Dimming assembly, preparation method thereof and vehicle
By arranging a sealant layer in the dimming component, the problem of poor water vapor blocking ability of traditional dimming components when the distance between the edge of the dimming layer and the edge of the transparent substrate is small is solved, achieving better water vapor protection effect.
Patent Information
- Application Number
- CN202411081401.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-15
AI Technical Summary
When the distance between the edge of the dimming layer and the edge of the transparent substrate is small, traditional dimming components have poor water vapor blocking capabilities and cannot effectively prevent water vapor erosion.
Introducing a sealant layer into the dimming component, the sealant layer is arranged in at least part of the retracted area, contacts the transparent substrate and the adhesive layer, the side edges do not exceed the edge of the substrate, and the retracted area is filled with the sealant layer, and the sealant layer is The width is 1mm~20mm, including polyurethane, butyl and POE sealant layers.
The water vapor erosion resistance of the dimming component is significantly improved, and it can effectively prevent water vapor erosion when the distance between the edge of the dimming layer and the edge of the transparent substrate is small.
Smart Images

Figure CN118778296A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of dimming, and in particular to a dimming component and a preparation method thereof, and a vehicle. Background Art
[0002] The traditional dimming component includes a first transparent substrate, a first bonding layer, a dimming layer, a second bonding layer and a second transparent substrate stacked in sequence. However, the traditional dimming component has a poor water vapor blocking ability when the distance between the edge of the dimming layer and the edge of the transparent substrate is small. Summary of the invention
[0003] Based on this, some embodiments of the present application provide a dimming component with improved resistance to water vapor corrosion.
[0004] In addition, other embodiments of the present application also provide a method for preparing a dimming component and a vehicle.
[0005] A dimming component, comprising:
[0006] a first transparent substrate;
[0007] A first adhesive layer is disposed on the surface of the first transparent substrate;
[0008] A dimming layer is disposed on a surface of the first bonding layer on a side away from the first transparent substrate;
[0009] A second bonding layer is disposed on a surface of the dimming layer away from the first transparent substrate;
[0010] A second transparent substrate is disposed on a surface of the second adhesive layer that is away from the first transparent substrate;
[0011] Among them, the first bonding layer, the dimming layer and the second bonding layer are all retracted relative to the first transparent substrate and the second transparent substrate, and the dimming component also includes a sealant layer, which is arranged in at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate, and the side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate, and the width of the sealant layer is 1mm~20mm.
[0012] In some embodiments, the first bonding layer, the dimming layer and the second bonding layer are flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is less than or equal to 5 mm, and the side edge of the sealant layer contacts the first bonding layer and the second bonding layer.
[0013] In some embodiments, the width of the sealant layer is greater than or equal to 3 mm.
[0014] In some embodiments, the width of the sealant layer is 3 mm to 10 mm.
[0015] In some embodiments, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is greater than 5 mm. A third bonding layer is also provided between the first bonding layer and the second bonding layer, and the third bonding layer contacts the side edge of the dimming layer. The sealant layer contacts the first bonding layer, the second bonding layer and the third bonding layer.
[0016] In some embodiments, the third bonding layer is flush with the first bonding layer and the second bonding layer; or,
[0017] The third adhesive layer is retracted relative to the first adhesive layer and the second adhesive layer, and the width of the sealant layer increases gradually from the first adhesive layer to the third adhesive layer and from the second adhesive layer to the third adhesive layer.
[0018] In some embodiments, the maximum width of the sealant layer is 1 mm to 5 mm.
[0019] In some of the embodiments, the sealant layer includes one or more of a polyurethane sealant layer, a butyl sealant layer and a POE sealant layer.
[0020] In some of the embodiments, a surface activation layer is further provided on the surface of the sealant layer facing the first transparent substrate and the second transparent substrate, and on the surface of the sealant layer facing the first bonding layer, the second bonding layer and the dimming layer.
[0021] A method for preparing a dimming component comprises the following steps:
[0022] Obtaining a laminate, wherein the laminate comprises a first transparent substrate, a first bonding layer, a dimming layer, a second bonding layer, and a second transparent substrate stacked in sequence;
[0023] Retract the dimming layer, the first bonding layer and the second bonding layer in the stack relative to the first transparent substrate and the second transparent substrate;
[0024] A sealant layer is arranged between the first transparent substrate and the second transparent substrate of the stack, so that the sealant layer fills at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate, the side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate, and the width of the sealant layer is greater than or equal to 1 mm, to obtain a dimming component.
[0025] In some embodiments, the width of the sealant layer is 1 mm to 20 mm;
[0026] Optionally, the width of the sealant layer is 1 mm to 10 mm.
[0027] In some embodiments, in the step of causing the dimming layer, the first bonding layer, and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the first bonding layer, the dimming layer, and the second bonding layer are made flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is less than or equal to 5 mm;
[0028] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate of the stacked component so that the sealant layer fills at least a portion of the retracted area comprises:
[0029] Disposing a support member with holes between the first transparent substrate and the second transparent substrate, so that the support member with holes is in contact with the side edges of the first adhesive layer and the second adhesive layer;
[0030] Pressing the stacked member provided with the perforated support member;
[0031] After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
[0032] In some embodiments, the width of the sealant layer is greater than or equal to 3 mm;
[0033] Optionally, the width of the sealant layer is 3 mm to 10 mm.
[0034] In some embodiments, in the step of causing the dimming layer, the first bonding layer and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm;
[0035] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises:
[0036] Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is flush with the side edges of the first adhesive layer and the second adhesive layer;
[0037] Disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer to obtain a laminate;
[0038] Laminating the laminated member provided with the third adhesive layer and the perforated support member;
[0039] After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
[0040] In some embodiments, the preparation method comprises:
[0041] Obtaining the laminate, making the first adhesive layer and the second adhesive layer in the laminate flush with the first transparent substrate and the second transparent substrate, and the dimming layer retracted relative to the first adhesive layer and the second adhesive layer;
[0042] Disposing a third bonding layer between the first bonding layer and the second bonding layer, so that the third bonding layer contacts the side edge of the dimming layer and is flush with the first bonding layer and the second bonding layer;
[0043] Laminating the laminated member provided with the third adhesive layer;
[0044] After the lamination is completed, a portion of the first adhesive layer, a portion of the second adhesive layer and a portion of the third adhesive layer are removed, so that the first adhesive layer, the second adhesive layer and the third adhesive layer are all retracted relative to the first transparent substrate and the second transparent substrate;
[0045] The dimming component is prepared by filling the sealant layer in the area where the first bonding layer, the second bonding layer and the third bonding layer are removed.
[0046] In some embodiments, in the step of causing the dimming layer, the first bonding layer and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm;
[0047] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises:
[0048] Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is retracted relative to both the first adhesive layer and the second adhesive layer;
[0049] Disposing a support member with holes between the first transparent substrate and the second transparent substrate, so that the support member with holes contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer;
[0050] Laminating the laminated member provided with the third adhesive layer and the perforated support member;
[0051] After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
[0052] In some embodiments, the maximum width of the sealant layer is 1 mm to 5 mm.
