Method for preparing polyurethane foam by using liquid carbon dioxide as foaming agent
By using liquid carbon dioxide as a blowing agent in the production of polyurethane foam, combined with high pressure and metal catalyst technology, the problem of ozone layer destruction by chlorofluorocarbons and the high density of water blowing agents is solved, and the production of low-density, high-flexibility foam is achieved. Has cost and environmental advantages.
Patent Information
- Application Number
- CN202410905552.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-15
AI Technical Summary
Chlorofluorocarbons used in existing polyurethane foam production cause damage to the ozone layer. When water is used as the blowing agent, the foam density is high and the cost is high, making it difficult to produce low-hardness foam.
Liquid carbon dioxide is used as the foaming agent, dissolved in polyether polyol under high pressure, and fully mixed with other additives to form a homogeneous system to promote the foaming reaction. Metal catalysts are used to increase the strength of the foam network skeleton, reduce foam density and improve Flexible.
Produce polyurethane foam with low density, good flexibility and high tear resistance, which can replace methylene chloride and Freon and has the advantages of low cost, non-toxic and harmless.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of household goods manufacturing, and in particular to a method for preparing polyurethane foam by using liquid carbon dioxide as a foaming agent. Background Art
[0002] Polyurethane foam is one of the main varieties of polyurethane synthetic materials. It has the characteristics of light weight and high specific strength due to its special pore structure. It also has excellent mechanical properties, high temperature resistance, chemical resistance, etc. It is widely used in aerospace, energy, transportation, communication, home, packaging and other fields. Polyurethane foam, i.e. sponge, which is widely used in our lives, mainly uses physical foaming agents that do not participate in the reaction in production, generally Freon (CFC-11) and dichloromethane MC (CH2Cl2). However, studies have shown that chlorofluorocarbons have a high ozone depletion potential (ODP) and stay in the atmosphere for 40 to 150 years. When exposed to strong high-energy ultraviolet rays from the sun, they will decompose into chlorine, which has a relatively large damage to the ozone layer.
[0003] Therefore, finding a blowing agent with zero or low ODP value to replace chlorofluorocarbons and dichloromethane is the most important issue in the polyurethane foam plastics industry. Currently, water is also used as a blowing agent in the industry, but the minimum density of the foam can only reach 22kg / m 3 , and it is impossible to produce low hardness foam, and the production cost is also high. Summary of the invention
[0004] In view of this, the present invention provides a method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent, which can solve the above problems.
[0005] A method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent comprises the following steps:
[0006] STEP 101: Provide raw materials for preparing the polyurethane foam, which are composed of polyether polyol, isocyanate, silicone surfactant, amine catalyst, metal catalyst, water, and liquid carbon dioxide, wherein based on 100 parts of polyether polyol, the isocyanate is 30 to 70 parts, the silicone surfactant is 0.1 to 3.0 parts, the metal catalyst is 0.05 to 1.0 parts, the amine catalyst is 0.1-3.0 parts, the liquid carbon dioxide is 0.5 to 8.0 parts, and the water is 1 to 5 parts;
[0007] STEP 102: Premix part of the polyether polyol, pressurize it to 20-35 bar by a high-pressure metering pump, and then inject liquid carbon dioxide into the polyether polyol stream, and transport it to a static mixer, where the carbon dioxide is uniformly dissolved to obtain a mixture 1. The carbon dioxide must remain in a liquid state during the entire metering process and the material mixing process;
[0008] STEP 103: Mixture 1 is decompressed to 10-15 bar, and mixed with the remaining polyether polyol, silicone surfactant, and amine catalyst to obtain mixture 2;
[0009] STEP 104: Provide nitrogen, and mix the nitrogen and isocyanate through a static mixer, and then pressurize them to 60-80 bar through a high-pressure metering pump to obtain a mixture 3;
[0010] STEP 105: Mixture 2, mixture 3, metal catalyst and water are fed into a mixing device, decompressed to 6-10 bar, stirred at a high speed of 2000-5000 rpm, and sprayed out from the discharge port of the mixing device to solidify and generate polyurethane foam.
