, but this is not conducive to cleaning and inspection of the inner surface. Especially for large-sized outer steel layers, the casting of the floating core is an issue that must be considered. If the outer steel layer 1 is welded using purchased hot-rolled pipes, the hot-rolled pipes are usually low-carbon steel or low-alloy steel, and their high-temperature strength is relatively low. If the outer steel layer 1 is cast as two symmetrical semicircular tube castings and welded, there is no casting floating core, and the inner surface is easy to clean by shot blasting and grinding, which also facilitates the inspection of the inner surface quality. Medium-carbon alloy steel can be used to improve its high-temperature strength, but the welding performance of the steel castings needs to be considered.
[0020] 2. Modeling The shape is as attached Figure 1 As shown, the connecting pipe 101 of the outer steel layer 1 is placed downward in the sand box or on the ground. The connecting pipe 101 cooperates with the refractory bricks 11 placed at its bottom and is sealed with refractory mud sealing paste 9. The crossbeam tube 102 is horizontal, and the clamping tube 103 is vertical. The crossbeam tube 102 is fixed with molding sand 12 to prevent the outer steel layer from tipping over during subsequent operations and pouring.
[0021] The upper end of the clamping tube 103 is provided with an insulating riser 4, which is placed in and supported by a steel bucket 5, with a refractory clay sealant 9 filled between the two. To facilitate supporting the steel bucket 5, a support plate 10 is provided on the upper portion of the clamping tube 103. Thus, the support plate 10 supports the steel bucket 5, which in turn supports the insulating riser 4. The insulating riser 4 and the upper end of the clamping tube 103 are sealed with a refractory clay sealant 9.
[0022] The induction coil 3 is placed outside the circumference of the clamping tube 103. In order to facilitate the removal of the induction coil and avoid damage to the induction coil when unpacking, the induction coil 3 is made as shown in the attached Figure 2 The form shown is a semicircular groove. The induction coil 3 is usually made of copper tube, which has good plastic deformation ability. After the induction coil 3 is placed outside the clamping tube 103, the groove opening of the induction coil 3 is bent inward, so that the distance between the copper tube induction coil and the outer wall of the clamping tube is consistent, but a certain gap is maintained between the induction coils to prevent contact, which facilitates uniform heating of the clamping tube.
[0023] 3. Pouring Before pouring, the induction coil 3 is energized, heating the clamping tube 103 to 200°C-300°C. At this temperature, the inner surface will not oxidize in a short period of time, remaining clean. Heat transfer from the outer steel layer keeps the outer steel layer at a constant temperature, preventing a significant temperature drop during aluminum pouring. This also dries the sealing paste, preventing the adverse effects of water vapor generated by the sealing paste on the aluminum liquid.
[0024] After the pouring ladle is aligned with the pouring cup and before pouring begins, the power of the induction coil is increased while molten aluminum is poured simultaneously, rapidly filling the outer steel layer. Pouring is stopped after the molten aluminum has filled the mold and entered the insulated riser. Insulation agent 8 is sprinkled onto the surface of the molten aluminum in the insulated riser. A sealing cap 6 is placed over the top of the steel hopper 5. This cap is equipped with an air inlet 7, which is connected to a pressurized gas pipeline. Once the sealing cap 6 is sealed, pressurized gas is introduced through the air inlet 7. The induction coil heats the clamping tube to near the melting point of the molten aluminum. Under the high pressure and temperature, the molten aluminum atoms diffuse toward the inner surface of the outer steel layer, forming a metallurgical bond upon solidification.