[0053] In some embodiments, the water vapor transmission rate of the sealant layer is ≤10 -3 g / m 2 d; and / or,
[0054] The sealant layer includes one or more of a polyurethane sealant layer, a butyl sealant layer and a POE sealant layer;
[0055] Optionally, the sealant layer includes one or more of a butyl sealant layer and a POE sealant layer.
[0056] A vehicle comprises the dimming component mentioned above or comprises the dimming component prepared by the above preparation method.
[0057] In a conventional dimming component, the dimming layer is inwardly shrunk relative to the transparent substrate and the bonding layer. To protect the dimming layer, a filler layer is provided on the side of the dimming layer and between the first bonding layer and the second bonding layer. The filler layer is usually made of a bonding layer material having a thickness equivalent to that of the dimming layer. The inventors have found that conventional bonding layer materials have a poor ability to block water vapor. By increasing the length of the bonding layer, a certain ability to block water vapor can be achieved. However, when the dimming layer is relatively close to the edge of the transparent substrate, the water vapor blocking effect is relatively poor.
[0058] Based on this, some embodiments of the present application provide a dimming component, including a first transparent substrate, a second transparent substrate, a first bonding layer, a dimming layer, a second bonding layer and a sealant layer. The first bonding layer, the dimming layer and the second bonding layer are all retracted relative to the transparent substrate, and a sealant layer with a width of 1mm~20mm is set in at least part of the retracted area. The sealant layer can prevent water vapor from corroding the inside of the dimming layer, and still has a certain anti-water vapor erosion effect when the edge of the dimming layer is close to the edge of the transparent substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0060] Figure 1 A schematic diagram of the structure of a traditional dimming component;
[0061] Figure 2 A schematic diagram of a dimming component in some embodiments of the present application;
[0062] Figure 3 A schematic structural diagram of a dimming component in the first embodiment;
[0063] Figure 4 is another structural schematic diagram of the dimming component of the first embodiment;
[0064] Figure 5 A structural schematic diagram of a dimming component in a second embodiment;
[0065] Figure 6 A schematic structural diagram of a dimming component according to a third embodiment;
[0066] Figure 7 is another structural schematic diagram of a dimming component according to the third embodiment;
[0067] Figure 8 is a process flow chart of a method for preparing a dimming component according to a first embodiment;
[0068] Fig. 9 for Figure 8 A schematic diagram of the process flow diagram shown;
[0069] Fig.10 A schematic diagram of the structure of a perforated support member used;
[0070] Fig.11 is a process flow chart of a method for preparing a dimming component according to a second embodiment;
[0071] Fig.12 is a process flow chart of a method for preparing a dimming component according to a third embodiment;
[0072] Fig.13 This is a process flow chart of a method for preparing a dimming component according to a fourth embodiment.
[0073] Description of reference numerals:
[0074] Figure 1In the conventional dimming component 100, the first transparent substrate 110, the first bonding layer 120, the dimming layer 130, the second bonding layer 140, the second transparent substrate 150, the edge filling layer 160, the first ink layer 112 and the second ink layer 152;
[0075] Figure 3 and Figure 4 In the first embodiment, the dimming component 200, the first transparent substrate 210, the first bonding layer 220, the dimming layer 230, the second bonding layer 240, the second transparent substrate 250, the sealant layer 260, the surface activation layer 270, the first shielding layer 212 and the second shielding layer 252;
[0076] Figure 5 In the second embodiment, the dimming component 300, the first transparent substrate 310, the first bonding layer 320, the dimming layer 330, the second bonding layer 340, the second transparent substrate 350, the third bonding layer 360, the sealant layer 370, the surface activation layer 380, the first shielding layer 312 and the second shielding layer 352;
[0077] Figure 6 and Figure 7 In the third embodiment, the dimming component 400, the first transparent substrate 410, the first bonding layer 420, the dimming layer 430, the second bonding layer 440, the second transparent substrate 450, the third bonding layer 460, the sealant layer 470, the surface activation layer 480, the first shielding layer 412 and the second shielding layer 452. DETAILED DESCRIPTION
[0078] In order to facilitate the understanding of the present application, the present application will be described more comprehensively below in conjunction with the specific embodiments. The preferred embodiments of the present application are provided in the specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0079] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0080] Unless otherwise specified or there is a contradiction, the terms and phrases used in this application have the following meanings:
[0081] In this application, "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features.
[0082] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.
[0083] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0084] The terms "including" and "having" and any variations thereof in the embodiments of the present application are intended to cover non-exclusive inclusions. For example, a process, method, system, product, or device that includes a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units that are not listed, or may optionally include other steps or components that are inherent to these processes, methods, products, or devices.
[0085] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application may be combined with other embodiments.
[0086] As described in the background art, in a conventional dimming component, the dimming layer is indented relative to the transparent substrate and the bonding layer, and a filler layer is provided on the side of the dimming layer and between the first bonding layer and the second bonding layer. The filler layer is usually made of a bonding layer material with a thickness equivalent to that of the dimming layer. For example, see Figure 1The conventional dimming component 100 comprises a first transparent substrate 110, a first adhesive layer 120, a dimming layer 130, a second adhesive layer 140 and a second transparent substrate 150 which are stacked in sequence, and a filler layer 160 is arranged between the first adhesive layer 120 and the second adhesive layer 140. A first ink layer 112 is also arranged on the side of the first transparent substrate 110 away from the second transparent substrate 250, and a second ink layer 152 is also arranged on the side of the second transparent substrate facing the first transparent substrate. The materials of the first adhesive layer 120, the second adhesive layer 140 and the filler layer 160 are generally polyvinyl butyral (PVB), ethylene-vinyl acetate copolymer (EVA), etc., which have poor water vapor blocking ability and are suitable for the case where the edge of the dimming layer is far away from the edge of the transparent substrate (usually greater than 30 mm). By increasing the length of the adhesive layer to achieve a certain ability to block water vapor, for example, for skylight glass, the printing area is large, the edge of the dimming layer is far away from the edge of the glass, and the water vapor blocking effect of conventional dimming components can be achieved. However, in the case where the edge of the dimming layer is close to the edge of the glass substrate, for example, door and window glass, there is no ink printing area or the ink printing area is small, and the edge of the dimming layer is close to the edge of the glass substrate. Conventional adhesive layers such as PVB, EVA and other materials cannot meet the water and oxygen barrier requirements of dimming layers that are sensitive to water and oxygen, such as EC, SPD or nano-dimming LV, and are easily corroded by water and oxygen, causing edge degradation or even loss of function.
[0087] Based on this, the present application provides a dimming component and a preparation method thereof, which can improve its ability to block water vapor.
[0088] In a first aspect, the present application provides a dimming component, including:
[0089] a first transparent substrate;
[0090] A first bonding layer is disposed on the surface of the first transparent substrate;
[0091] The dimming layer is arranged on a surface of the first bonding layer on a side away from the first transparent substrate;
[0092] A second bonding layer is provided on a surface of the dimming layer away from the first transparent substrate;
[0093] A second transparent substrate is disposed on a surface of the second adhesive layer on a side away from the first transparent substrate;
[0094] Among them, the first bonding layer, the dimming layer and the second bonding layer are all retracted relative to the first transparent substrate and the second transparent substrate. The dimming component also includes a sealant layer, which is arranged in at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate. The side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate. The width of the sealant layer is 1mm~20mm.