[0011] Furthermore, the organosilicon surfactant is hydrophobic.
[0012] Furthermore, the organosilicon surfactant is a polysiloxane compound with a chemical formula of R3SiO[Si(CH3)2O]nSiR3.
[0013] Furthermore, the amine catalyst may be a tertiary amine catalyst, and the tertiary amine catalyst may be one or more of pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, triethylenediamine, triethylamine, and bis(dimethylamino)ethyl ether.
[0014] Furthermore, the metal catalyst is one or more of potassium isooctanoate, quaternary ammonium formate, potassium acetate, organic tin, organic zinc, tin neodecanoate, bismuth neodecanoate and potassium oleate.
[0015] Furthermore, in STEP 101, when dissolving carbon dioxide into the polyether polyol, the high-pressure metering pump is pressurized to 28.2 bar, 30 bar, or 30.8 bar.
[0016] Furthermore, in STEP 102, when the remaining part of the polyether polyol, the silicone surfactant, and the amine catalyst are mixed with the polyether polyol dissolved with carbon dioxide, the high-pressure metering pump is pressurized to 10.5 bar, 12 bar, or 10 bar.
[0017] Furthermore, in STEP 105, the pressure in the mixing device is 8.5 bar, 6.9 bar, or 6.2 bar.
[0018] Compared with the prior art, the method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent provided by the present invention firstly dissolves the liquid carbon dioxide fully into a part of the polyether polyol under high pressure, and then reduces the pressure so that the polyether polyol dissolved with carbon dioxide can be fully mixed with the remaining part of the polyether polyol, the organic silicon surfactant, the amine catalyst and other additives, so that the amine catalyst is uniformly dispersed in the mixture under the action of the organic silicon surfactant to form a homogeneous system, and the alkaline tertiary amine compound has a high affinity to the C + The ions undergo nucleophilic attack to form an active transition compound, which is easy to react with the polyether polyol. The alkaline catalyst is separated from the transition compound and continues to form an active transition compound with another isocyanate molecule to promote the foaming reaction. Finally, the nitrogen is mixed with the isocyanate by high pressure, and the mixture is finally sent to a mixing device, in which a metal catalyst is added, and then the mixture is ejected from the discharge port of the mixing device by decompression again, and solidified to form polyurethane foam. Since there is a larger electron-donating group behind the hydroxyl group of the polyether polyol, the electron cloud density of the alcohol hydroxyl group is higher than that of water, and its coordination ability with the empty orbit of the metal atom is stronger than that of water. Therefore, the metal catalyst has a strong catalytic effect on the reaction of isocyanate and polyol, which ensures the strength of the foam network skeleton, so that small bubbles are trapped inside, thereby ensuring that high-quality foam can be produced. At the same time, due to the presence of carbon dioxide, there are more pores in the mixture and the pores are relatively stable. At the same time, the prepared foam material has a lower density, better flexibility, and higher tear strength. At the same time, this liquid carbon dioxide can replace the use of dichloromethane and Freon, and is also part of the atmospheric cycle. It has the advantages of low cost, non-toxicity, harmlessness, and non-flammability. DETAILED DESCRIPTION
[0019] The specific embodiments of the present invention are further described in detail below. It should be understood that the description of the embodiments of the present invention herein is not intended to limit the protection scope of the present invention.