[0025] The sealing cap 6 and the steel hopper 5 should be connected by a snap-on design. Before sealing, apply sealing paste for quick and easy sealing. The heat-insulating agent 8 helps maintain the temperature of the molten aluminum while also allowing it to penetrate the gas, allowing the high-pressure gas to act on the surface of the molten aluminum. The high-pressure gas should be an inexpensive, non-combustible or inert gas, such as argon, nitrogen, or carbon dioxide. Coal gas or liquefied petroleum gas can also be used. The induction heating temperature for the clamping tube is preferably 650°C-680°C (the melting point of aluminum is approximately 660°C). Higher temperatures reduce the strength of the cast steel, making gas pressurization less effective. Lower temperatures reduce the diffusion capacity of the molten aluminum atoms, hindering metallurgical bonding. The gas pressure is directly related to the high-temperature strength of the cast steel; within its tolerable range, the higher the pressure, the better. After 2-5 minutes of high-temperature heating, the induction coil power gradually decreases, allowing the molten aluminum to fully contract under the action of the gas pressure. The outer steel layer cools along with the molten aluminum. Although their shrinkage coefficients differ, the difference is minimal (cast aluminum's shrinkage is generally around 1%, while cast steel's linear shrinkage is around 1%). Furthermore, cast aluminum has good plasticity and avoids shrinkage cracks. After the molten aluminum solidifies, the pressurized gas is removed. After the entire unit has cooled, the induction coil slot is opened outward, the induction coil is removed, and the box is unpacked.
[0026] 4. Cleaning After unpacking, remove the pouring head, shot blast to clean the oxide scale on the outer surface, and knock to check the metallurgical bonding between the inside and outside.
[0027] In this embodiment, 42CrMo cast steel is used to make the outer steel layer. 42CrMo cast steel can be welded with E10015 or MG600 welding materials, preheated before welding and heated after welding to reduce or eliminate welding stress. The cast steel has high high-temperature strength and can work below 600°C for a long time. After the aluminum liquid is poured, the induction heating is maintained at 660°C-6700°C, the gas pressure is 0.2MPa, and the high-temperature induction heating time is 3min. After the riser is removed, the cross section is not loose and has no pores. Destructive sampling and testing of the beam tube and the clamping tube showed no cracks or gaps. Low-magnification inspection of the inner and outer joint surfaces of the clamping tube showed only black lines and no gaps. Example 2
[0028] This embodiment is applicable to the outer steel layer of a hot-rolled tube. Since the hot-rolled tube is made of low-carbon steel or low-alloy steel and has low high-temperature strength, measures need to be taken to improve its high-temperature deformation resistance to meet the gas pressure requirements.
[0029] 1. Make the outer steel layer The outer steel layer 1 is welded together by the hot-rolled connecting tube 101, the hot-rolled beam tube 102 and the hot-rolled clamping tube 103. Before welding, the inner surface is cleaned of debris to avoid affecting the diffusion of aluminum liquid atoms.
[0030] 2. Modeling The shape is as attached Figure 3 As shown, the difference from Example 1 is that the sand embedding method of the outer steel layer is different.
[0031] The outer steel layer is placed in a vacuum flask. Dry sand is used without a binder, and angular sand particles are preferred to increase friction between the sand particles. After the induction coil is placed, the sand is buried up to the insulation riser. The flask is vibrated to compact the sand, and then covered with plastic film 13. The plastic film 13 should be positioned away from the induction coil or the clamping tube. The clamping tube and the steel bucket should not only be sealed but also insulated to prevent thermal damage to the plastic film 13, which could affect the vacuum level of the flask. After covering with plastic film, vacuum is applied to check for leaks. After plugging the leaks, a layer of sand is sprinkled on the surface of the plastic film to prevent splashing of the hot aluminum liquid.
[0032] The molding sand of this embodiment adopts vacuum molding sand, which refers to sand grains without binder. It is dense under vacuum state, and the strength of the molding sand can still meet the need to prevent the deformation of the clamping tube under high temperature conditions. The sand grains have good fluidity after the vacuum is removed. The disadvantage of vacuum molding sand is that the operation is complicated, such as covering with agricultural film, vacuuming, etc. Its advantage is that the sand can be recycled, there is no adhesive, and no sand treatment is required. The biggest advantage is that even if the local high temperature of the molding sand is not affected, it will not affect the strength of the molding sand, and it can meet the requirements of resisting the high-temperature deformation of the clamping tube under pressure for a long time. However, molding sand that uses binders, such as resin sand, water glass sand, etc., will cause the binder to fail due to high temperature, and the molding sand will lose its strength and cannot resist the high-temperature deformation of the clamping tube.