[0095] The above-mentioned dimming component includes a first transparent substrate, a second transparent substrate, a first bonding layer, a dimming layer, a second bonding layer and a sealant layer. The first bonding layer, the dimming layer and the second bonding layer are all retracted relative to the transparent substrate. A sealant layer with a width of 1mm~20mm is set in at least part of the retracted area. The sealant layer can prevent water vapor from corroding the inside of the dimming layer, and still has a certain anti-water vapor erosion effect when the edge of the dimming layer is close to the edge of the transparent substrate.
[0096] In this article, contact includes direct contact and indirect contact. For example, the sealant layer contacting the first transparent substrate includes the sealant layer directly contacting the first transparent substrate without any other structure between the two, and also includes the sealant layer and the first transparent substrate contacting each other by providing one or more other structures, such as the surface activation layer mentioned below. Contact between other two layers has a similar meaning and will not be described in detail.
[0097] In some embodiments, the first transparent plastic substrate and the second transparent substrate are each independently selected from one of glass and polycarbonate (PC). In some embodiments, the surface of the first transparent substrate away from the second transparent substrate is the incident surface, that is, the first transparent substrate faces the direct sunlight exposure surface.
[0098] In some embodiments, a first shielding layer is provided on at least one surface of the first transparent substrate, the edge of the first shielding layer is flush with the edge of the first transparent substrate, and the width of the first shielding layer is less than or equal to 30 mm. Optionally, the width of the first shielding layer is 10 mm to 30 mm.
[0099] In some embodiments, there are two first shielding layers, and the two first shielding layers are spaced apart and symmetrically disposed at two ends of the first transparent substrate.
[0100] In one embodiment, the first shielding layer is arranged on a side surface of the first transparent substrate facing the second transparent substrate. It can be understood that in another embodiment, the first shielding layer can also be arranged on a side surface of the first transparent substrate away from the second transparent substrate, or the first shielding layer is arranged on both the side surfaces of the first transparent substrate facing and away from the second transparent substrate.
[0101] In one embodiment, the first shielding layer is an opaque layer relative to the first transparent substrate. For example, the first shielding layer can be, but is not limited to, an ink layer.
[0102] In some embodiments, a second shielding layer is provided on at least one surface of the second transparent substrate, the edge of the second shielding layer is flush with the edge of the second transparent substrate, and the width of the second shielding layer is less than or equal to 30 mm. Optionally, the width of the second shielding layer is 10 mm to 30 mm.
[0103] In some embodiments, there are two second shielding layers, and the two second shielding layers are spaced apart and symmetrically disposed at two ends of the first transparent substrate.
[0104] In one embodiment, the second shielding layer is arranged on a side surface of the second transparent substrate facing the first transparent substrate. It can be understood that in another embodiment, the second shielding layer can also be arranged on a side surface of the second transparent substrate away from the first transparent substrate, or the second shielding layer is arranged on both the side surfaces of the second transparent substrate facing and away from the first transparent substrate.
[0105] In one embodiment, the second shielding layer is an opaque layer relative to the second transparent substrate. For example, the second shielding layer can be, but is not limited to, an ink layer.
[0106] It can be understood that the width of the first shielding layer may be the same as or different from the width of the second shielding layer. Optionally, the width of the first shielding layer is the same as the width of the second shielding layer.
[0107] In some embodiments, the first adhesive layer and the second adhesive layer are each independently one of a PVB adhesive layer and an EVA adhesive layer. Specifically, the PVB adhesive layer and the EVA adhesive layer can be ordinary adhesive layers or adhesive layers with UV isolation effect. In some embodiments, the PVB adhesive layer and the EVA adhesive layer can be adhesive layers with high UV isolation, for example, the UV cutoff band is ≥390nm, and the isolation rate is ≥99%. Optionally, the UV cutoff band is 400nm.
[0108] In some of the embodiments, the first adhesive layer is closer to the first transparent substrate than the second adhesive layer, the first adhesive layer is selected from one of a PVB adhesive layer with a UV shielding effect and an EVA adhesive layer with a UV shielding effect, and the second adhesive layer is selected from one of an ordinary PVB adhesive layer without a UV shielding effect and an ordinary EVA adhesive layer without a UV shielding effect.
[0109] In some embodiments, the dimming layer is selected from one of an EC (electroluminescence) dimming layer, an SPD (suspended particle) dimming layer, an LV nano light valve dimming layer, and a dye liquid crystal dimming layer (abbreviated as LC or DLC). Specifically, the dimming layer has an electrode.
[0110] In some embodiments, the dimming layer is retracted by 3 mm to 30 mm relative to the first transparent substrate and the second transparent substrate. Optionally, the dimming layer is retracted by 3 mm to 15 mm relative to the first transparent substrate and the second transparent substrate. Optionally, the dimming layer is retracted by 3 mm to 10 mm relative to the first transparent substrate and the second transparent substrate. The specific retracted distance can be adjusted according to the purpose of the dimming component.
[0111] In some embodiments, the water vapor transmission rate of the sealant layer is ≤10-3 g / m 2 ·d (g / m2·day). The test reference standard for water vapor transmission rate is ISO 15106-3.
[0112] Specifically, the sealant layer includes one or more of a polyurethane sealant layer, a butyl layer and a POE sealant layer. Optionally, the sealant layer includes one or more of a butyl layer and a POE sealant layer. It can be understood that only several commonly used sealant layers are given above, but are not limited thereto.
[0113] In some embodiments, the width of the sealant layer is greater than or equal to 1 mm. For example, the width of the sealant layer can be, but is not limited to, 1 mm, 2 mm, 3 mm, 5 mm, 8 mm, 10 mm, 12 mm, 15 mm, 18 mm, 20 mm, 25 mm, 30 mm, or a range consisting of any two of these values. It is understood that the width of the sealant layer is less than or equal to the width of the first bonding layer, the dimming layer, and the second bonding layer relative to the first transparent substrate and the second transparent substrate indentation area. The specific width of the sealant layer can be adjusted according to the width of the indentation area. In some embodiments, the width of the sealant layer is 1 mm to 20 mm, 1 mm to 15 mm, 1 mm to 10 mm, etc.
[0114] In some embodiments, the thickness of the sealant layer is equal to the total thickness of the first bonding layer, the dimming layer and the second bonding layer, wherein the thickness equal means that the absolute value of the difference between the thickness of the sealant layer and the total thickness of the first bonding layer, the dimming layer and the second bonding layer is ≤ 0.2 mm.
[0115] In some embodiments, a surface activation layer is further provided on the surface of the sealant layer facing the first transparent substrate and the second transparent substrate, and on the side of the sealant layer facing the first bonding layer, the second bonding layer and the dimming layer. The surface activation layer is provided to improve the adhesion between the sealant layer and the first transparent substrate, the second transparent substrate and the bonding layer, and further improve the anti-water vapor erosion effect.
[0116] In some embodiments, the material of the surfactant layer includes a surfactant.