[0020] The present invention provides a method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent, which comprises the following steps:
[0021] STEP 101: Provide raw materials for preparing the polyurethane foam, which are composed of polyether polyol, isocyanate, silicone surfactant, amine catalyst, metal catalyst, water, and liquid carbon dioxide, wherein based on 100 parts of polyether polyol, the isocyanate is 30 to 70 parts, the silicone surfactant is 0.1 to 3.0 parts, the metal catalyst is 0.05 to 1.0 parts, the amine catalyst is 0.1-3.0 parts, the liquid carbon dioxide is 0.5 to 8.0 parts, and the water is 1 to 5 parts;
[0022] STEP 102: Premix part of the polyether polyol, pressurize it to 20-35 bar by a high-pressure metering pump, and then inject liquid carbon dioxide into the polyether polyol stream, and transport it to a static mixer, where the carbon dioxide is uniformly dissolved to obtain a mixture 1. The carbon dioxide must remain in a liquid state during the entire metering process and the material mixing process;
[0023] STEP 103: Mixture 1 is decompressed to 10-15 bar, and mixed with the remaining polyether polyol, silicone surfactant, amine catalyst and other additives to obtain mixture 2;
[0024] STEP 104: Provide nitrogen, and mix the nitrogen and isocyanate through a static mixer, and then pressurize them to 60-80 bar through a high-pressure metering pump to obtain a mixture 3;
[0025] STEP 105: Mixture 2, mixture 3, metal catalyst and water are fed into a mixing device, decompressed to 6-10 bar, stirred at a high speed of 2000-5000 rpm, and sprayed out from the discharge port of the mixing device to solidify and generate polyurethane foam.
[0026] In STEP101, the polyether polyol, isocyanate, and liquid carbon dioxide are prior art and are not described in detail here. The organosilicon surfactant is a polysiloxane compound with a chemical formula of R3SiO[Si(CH3)2O]nSiR3. Among them, R is generally an organic group such as methyl or phenyl. The structure of the organosilicon surfactant is similar to a chain, with silicon atoms and oxygen atoms on the chain arranged alternately, and the chains are connected by organic groups. The organosilicon surfactant is hydrophilic and hydrophobic, and the hydrophobicity and hydrophilicity are determined by its molecular structure. In the invention, the organosilicon surfactant must be hydrophobic. Because the hydrophobic organosilicon surfactant can make CO2 and water form an emulsion, and by adjusting the EO number, the "hydrophilic CO2 balance value" of the organosilicon surfactant is changed, so that the emulsion can be transformed from CO2-water to water-CO2, thereby playing the role of emulsifying materials, stabilizing foam and regulating pores. At the same time, the hydrophobic organosilicon surfactant also increases the mutual solubility of the components, which is beneficial to the production of bubbles, controls the size and uniformity of the pores, and promotes the balance of the gel tension of the foam pores, making the pore walls elastic to retain gas and prevent foam collapse.
[0027] In STEP102, the high-pressure metering pump is pressurized to 20-35 bar to ensure that the carbon dioxide is in a liquid state, so that the liquid carbon dioxide can be dissolved in the polyether polyol. In the conventional foaming process using a foaming agent, the foaming gas is a separate phase in the mixture, and the liquid is made into small bubbles by mechanical stirring. When the foaming reaction releases heat, the gas expands due to heat. In this high-pressure foaming process, the carbon dioxide is evenly distributed in the mixture before extrusion. When the mixture is extruded, it changes from high pressure to low pressure and becomes a large amount of gas phase in a short time. The gaseous carbon dioxide becomes a large number of bubble nuclei. The expansion speed of the foam is much greater than that of conventional foaming, and carbon dioxide also becomes part of the product. The pressure of the high-pressure metering pump is set between 20 and 35 bar to ensure the solubility of carbon dioxide, and therefore the solubility of carbon dioxide is adjusted by the pressure of the fluid. Therefore, the carbon dioxide must remain in a liquid state during the entire metering and material mixing process.