[0033] 3. Pouring Before pouring, the induction coil 3 is energized and the clamping tube is preheated to 200°C-300°C. The sand box is evacuated, and the molding sand is dense under vacuum conditions, and the strength is greatly increased, which can prevent the high-temperature clamping tube from deforming under the action of air pressure. After the pouring ladle is aligned with the pouring cup, the power of the induction coil is increased, and the aluminum liquid is poured at the same time to quickly fill the mold in the outer steel layer. The subsequent operations are the same as in Example 1, with only slight differences in the unpacking operations. After the temperature of the clamping tube is reduced and the strength is increased, the vacuum in the sand box can be removed, but this is not the focus of the operation of this application. It should be noted that since the high-temperature clamping tube in this embodiment is supported by the vacuum molding sand and does not deform, the induction heating temperature can be higher than 680°C in Example 1. However, the higher the temperature, the greater the temperature difference in the aluminum liquid, which is less conducive to cooling and shrinkage compensation. Moreover, it is not recommended to exceed the phase change temperature, and it is advisable to control it below 720°C. Furthermore, because the high-temperature clamping tube is supported by vacuum sand, the gas pressure can be increased to 0.4 MPa or above. This increased pressure not only facilitates metallurgical bonding through atomic diffusion but also facilitates shrinkage feeding of the molten aluminum. However, higher pressure increases both cavity sealing and power consumption, and the thickness of the metallurgical bonding layer does not increase proportionally.
[0034] To meet the needs of large-scale industrial production, the outer steel layer should be cleaned before molding and pouring immediately to prevent re-oxidation of the inner surface, which could hinder atomic diffusion. However, if the interval between cleaning and molding is long, the outer steel layer should be heated to 100-200°C and the inner surface sprinkled with boric acid. The melted boric acid will coat the inner surface, isolating it from air and preventing oxidation. Furthermore, boric acid increases surface activity and promotes atomic diffusion. Before pouring, the boric acid is heated to a liquid state. After the aluminum is poured and remains liquid for a long time, the boric acid floats into the riser, preventing the casting quality of the aluminum core. This measure increases production flexibility and facilitates production planning and organization.
[0035] This invention utilizes high temperature and high pressure to promote atomic diffusion in the molten aluminum, creating a metallurgical bond at the aluminum-steel interface. The aluminum core of the anode claw is fully supported and protected by the outer steel layer, fulfilling its sole function of conducting electricity. Furthermore, after the molten aluminum is poured, it is completely isolated from the air, preventing oxidation contamination of the molten aluminum. The gas pressure also aids in shrinkage feeding of the molten aluminum, improving casting quality of the aluminum core, reducing riser size, and increasing metal utilization.
Claims
1. A method for producing a steel-aluminum composite anode claw, comprising the following steps: 1) Make the outer steel layer: The connecting pipe, beam pipe and clamping pipe of the outer steel layer are cast or welded into one piece, and the inner surface is cleaned; 2) Modeling: The connecting pipe is sealed with the refractory bricks placed at the bottom thereof, the crossbeam pipe is fixed with molding sand, and the upper end of the clamping pipe is sealed and placed with a heat-insulating riser; an induction coil is arranged on the outside of the clamping pipe, and the distance between the induction coil and the outer wall of the clamping pipe is consistent; 3) Pouring: Before pouring, the clamping tube is induction heated to 200℃-300℃; after pouring, the clamping tube is induction heated to 650℃-720℃, and a heat preservation agent is sprinkled on the surface of the aluminum liquid in the insulation riser; the insulation riser is covered with a sealing cover, and pressurized gas is sent into the insulation riser through the air inlet hole on the sealing cover; after 2-5 minutes, the induction coil is powered off and cooled; after the aluminum liquid solidifies, the pressurized gas is removed; 4) Cleaning: Remove the pouring riser.
2. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: The heat-insulating riser is placed in and supported by the steel bucket, and refractory mud sealing paste is filled between the two.
3. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: The induction coil is in the shape of a semicircular groove, the opening of which bends inwards when placed and opens outwards when unpacked.
4. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: In the step 3), the induction heating temperature after pouring is preferably 650°C-680°C.
5. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: In the step 3), the pressure of the pressurized gas is 0.2-0.4 MPa.
6. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: In the step 2), the clamping tube is supported by vacuum molding sand.
7. The method for producing a steel-aluminum composite anode claw according to claim 1, characterized in that: In the step 1), the outer steel layer is heated to 100-200° C., and boric acid is sprinkled on the inner surface.