[0117] In some embodiments, the sealant layer is disposed on three sides of the dimming component. Figure 2 An electrode line is arranged at the bottom edge of the dimming component, and a sealant layer is not required here, and a sealant layer can be arranged on the other three sides.
[0118] The following is a detailed description of the dimming component and its structure in combination with different settings of the sealant layer:
[0119] In the first embodiment, the first bonding layer, the dimming layer and the second bonding layer are flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is less than or equal to 5 mm. The sealant layer is arranged between the first transparent substrate and the second transparent substrate, and the side edge contacts the first bonding layer and the second bonding layer.
[0120] Specifically, see Figure 3 The dimming component 200 includes a first transparent substrate 210, a first adhesive layer 220, a dimming layer 230, a second adhesive layer 240 and a second transparent substrate 250 which are stacked in sequence. The first adhesive layer 220, the dimming layer 230 and the second adhesive layer 240 are all retracted relative to the first transparent substrate 210 and the second transparent substrate 250. A sealant layer 260 is also disposed between the first transparent substrate 210 and the second transparent substrate 250. The sealant layer 260 contacts the side edges of the first adhesive layer 220 and the second adhesive layer 240, and the side edges do not exceed the side edges of the first transparent substrate 210 and the second transparent substrate 250. A first shielding layer 212 is disposed on a side of the first transparent substrate 210 away from the second transparent substrate 250, and a second shielding layer 252 is disposed on a side of the second transparent substrate facing the first transparent substrate 250.
[0121] The above configuration is helpful to improve the water vapor corrosion resistance of the dimming component 200.
[0122] In some embodiments, the dimming layer 230 is flush with the first adhesive layer 220 and the second adhesive layer 240, or the dimming layer 230 is retracted relative to the first adhesive layer 220 and the second adhesive layer 240, and the retracted distance is less than or equal to 5 mm. In the case where the dimming layer 230 is less sensitive to water vapor, for example, the dimming layer 230 is a PDLC dimming layer, which is not sensitive to water and oxygen and does not react with the sealant layer 260, in this case, the dimming layer 230 can be set to be flush with the first adhesive layer 220 and the second adhesive layer 240. In the case where the dimming layer 230 is sensitive to water and oxygen, for example, the dimming layer 230 is an EC dimming layer, by shrinking the dimming layer 230 relative to the first adhesive layer 220 and the second adhesive layer 240 by less than or equal to 5 mm, during the lamination process, the first adhesive layer 220 and the second adhesive layer 240 soften and wrap the dimming layer 230, further improving the waterproof oxygen erosion effect of the dimming component 200.
[0123] In some embodiments, the sealant layer 260 fills the entire area where the first adhesive layer 220 and the second adhesive layer 240 are retracted relative to the first transparent substrate 210 and the second transparent substrate 250. Specifically, the width of the area where the first adhesive layer 220 and the second adhesive layer 240 are retracted relative to the first transparent substrate 210 and the second transparent substrate 250 is greater than or equal to 3 mm. At this time, the width of the sealant layer 260 is greater than or equal to 3 mm.
[0124] It can be understood that the width of the sealant layer 260 can be adjusted according to the width of the retracted area of the first adhesive layer 220 and the second adhesive layer 240 relative to the first transparent substrate 210 and the second transparent substrate 250. For example, the width of the retracted area of the first adhesive layer 220 and the second adhesive layer 240 relative to the first transparent substrate 210 and the second transparent substrate 250 is 3mm~15mm, and the width of the sealant layer 260 is 3mm~15mm. Alternatively, the width of the retracted area of the first adhesive layer 220 and the second adhesive layer 240 relative to the first transparent substrate 210 and the second transparent substrate 250 is 3mm~10mm, and the width of the sealant layer 260 is 3mm~10mm.
[0125] It can be understood that in some other embodiments, the sealant layer 260 can also fill the partial area where the first bonding layer 220 and the second bonding layer 240 are retracted relative to the first transparent substrate 210 and the second transparent substrate 250, as long as the width of the sealant layer 260 is 3mm~10mm. Optionally, the width of the sealant layer 260 is 6mm.
[0126] Please also read Figure 4 In some embodiments, the dimming component 200 further includes a surface activation layer 270. The surface activation layer 270 is disposed on a surface of the sealant layer 260 facing the first transparent substrate 210 and the second transparent substrate 250, and a surface of the sealant layer 260 facing the first bonding layer 220, the second bonding layer 240 and the dimming layer 230.
[0127] exist Figure 3 and Figure 4 In the embodiment, the side surfaces of the dimming layer 230 and the side surfaces of the first bonding layer 220 and the second bonding layer 240 are sealed by the sealant layer 260, which is beneficial to improve the water vapor erosion resistance effect.
[0128] In the second embodiment, the dimming layer is retracted relative to the first adhesive layer and the second adhesive layer, the retracted distance is greater than 5 mm, a third adhesive layer is further provided between the first adhesive layer and the second adhesive layer, the third adhesive layer contacts the side edge of the dimming layer, and the sealant layer contacts the first adhesive layer, the second adhesive layer and the third adhesive layer. The first adhesive layer, the second adhesive layer and the third adhesive layer are all flush.
[0129] Specifically, see Figure 5The dimming component 300 includes a first transparent substrate 310, a first adhesive layer 320, a dimming layer 330, a second adhesive layer 340 and a second transparent substrate 350 which are stacked in sequence. The dimming layer 330 is retracted relative to the first adhesive layer 320 and the second adhesive layer 340, and the retracted distance is greater than 5 mm. A third adhesive layer 360 is further provided between the first adhesive layer 320 and the second adhesive layer 340, and the third adhesive layer 360 contacts the side edge of the dimming layer 330. The third adhesive layer 360 is flush with the first adhesive layer 320 and the second adhesive layer 340, and is retracted relative to the first transparent substrate 310 and the second transparent substrate 350. A sealant layer 370 is further provided between the first transparent substrate 310 and the second transparent substrate 350, and the sealant layer 370 contacts the first adhesive layer 320, the second adhesive layer 340 and the third adhesive layer 360. A first shielding layer 312 is disposed on a side of the first transparent substrate 310 away from the second transparent substrate 350 , and a second shielding layer 352 is disposed on a side of the second transparent substrate 350 facing the first transparent substrate 310 .
[0130] Specifically, the width of the sealant layer 370 is 1 mm to 5 mm.
[0131] exist Figure 5 In the embodiment, the third adhesive layer 360 is flush with the first adhesive layer 320 and the second adhesive layer 340, and the width of the sealant layer 370 is equal from the first adhesive layer 320 to the third adhesive layer 360 and from the second adhesive layer 340 to the third adhesive layer 360.
[0132] In some embodiments, the third adhesive layer 360 is one of a PVB adhesive layer and an EVA adhesive layer. It is understood that the third adhesive layer 360 can be the same as the first adhesive layer 320 and the second adhesive layer 340, or different.
[0133] exist Figure 5 In the embodiment, the dimming component 300 is further provided with a surface activation layer 380. It is understood that in other embodiments, the surface activation layer 380 may also be omitted.