[0028] In STEP103, the amine catalyst may be a tertiary amine catalyst, and the tertiary amine catalyst may be one or more of pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, triethylenediamine, triethylamine, and bis(dimethylamino)ethyl ether. In STEP103, the reason for using only amine catalysts is that in the process of preparing polyurethane foam using carbon dioxide as a foaming agent, it is necessary to adjust the speed of the foaming reaction and the gel reaction so that they are in a good equilibrium state, that is, after the foaming reaction is completed, the strength of the foam network skeleton must be sufficient to trap small bubbles inside to ensure that high-quality foam can be produced. If the strength of the foam network skeleton is not strong enough and collapses, there will be no small bubbles inside, which will make the foam produced have poor stiffness, poor softness, and easy deformation. After the polyether polyol, silicone surfactant, and amine catalyst are pre-mixed under stirring in a homogenizer to form a homogeneous system, the alkaline tertiary amine compound has an effect on C + The ions undergo nucleophilic attacks to form active transition compounds, which are easy to react with polyether polyols. The alkaline catalyst detaches from the transition compound and continues to form active transition compounds with another isocyanate molecule. The nitrogen atom in the molecular structure of the amine catalyst complexes with isocyanate to reduce the reaction activation energy of isocyanate, activate the polyether polyol to form hydrogen cations and corresponding anion groups, and under the action of the organosilicon surfactant, the components are well mixed and emulsified, the mutual solubility of the components is increased, and the mixture forms a homogeneous system, which can not only promote the foaming reaction, that is, promote the reaction of isocyanate and water, but also form bubbles of uniform size.
[0029] In STEP 104, the role of the nitrogen is the same as that of the carbon dioxide. The purpose of mixing the nitrogen with the isocyanate is to make all the raw materials contain the foaming agent, so that the subsequent liquid mixing can be more uniform. The raw materials are kept under high pressure throughout the process from the raw materials entering to the materials being discharged after mixing. If the pressure is low, the carbon dioxide will dissolve prematurely and the foam will rise prematurely.
[0030] In STEP105, after the mixture is loaded into the mixing device, it is necessary to reduce the pressure to 6 to 10 bar. Because after changing from high pressure to low pressure, carbon dioxide will quickly gasify and become a large amount of gas, and the gaseous carbon dioxide will become a large number of bubble nuclei, thereby forming a porous structure in the polyurethane. To produce foams of the same density and hardness, the use of water can be reduced by adopting high-pressure mixing technology, and the consumption of isocyanate can be correspondingly reduced, which is conducive to reducing costs. In STEP105, only and only metal catalysts are used to promote gel reaction. The metal catalyst is one or more of potassium isooctanoate, quaternary ammonium formate, potassium acetate, organic tin, organic zinc, tin neodecanoate, bismuth neodecanoate and potassium oleate. In STEP103, isocyanate and water are fully reacted and fully foamed by an amine catalyst to form foam. Therefore, gel reaction is performed again in STEP105 to ensure the strength of the foam network skeleton. The metal catalyst can promote gel reaction, that is, promote the reaction of isocyanate and polyol. Since there is a large electron-donating group behind the hydroxyl group of the polyether polyol, the electron cloud density of the alcohol hydroxyl group is higher than that of water, and its coordination ability with the empty orbit of the metal atom is stronger than that of water. Therefore, the metal catalyst has a strong catalytic effect on the reaction between isocyanate and polyol, achieving the purpose of ensuring the strength of the foam network skeleton to the extent that small bubbles are trapped inside, thereby ensuring that high-quality foam can be produced. The purpose of ensuring the strength of the foam network skeleton to the extent that small bubbles are trapped inside, thereby ensuring that high-quality foam can be produced. In addition, the metal catalyst is unstable. It is very easy to hydrolyze and oxidize in the polyether mixture containing water and amine catalyst and lose its function, so it should be added to the mixture last.
[0031] At the same time, due to the presence of carbon dioxide in the entire foaming process, the mixture has more pores and the bubbles are relatively stable. At the same time, the prepared foam material has lower density, better flexibility and higher tear resistance.
[0032] Embodiment 1:
[0033] (1) First, 100 parts of polyether polyol 560S are pressurized to 28.2 bar by a high-pressure metering pump, and then 3 parts of liquid carbon dioxide are injected into the polyol stream and transported to a static mixer; in the static mixer, the carbon dioxide is uniformly dissolved to obtain a mixture 1. CO2 must remain in a liquid state during the entire metering and material mixing process.
[0034] (2) Mixture 1 was decompressed to 10.5 bar, and mixed with the remaining 18 parts of polyether polyol 560S, 1.3 parts of silicone oil, 0.14 parts of amine catalyst and other additives to obtain mixture 2;
[0035] (3) injecting 10 parts of nitrogen into 57.5 parts of toluene diisocyanate stream, and then feeding the stream into a static mixer for mixing to obtain a mixture 3;
[0036] (4) Mixture 2 is depressurized to 8.5 bar through a filter screen at the feed outlet of the mixer, and is fed into a mixing device together with mixture 3, 4.3 parts of water, 0.15 parts of stannous octoate, etc., and then ejected from the feed outlet of the mixing device under high-speed stirring to solidify and form polyurethane foam.
[0037] Comparative Example 1 :
[0038] Using a one-step foaming method, 100 parts of polyether polyol 560S, 1.3 parts of silicone oil, 0.14 parts of amine catalyst, 4.3 parts of water, 0.15 parts of stannous octoate, 11 parts of dichloromethane and 57.5 parts of toluene diisocyanate are respectively delivered from storage tanks into a high-speed stirring mixing head in proportion by several groups of precision metering pumps, quickly mixed evenly under high-speed stirring, and injected onto a belt conveyor for foaming.
[0039] Table 1 Physical properties of the foams formed by Example 1 and Comparative Example 1
[0040] raw material Example 1 Comparative Example 1 Polyether polyol 560S 100 100 Toluene isocyanate 57.5 57.5 Silicone oil 1.3 1.3 Amine Catalyst 0.14 0.14 Stannous Octoate 0.15 0.15 water 4.3 4.3 carbon dioxide 3 —— Dichloromethane —— 11 Test items Example 1 Comparative Example 1 <![CDATA[Density kg / m 3 > 17.1 17.3 40% indentation hardness N 82.7 91 75% Compression set% 4 6 Rebound rate % 41.8 39 Tensile strength kPa 75 81 Elongation % 267.4 253 Tear strength N / cm 3.7 2.3
[0041] Example 2 :
[0042] (1) First, 100 parts of polyether polyol 560S are pressurized to 30 bar by a high-pressure metering pump, and then 2.5 parts of liquid carbon dioxide are injected into the polyol stream and transported to a static mixer; in the static mixer, the carbon dioxide is uniformly dissolved to obtain a mixture 1. CO2 must remain in a liquid state during the entire metering and material mixing process.
[0043] (2) Mixture 1 was decompressed to 12 bar, and mixed with the remaining 18 parts of polyether polyol 560S, 1.3 parts of silicone oil, 0.24 parts of amine catalyst and other additives to obtain mixture 2;
[0044] (3) injecting 12 parts of nitrogen into 49 parts of toluene diisocyanate stream, and then feeding the stream into a static mixer for mixing to obtain a mixture 3;
[0045] (4) Mixture 2 is depressurized to 6.9 bar through a filter screen at the mixer discharge port, and is fed into a mixing device together with mixture 3, 3.7 parts of water, 0.18 parts of stannous octoate, etc., and is ejected from the discharge port of the mixing device under high-speed stirring to solidify and form polyurethane foam.
[0046] Comparative Example 2 :
[0047] Using a one-step foaming method, 100 parts of polyether polyol 560S, 1.3 parts of silicone oil, 0.24 parts of amine catalyst, 3.7 parts of water, 0.18 parts of stannous octoate, 9.2 parts of dichloromethane and 49 parts of toluene diisocyanate are respectively delivered from storage tanks into a high-speed stirring mixing head in proportion by several groups of precision metering pumps, quickly mixed evenly under high-speed stirring, and injected onto a belt conveyor for foaming.