[0134] Figure 5 The dimming component 300 and Figure 3 and Figure 4 The difference between the dimming component 200 is that Figure 5 In the figure, the dimming layer 330 is retracted a large distance relative to the first bonding layer 320 and the second bonding layer 340, and a third bonding layer 360 is provided in the retracted area of the dimming layer 330 relative to the first bonding layer 320 and the second bonding layer 340. On the one hand, the water and oxygen erosion resistance is further improved, and on the other hand, the dimming layer 330 is protected during the lamination process.
[0135] In the third embodiment, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is greater than 5 mm. A third bonding layer is also provided between the first bonding layer and the second bonding layer, and the third bonding layer contacts the side edge of the dimming layer. The sealant layer contacts the first bonding layer, the second bonding layer and the third bonding layer. The third bonding layer is retracted relative to the first bonding layer and the second bonding layer, and the width of the sealant layer increases from the first bonding layer to the third bonding layer and from the second bonding layer to the third bonding layer.
[0136] Specifically, see Figure 6 and Figure 7 The dimming component 400 includes a first transparent substrate 410, a first adhesive layer 420, a dimming layer 430, a second adhesive layer 440 and a second transparent substrate 450 which are stacked in sequence. The dimming layer 430 is retracted relative to the first adhesive layer 420 and the second adhesive layer 440, and the retracted distance is greater than 5 mm. A third adhesive layer 460 is further provided between the first adhesive layer 420 and the second adhesive layer 440, and the third adhesive layer 460 contacts the side edge of the dimming layer 430. The first adhesive layer 420 and the second adhesive layer 440 are both retracted relative to the first transparent substrate 410 and the second transparent substrate 450. A sealant layer 470 is further provided between the first transparent substrate 410 and the second transparent substrate 450, and the sealant layer 470 contacts the first adhesive layer 420, the second adhesive layer 440 and the third adhesive layer 460. The third adhesive layer 460 is retracted relative to the first adhesive layer 420 and the second adhesive layer 440 , and the width of the sealant layer 470 increases from the first adhesive layer 420 to the third adhesive layer 460 and from the second adhesive layer 440 to the third adhesive layer 460 .
[0137] Specifically, the maximum width of the sealant layer 470 is 1 mm to 5 mm. It can be understood that the maximum width of the sealant layer 470 is the width of the sealant layer 470 corresponding to the side of the dimming layer 430 .
[0138] exist Figure 6 and Figure 7 In the embodiment, the dimming component 400 is further provided with a surface activation layer 480. It is understood that in other embodiments, the surface activation layer 480 may also be omitted.
[0139] Understandably, the above Figure 6 and Figure 7 Only two schematic diagrams of different shapes of the sealant layer are provided, but the present invention is not limited thereto. The shape of the sealant layer can also be adjusted according to actual conditions, as long as the maximum width of the sealant layer is 1 mm to 5 mm.
[0140] exist Figure 5~Figure 7 In the embodiment, a third bonding layer and a sealing adhesive layer are provided on the side of the dimming layer, and the cooperation of the third bonding layer and the sealing adhesive layer can improve the water vapor erosion resistance of the dimming component.
[0141] In a second aspect, the present application provides a method for preparing a dimming component, comprising the following steps:
[0142] Obtaining a laminate, the laminate comprising a first transparent substrate, a first bonding layer, a dimming layer, a second bonding layer, and a second transparent substrate stacked in sequence;
[0143] The dimming layer, the first bonding layer and the second bonding layer in the stack are retracted relative to the first transparent substrate and the second transparent substrate;
[0144] A sealant layer is arranged between the first transparent substrate and the second transparent substrate of the stack, so that the sealant layer fills at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate, the side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate, and the width of the sealant layer is greater than or equal to 1 mm, thereby obtaining a dimming component.
[0145] Herein, the term "stacked in sequence" is only used to indicate the stacking order between the layers, and other layers may be stacked between the layers without any particular limitation.
[0146] In some embodiments, in the step of causing the dimming layer, the first bonding layer, and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the first bonding layer, the dimming layer, and the second bonding layer are made flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is less than or equal to 5 mm;
[0147] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate of the stack so that the sealant layer fills at least a portion of the retracted area comprises:
[0148] Disposing a perforated support member between the first transparent substrate and the second transparent substrate so that the perforated support member contacts the side edges of the first adhesive layer and the second adhesive layer;
[0149] Laminating the laminated member provided with the perforated support member;
[0150] After the lamination is completed, the support member with holes is removed, and a sealant layer is filled in the area where the support member with holes is located.
[0151] In some other embodiments, in the step of causing the dimming layer, the first bonding layer, and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm;
[0152] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises:
[0153] Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer so that the third adhesive layer is flush with the first adhesive layer and the second adhesive layer;
[0154] Disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer to obtain a laminate;
[0155] Laminating the laminated member provided with the third adhesive layer and the perforated support member;
[0156] After the lamination is completed, the support member with holes is removed, and a sealant layer is filled in the area where the support member with holes is located.
[0157] In some further embodiments, a method for preparing a dimming component includes:
[0158] Obtaining a laminated component, wherein the first adhesive layer and the second adhesive layer in the laminated component are flush with the first transparent substrate and the second transparent substrate, and the dimming layer is retracted relative to the first adhesive layer and the second adhesive layer;
[0159] Disposing a third bonding layer between the first bonding layer and the second bonding layer, so that the third bonding layer contacts the side edge of the dimming layer and is flush with the first bonding layer and the second bonding layer;
[0160] Laminating the laminated member provided with the third adhesive layer;
[0161] After the lamination is completed, a portion of the first adhesive layer, a portion of the second adhesive layer and a portion of the third adhesive layer are removed, so that the first adhesive layer, the second adhesive layer and the third adhesive layer are all retracted relative to the first transparent substrate and the second transparent substrate;
[0162] The sealing layer is filled in the removed areas of the first bonding layer, the second bonding layer and the third bonding layer to prepare a dimming component.
[0163] In some other embodiments, in the step of causing the dimming layer, the first bonding layer, and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm;
[0164] The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises:
[0165] A third adhesive layer is arranged between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is retracted relative to the first adhesive layer and the second adhesive layer;
[0166] Disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer;
[0167] Laminating the laminated member provided with the third adhesive layer and the perforated support member;
[0168] After the lamination is completed, the support member with holes is removed, and a sealant layer is filled in the area where the support member with holes is located.
[0169] The following describes in detail the preparation methods of the above dimming components in combination with the different structures of the dimming components.
[0170] Specifically, in the first embodiment, the structure of the dimming component is as follows: Figure 3 Please refer to Figure 8 , the preparation method of the dimming component comprises the following steps:
[0171] Step S510: Stack the first transparent substrate, the first bonding layer, the dimming layer, the second bonding layer and the second transparent substrate in sequence to obtain a stacked piece, so that the first bonding layer, the dimming layer and the second bonding layer are flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is less than or equal to 5 mm, and the first bonding layer and the second bonding layer are both retracted relative to the first transparent substrate and the second transparent substrate.
[0172] Step S520: disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer and the second adhesive layer.
[0173] Step S530: Pressing the stacked parts provided with the perforated support parts.
[0174] Step S540: After the pressing is completed, the support member with holes is removed.
[0175] Step S550: Filling a sealant layer in the area where the perforated support member is located to prepare a dimming component.
[0176] By adopting the above method, it is possible to realize the preparation of dimming components, such as door glass, in which the dimming layer that is sensitive to water and oxygen is close to the edge of the glass (≤30mm, further ≤20mm). In addition, when the pieces are packaged together, the size of the bonding layer and the dimming layer is comparable (that is, the side edges of the first bonding layer, the dimming layer and the second bonding layer are flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is less than or equal to 5mm), which is beneficial to reduce the dimming layer edge filling process and improve efficiency. And when the pieces are packaged together, a perforated support member of equal thickness is used to fill the retracted area to avoid the thickness difference of the edge of the transparent substrate caused by the processing process, and at the same time, the local stress (fragile) of the glass is formed due to the thickness difference. And the use of a perforated support member is conducive to the discharge of gas during the assembly process.
[0177] Figure 8 This is a flow chart of a method for preparing a dimming component according to an embodiment of the present application. It should be understood that although Figure 8 The steps in the flowchart are shown in sequence as indicated by the arrows, but these steps are not necessarily performed in the order indicated by the arrows. Unless otherwise specified in this document, there is no strict order restriction for the execution of these steps, and they can be performed in other orders. Figure 8 At least part of the steps may include multiple sub-steps or multiple stages. These sub-steps or stages are not necessarily executed at the same time, but can be executed at different times. The order of execution is not necessarily sequential, but can be executed in turn or alternately with other steps or at least part of other sub-steps or stages.
[0178] In some embodiments, please refer to Fig. 9 , Fig. 9 for Figure 8 A schematic diagram of a process flow chart for preparing a dimming component is shown. Fig. 9 In the figure, a is a schematic diagram of step S510, wherein the first transparent substrate 210, the first adhesive layer 220, the dimming layer 230, the second adhesive layer 240 and the second transparent substrate 250 are sequentially stacked to obtain a stacked component, so that the first adhesive layer 220, the dimming layer 230 and the second adhesive layer 240 are flush or the dimming layer 230 is retracted relative to the first adhesive layer 220 and the second adhesive layer 240, and the retraction distance is less than or equal to 5 mm, and the first adhesive layer 220 and the second adhesive layer 240 are both retracted relative to the first transparent substrate 210 and the second transparent substrate 250. b is a schematic diagram of step S520, wherein a perforated support member 280 is provided between the first transparent substrate 210 and the second transparent substrate 250, so that the perforated support member 280 is in contact with the side edges of the first adhesive layer 220 and the second adhesive layer 240. c is a schematic diagram of step S530, wherein the stacked component provided with the perforated support member 280 is pressed. d is a schematic diagram of step S540, after the pressing is completed, the support member with holes 280 is removed. e is a schematic diagram of step S550, the sealant layer 260 is filled in the area where the support member with holes is located to prepare a dimming component.
[0179] Understandably, Fig. 9 In the embodiment, the hole in the hole-bearing support member 280 is in the shape of a triangle, but is not limited thereto. Fig.10 , Fig.10 Schematic diagrams of longitudinal sections of several common perforated support structures are given. Fig.10 In the figure, from left to right, the perforated support member has a circular through hole on the side, a semicircular blind hole on the upper surface and the lower surface, and a triangular blind hole on the upper surface and the lower surface. It can be understood that in other embodiments, the perforated support member can also have circular through holes on the upper surface and the lower surface. The longitudinal section refers to a plane cut along a direction perpendicular to the upper and lower surfaces.
[0180] In some embodiments, the material of the perforated support member includes but is not limited to Teflon. For example, the perforated support member can be but is not limited to a perforated Teflon plug.
[0181] In some embodiments, the pressing process may be commonly used in the art, for example, the pressing process includes initial pressing and high pressing.
[0182] In some embodiments, the thickness of the sealant layer is equal to the total thickness of the first bonding layer, the dimming layer and the second bonding layer, wherein the thickness equal means that the absolute value of the difference between the thickness of the sealant layer and the total thickness of the first bonding layer, the dimming layer and the second bonding layer is ≤ 0.2 mm.
[0183] In some embodiments, the method further includes: a step of scraping glue. Specifically, the excess sealant is removed by flat scraping or U-shaped scraping.
[0184] In some embodiments, the sealant layer is filled within 8 hours after lamination.
[0185] It can be understood that in the actual process, after the sheets are assembled, a sealant layer is used to seal the three sides of the transparent substrate (the distance between the dimming layer and the edge of the transparent substrate is ≤30 mm, and further ≤20 mm).
[0186] In some embodiments, before the step of filling the sealant layer in the area where the perforated support member is located, the step further includes filling the surface activation layer in the area where the perforated support member is located. By filling the surface activation layer first and then filling the sealant layer, it is beneficial to improve the adhesion between the sealant layer and the first transparent substrate, the second transparent substrate and the bonding layer, and further improve the anti-water vapor erosion effect.
[0187] In the second embodiment, the structure of the dimming component is as follows: Figure 5 Please refer to Fig.11 , the preparation method of the dimming component comprises the following steps:
[0188] Step S610: stack the first transparent substrate, the first bonding layer, the dimming layer, the second bonding layer and the second transparent substrate in sequence to obtain a stacked component, so that the dimming layer is retracted relative to the first bonding layer and the second bonding layer, the retraction distance is greater than 5 mm, and the first bonding layer and the second bonding layer are retracted relative to the first transparent substrate and the second transparent substrate.
[0189] Step S620: Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer so that the third adhesive layer is flush with the first adhesive layer and the second adhesive layer.
[0190] Step S630: disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer.
[0191] Step S640: Laminating the laminated member provided with the third adhesive layer and the perforated support member.
[0192] Step S650: After the pressing is completed, the support member with holes is removed.
[0193] Step S660: Filling a sealant layer in the area where the perforated support member is located to prepare a dimming component.
[0194] The difference between the preparation method of the dimming component of the second embodiment and the preparation method of the dimming component of the first embodiment is that before the step of providing the perforated support member between the first transparent substrate and the second transparent substrate, a third bonding layer is provided between the first bonding layer and the second bonding layer. The other steps are the same as those of the first embodiment and will not be repeated.
[0195] In some embodiments, the thickness of the third bonding layer is comparable to that of the dimming layer, wherein the comparable thickness means that the absolute value of the difference between the thickness of the third bonding layer and the thickness of the dimming layer is ≤ 0.2 mm.
[0196] In the third embodiment, the structure of the dimming component is as follows: Figure 6 and Figure 7 Please refer to Fig.12 The preparation method of the dimming component of the third embodiment comprises the following steps:
[0197] Step S710: stack the first transparent substrate, the first bonding layer, the dimming layer, the second bonding layer and the second transparent substrate in sequence to obtain a stacked component, so that the first transparent substrate, the first bonding layer, the second bonding layer and the second transparent substrate are flush, and the dimming layer is retracted relative to the first bonding layer and the second bonding layer.
[0198] Step S720: a third bonding layer is disposed between the first bonding layer and the second bonding layer, so that the third bonding layer contacts the side edge of the dimming layer and is flush with the first bonding layer and the second bonding layer.