[0048] Table 2 Physical properties of the foams formed by Example 2 and Comparative Example 2
[0049] raw material Example 2 Comparative Example 2 Polyether polyol 560S 100 100 Toluene isocyanate 49 49 Silicone oil 1.3 1.3 Amine Catalyst 0.24 0.24 Stannous Octoate 0.18 0.18 water 3.7 3.7 carbon dioxide 2.5 —— Dichloromethane —— 9.2 Test items Example 2 Comparative Example 2 <![CDATA[Density kg / m 3 > 20 18.2 40% indentation hardness N 92 100 75% Compression set% 6 6 Rebound rate % 46 40 Tensile strength kPa 82 71 Elongation % 277 243 Tear strength N / cm 3.4 2.0
[0050] Embodiment 3:
[0051] (1) First, 100 parts of polyether polyol 560S are pressurized to 30.8 bar by a high-pressure metering pump, and then 1.9 parts of liquid carbon dioxide are injected into the polyol stream and transported to a static mixer; in the static mixer, the carbon dioxide is uniformly dissolved to obtain a mixture 1. CO2 must remain in a liquid state during the entire metering and material mixing process;
[0052] (2) Mixture 1 was decompressed to 10 bar, and mixed with the remaining 18 parts of polyether polyol 560S, 1.1 parts of silicone oil, 0.18 parts of amine catalyst and other additives to obtain mixture 2;
[0053] (3) injecting 15 parts of nitrogen into 40.8 parts of toluene diisocyanate stream, and then feeding the stream into a static mixer for mixing to obtain a mixture 3;
[0054] (4) Mixture 2 is depressurized to 6.2 bar through a filter screen at the mixer discharge port, and is fed into a mixing device together with mixture 3, 3 parts of water, 0.17 parts of stannous octoate, etc., and is ejected from the discharge port of the mixing device under high-speed stirring to solidify and form polyurethane foam.
[0055] Comparative Example 3 :
[0056] Using a one-step foaming method, 100 parts of polyether polyol 560S, 1.1 parts of silicone oil, 0.18 parts of amine catalyst, 3 parts of water, 0.17 parts of stannous octoate, 7 parts of dichloromethane and 40.8 parts of toluene diisocyanate are respectively delivered in proportion from storage tanks by several groups of precision metering pumps into a high-speed stirring mixing head, quickly mixed evenly under high-speed stirring, and injected onto a belt conveyor for foaming.
[0057] Table 3 Physical properties of the foams formed by Example 3 and Comparative Example 3
[0058] raw material Example 3 Comparative Example 3 Polyether polyol 560S 100 100 Toluene isocyanate 40.8 40.8 Silicone oil 1.1 1.1 Amine Catalyst 0.18 0.18 Stannous Octoate 0.17 0.17 water 3 3 carbon dioxide 1.9 —— Dichloromethane —— 7 Test items Example 3 Comparative Example 3 <![CDATA[Density kg / m 3 > 25 24.3 40% indentation hardness N 92 126 75% Compression set% 6 5 Rebound rate % 49.6 46 Tensile strength kPa 107 114 Elongation % 276 226 Tear strength N / cm 4.2 2.0
[0059] Summary: In Comparative Examples 1, 2, and 3, dichloromethane is used as a foaming agent, and the foams prepared in Examples 1, 2, and 3 are softer and have better tear strength than the comparative examples. In the liquid carbon dioxide foaming technology, the pores in the mixture can be easily removed, and the pores are relatively stable, which is conducive to the formation of regular pores.
[0060] Compared with the prior art, the method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent provided by the present invention firstly dissolves the liquid carbon dioxide fully into a part of the polyether polyol under high pressure, and then reduces the pressure so that the polyether polyol dissolved with carbon dioxide can be fully mixed with the remaining part of the polyether polyol, the organic silicon surfactant, the amine catalyst and other additives, so that the amine catalyst is uniformly dispersed in the mixture under the action of the organic silicon surfactant to form a homogeneous system, and the alkaline tertiary amine compound has a high affinity to the C + The ions undergo nucleophilic attack to form an active transition compound, which is easy to react with the polyether polyol. The alkaline catalyst is separated from the transition compound and continues to form an active transition compound with another isocyanate molecule to promote the foaming reaction. Finally, the nitrogen is mixed with the isocyanate by high pressure, and the mixture is finally sent to a mixing device, in which a metal catalyst is added, and then the mixture is ejected from the discharge port of the mixing device by decompression again, and solidified to form polyurethane foam. Since there is a larger electron-donating group behind the hydroxyl group of the polyether polyol, the electron cloud density of the alcohol hydroxyl group is higher than that of water, and its coordination ability with the empty orbit of the metal atom is stronger than that of water. Therefore, the metal catalyst has a strong catalytic effect on the reaction of isocyanate and polyol, which ensures the strength of the foam network skeleton, so that small bubbles are trapped inside, thereby ensuring that high-quality foam can be produced. At the same time, due to the presence of carbon dioxide, there are more pores in the mixture and the pores are relatively stable. At the same time, the prepared foam material has a lower density, better flexibility, and higher tear strength. At the same time, this liquid carbon dioxide can replace the use of dichloromethane and Freon, and is also part of the atmospheric cycle. It has the advantages of low cost, non-toxicity, harmlessness, and non-flammability.
[0061] The above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modification, equivalent substitution or improvement within the spirit of the present invention is included in the scope of the claims of the present invention.
Claims
1. A method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent, comprising the following steps: STEP 101: Provide raw materials for preparing the polyurethane foam, which are composed of polyether polyol, isocyanate, silicone surfactant, amine catalyst, metal catalyst, water, and liquid carbon dioxide, wherein based on 100 parts of polyether polyol, the isocyanate is 30 to 70 parts, the silicone surfactant is 0.1 to 3.0 parts, the metal catalyst is 0.05 to 1.0 parts, the amine catalyst is 0.1-3.0 parts, the liquid carbon dioxide is 0.5 to 8.0 parts, and the water is 1 to 5 parts; STEP 102: Premix part of the polyether polyol, pressurize it to 20-35 bar by a high-pressure metering pump, and then inject liquid carbon dioxide into the polyether polyol stream, and transport it to a static mixer, where the carbon dioxide is uniformly dissolved to obtain a mixture 1. The carbon dioxide must remain in a liquid state during the entire metering process and the material mixing process; STEP 103: Mixture 1 is decompressed to 10-15 bar, and mixed with the remaining polyether polyol, silicone surfactant, and amine catalyst to obtain mixture 2; STEP 104: Provide nitrogen, and mix the nitrogen and isocyanate through a static mixer, and then pressurize them to 60-80 bar through a high-pressure metering pump to obtain a mixture 3; STEP 105: Mixture 2, mixture 3, metal catalyst and water are fed into a mixing device, decompressed to 6-10 bar, stirred at a high speed of 2000-5000 rpm, and sprayed out from the discharge port of the mixing device to solidify and generate polyurethane foam.
2. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: The silicone surfactant is hydrophobic.
3. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: The organosilicon surfactant is a polysiloxane compound with a chemical formula of R3SiO[Si(CH3)2O]nSiR3.
4. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: The amine catalyst may be a tertiary amine catalyst, and the tertiary amine catalyst may be one or more of pentamethyldiethylenetriamine, N,N-dimethylcyclohexylamine, triethylenediamine, triethylamine, and bis(dimethylamino)ethyl ether.
5. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: The metal catalyst is one or more of potassium isooctanoate, quaternary ammonium formate, potassium acetate, organic tin, organic zinc, tin neodecanoate, bismuth neodecanoate and potassium oleate.
6. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: In STEP 101, when dissolving liquid carbon dioxide into the polyether polyol, the high-pressure metering pump is pressurized to 28.2 bar, 30 bar, or 30.8 bar.
7. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: In STEP 102, when the remaining part of the polyether polyol, the silicone surfactant, and the amine catalyst are mixed with the polyether polyol dissolved with carbon dioxide, the high-pressure metering pump is pressurized to 10.5 bar, 12 bar, or 10 bar.
8. The method for preparing polyurethane foam using liquid carbon dioxide as a foaming agent as claimed in claim 1, characterized in that: In STEP 105, the pressure in the mixing device is 8.5 bar, 6.9 bar, or 6.2 bar.
Citation Information
Cited By
Preparation method of polyurethane foam
CN121086322A
Polymer polyol foaming method adopting liquid carbon dioxide pressurization
CN121135998A
A method for foaming a polymer polyol using pressurized liquid carbon dioxide
CN121135998B