[0199] Step S730: Laminating the laminated member provided with the third adhesive layer.
[0200] Step S740: after lamination, remove part of the first adhesive layer, part of the second adhesive layer and part of the third adhesive layer, so that the first adhesive layer, the second adhesive layer and the third adhesive layer are all retracted relative to the first transparent substrate and the second transparent substrate.
[0201] Step S750: Filling a sealant layer in the removed areas of the first adhesive layer, the second adhesive layer, and the third adhesive layer to prepare a dimming component.
[0202] In some embodiments, a hook knife is used to remove a portion of the first adhesive layer, a portion of the second adhesive layer, and a portion of the third adhesive layer.
[0203] In some embodiments, before the step of filling the sealant layer in the removed regions of the first adhesive layer, the second adhesive layer, and the third adhesive layer, the step of filling the surface activation layer in the removed regions of the first adhesive layer, the second adhesive layer, and the third adhesive layer is included. By filling the surface activation layer first and then the sealant layer, it is beneficial to improve the adhesion between the sealant layer and the first transparent substrate, the second transparent substrate, and the adhesive layer, and further improve the anti-water vapor erosion effect.
[0204] The preparation method of the dimming component of the third embodiment mentioned above can adopt the traditional dimming component assembly and packaging process, without changing the existing process and production line. After assembly, in the packaging stage, a hook knife is used to trim off part of the adhesive layer, and then the sealant layer is filled in the removed adhesive layer area. After sealing, the dimming component is protected from erosion by water (oxygen) vapor, and finally the product requirement of the dimming layer being narrow from the edge of the transparent substrate is achieved.
[0205] It can be understood that in other embodiments, the structure of the dimming component is as follows: Figure 5 As shown, the preparation method of the dimming component can also adopt the preparation method of the third embodiment. At this time, in step S740, after the lamination is completed, a part of the first adhesive layer, a part of the second adhesive layer and a part of the third adhesive layer are removed, and in the step of making the first adhesive layer, the second adhesive layer and the third adhesive layer shrink relative to the first transparent substrate and the second transparent substrate, the area of the removed first adhesive layer, the removed second adhesive layer and the removed third adhesive layer is the same.
[0206] In the fourth embodiment, the structure of the dimming component is as follows: Figure 6 and Figure 7 Please refer to Fig.13 The preparation method of the dimming component of the fourth embodiment comprises the following steps:
[0207] Step S810: stack the first transparent substrate, the first bonding layer, the dimming layer, the second bonding layer and the second transparent substrate in sequence to obtain a stacked piece, so that the dimming layer is retracted relative to the first bonding layer and the second bonding layer, the retraction distance is greater than 5 mm, and the first bonding layer and the second bonding layer are retracted relative to the first transparent substrate and the second transparent substrate.
[0208] Step S820: Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is retracted relative to both the first adhesive layer and the second adhesive layer.
[0209] Step S830: disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer.
[0210] Step S840: Laminating the laminated member provided with the third adhesive layer and the perforated support member.
[0211] Step S850: After the pressing is completed, the support member with holes is removed.
[0212] Step S860: Fill a sealant layer in the area where the perforated support member is located to prepare a dimming component.
[0213] It can be understood that in step S820, the third adhesive layer is inwardly contracted relative to the first adhesive layer and the second adhesive layer, that is, the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer are irregular. In step S830, by providing a special-shaped perforated support member, the perforated support member is in contact with the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer. The specific shape of the perforated support member can be adjusted according to the shape of the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer.
[0214] In a third aspect, the present application provides a vehicle, comprising the dimming component of the first aspect or a dimming component prepared by the preparation method of the dimming component of the second aspect.
[0215] In some of the embodiments, the dimming component can be used as a door glass or a sunroof glass of a vehicle.
[0216] In order to make the purpose and advantages of the present application clearer, the dimming component of the present application and its effects are further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and shall not be used to limit the present application. The following embodiments do not include other components except unavoidable impurities unless otherwise specified. The drugs and instruments used in the examples are conventionally selected in the art unless otherwise specified. The experimental methods for which specific conditions are not specified in the examples are implemented according to conventional conditions, such as the conditions described in the literature and books or the methods recommended by the manufacturer.
[0217] Example 1
[0218] This embodiment provides a dimming component, the structure of which is as follows Figure 3As shown, the dimming component 200 includes a first transparent substrate 210, a first adhesive layer 220, a dimming layer 230, a second adhesive layer 240 and a second transparent substrate 250 which are stacked in sequence. The dimming layer 230 is flush with the first adhesive layer 220 and the second adhesive layer 240, and is retracted relative to the first transparent substrate 210 and the second transparent substrate 250, and the retracted distance is 5mm. A sealant layer 260 is also arranged between the first transparent substrate 210 and the second transparent substrate 250. Among them, the first transparent substrate 210 and the second transparent substrate 220 are both glass, and the first adhesive layer 220 and the second adhesive layer 240 are both PVB adhesive layers. The dimming layer 230 is an EC dimming layer, and the sealant layer 260 is butyl rubber. The width of the sealant layer 260 is 5mm.
[0219] Example 2
[0220] This embodiment provides a dimming component, which is similar to the dimming component of Embodiment 1, except that the first bonding layer 220, the dimming layer 230 and the second bonding layer 240 are all retracted relative to the first transparent substrate 210 and the second transparent substrate 250, the retracted distance is 10 mm, and the width of the sealant layer 260 is 10 mm.
[0221] Example 3
[0222] This embodiment provides a dimming component, which is similar to the dimming component of Embodiment 1, except that the first bonding layer 220, the dimming layer 230 and the second bonding layer 240 are all retracted relative to the first transparent substrate 210 and the second transparent substrate 250, the retracted distance is 20 mm, and the width of the sealant layer 260 is 20 mm. The sealant layer 260 is a polyurethane sealant.
[0223] Example 4
[0224] This embodiment provides a dimming component, which is similar to the dimming component of Embodiment 1, except that the dimming layer 230 is an LV dimming layer, the first bonding layer 220, the dimming layer 230 and the second bonding layer 240 are all retracted relative to the first transparent substrate 210 and the second transparent substrate 250, the retracted distance is 10 mm, and the width of the sealant layer 260 is 10 mm. The sealant layer 260 is POE sealant.
[0225] Comparative Example 1
[0226] Comparative Example 1 provides a dimming component, which is similar to the dimming component of Example 1, except that the sealant layer in Comparative Example 1 is replaced by a PVB adhesive layer.
[0227] Comparative Example 2
[0228] Comparative Example 2 provides a dimming component, which is similar to the dimming component of Example 2, except that the sealant layer in Comparative Example 2 is replaced by a PVB adhesive layer.
[0229] Comparative Example 3
[0230] Comparative Example 3 provides a dimming component, which is similar to the dimming component of Example 3, except that the sealant layer in Comparative Example 3 is replaced by a PVB adhesive layer.
[0231] Comparative Example 4
[0232] Comparative Example 4 provides a dimming component, which is similar to the dimming component of Example 4, except that the sealant layer in Comparative Example 4 is replaced by a PVB adhesive layer.
[0233] The dimming components of the above-mentioned embodiment and comparative example were subjected to a damp heat test, and the test results are shown in Table 1 below.
[0234] Table 1 Results of damp heat tests on dimming components of various embodiments and comparative examples
[0235]
[0236] In Table 1 above, in Comparative Example 1, the EC film edge 10mm~20mm abnormality refers to the abnormality occurring in the dimming layer within the dimming layer, 10mm~20mm away from the edge of the dimming layer. Other comparative examples have similar meanings and will not be repeated.
[0237] It can be seen from Table 1 above that the provision of a sealant layer is beneficial to improving the water vapor erosion resistance of the dimming component. Figure 4~Figure 7 When the sealant layer is provided, it is also beneficial to improve the water vapor erosion resistance of the dimming component, which will not be described in detail here.
[0238] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0239] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.
Claims
1. A dimming component, characterized in that: include: a first transparent substrate; A first adhesive layer is disposed on the surface of the first transparent substrate; A dimming layer is disposed on a surface of the first bonding layer on a side away from the first transparent substrate; A second bonding layer is disposed on a surface of the dimming layer away from the first transparent substrate; A second transparent substrate is disposed on a surface of the second adhesive layer that is away from the first transparent substrate; Among them, the first bonding layer, the dimming layer and the second bonding layer are all retracted relative to the first transparent substrate and the second transparent substrate, and the dimming component also includes a sealant layer, which is arranged in at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate, and the side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate, and the width of the sealant layer is 1mm~20mm.
2. The dimming component according to claim 1, characterized in that: The first bonding layer, the dimming layer and the second bonding layer are flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retraction distance is less than or equal to 5 mm, and the side edge of the sealant layer contacts the first bonding layer and the second bonding layer.
3. The dimming component according to claim 1, characterized in that: The dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm. A third bonding layer is also provided between the first bonding layer and the second bonding layer, and the third bonding layer contacts the side edge of the dimming layer. The sealant layer contacts the first bonding layer, the second bonding layer and the third bonding layer.
4. The dimming component according to claim 3, characterized in that: The third bonding layer is flush with both the first bonding layer and the second bonding layer; or, The third adhesive layer is retracted relative to the first adhesive layer and the second adhesive layer, and the width of the sealant layer increases gradually from the first adhesive layer to the third adhesive layer and from the second adhesive layer to the third adhesive layer.
5. The dimming component according to any one of claims 1 to 4, characterized in that: A surface activation layer is also provided on one surface of the sealant layer facing the first transparent substrate and the second transparent substrate, and on one surface of the sealant layer facing the first bonding layer, the second bonding layer and the dimming layer.
6. A method for preparing a dimming component, characterized in that: The steps include: Obtaining a laminate, wherein the laminate comprises a first transparent substrate, a first bonding layer, a dimming layer, a second bonding layer, and a second transparent substrate stacked in sequence; Retract the dimming layer, the first bonding layer and the second bonding layer in the stack relative to the first transparent substrate and the second transparent substrate; A sealant layer is arranged between the first transparent substrate and the second transparent substrate of the stack, so that the sealant layer fills at least part of the retracted area and contacts the first transparent substrate and the second transparent substrate, the side edge of the sealant layer does not exceed the side edge of the first transparent substrate and the second transparent substrate, and the width of the sealant layer is greater than or equal to 1 mm, to obtain a dimming component.
7. The method for preparing a dimming component according to claim 6, characterized in that: The width of the sealant layer is 1 mm to 20 mm; Optionally, the width of the sealant layer is 1 mm to 10 mm.
8. The method for preparing a dimming component according to claim 6 or 7, characterized in that: In the step of causing the dimming layer, the first bonding layer and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the first bonding layer, the dimming layer and the second bonding layer are made flush or the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is less than or equal to 5 mm; The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate of the stacked component so that the sealant layer fills at least a portion of the retracted area comprises: Disposing a perforated support member between the first transparent substrate and the second transparent substrate, so that the perforated support member contacts the side edges of the first adhesive layer and the second adhesive layer; Pressing the stacked member provided with the perforated support member; After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
9. The method for preparing a dimming component according to claim 8, characterized in that: The width of the sealant layer is greater than or equal to 3 mm; Optionally, the width of the sealant layer is 3 mm to 10 mm.
10. The method for preparing a dimming component according to claim 6, characterized in that: In the step of causing the dimming layer, the first bonding layer and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm; The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises: Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is flush with the first adhesive layer and the second adhesive layer; Disposing a support member with holes between the first transparent substrate and the second transparent substrate, so that the support member with holes contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer; Laminating the laminated member provided with the third adhesive layer and the perforated support member; After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
11. The method for preparing a dimming component according to claim 6, characterized in that: The preparation method comprises: Obtaining the laminate, making the first adhesive layer and the second adhesive layer in the laminate flush with the first transparent substrate and the second transparent substrate, and the dimming layer retracted relative to the first adhesive layer and the second adhesive layer; Disposing a third bonding layer between the first bonding layer and the second bonding layer, so that the third bonding layer contacts the side edge of the dimming layer and is flush with the first bonding layer and the second bonding layer; Laminating the laminated member provided with the third adhesive layer; After the lamination is completed, a portion of the first adhesive layer, a portion of the second adhesive layer and a portion of the third adhesive layer are removed, so that the first adhesive layer, the second adhesive layer and the third adhesive layer are all retracted relative to the first transparent substrate and the second transparent substrate; The dimming component is prepared by filling the sealant layer in the removed areas of the first bonding layer, the second bonding layer and the third bonding layer.
12. The method for preparing a dimming component according to claim 6, characterized in that: In the step of causing the dimming layer, the first bonding layer and the second bonding layer in the stack to retract relative to the first transparent substrate and the second transparent substrate, the dimming layer is retracted relative to the first bonding layer and the second bonding layer, and the retracted distance is greater than 5 mm; The step of disposing a sealant layer between the first transparent substrate and the second transparent substrate so that the sealant layer fills at least a portion of the retracted area comprises: Disposing a third adhesive layer between the first adhesive layer and the second adhesive layer, so that the third adhesive layer is retracted relative to both the first adhesive layer and the second adhesive layer; Disposing a support member with holes between the first transparent substrate and the second transparent substrate, so that the support member with holes contacts the side edges of the first adhesive layer, the second adhesive layer and the third adhesive layer; Laminating the laminated member provided with the third adhesive layer and the perforated support member; After the lamination is completed, the support member with holes is removed, and the sealant layer is filled in the area where the support member with holes is located.
13. The method for preparing a dimming component according to any one of claims 10 to 12, characterized in that: The maximum width of the sealant layer is 1 mm to 5 mm.
14. The method for preparing a dimming component according to any one of claims 6 to 7 and 9 to 12, characterized in that: The water vapor transmission rate of the sealant layer is ≤10 -3 g / m 2 d; and / or, The sealant layer includes one or more of a polyurethane sealant layer, a butyl sealant layer and a POE sealant layer; Optionally, the sealant layer includes one or more of a butyl sealant layer and a POE sealant layer.
15. A vehicle, characterized in that: The invention comprises the dimming component described in any one of claims 1 to 5 or the dimming component prepared by the preparation method described in any one of claims 6 to 14.
Citation Information
Patent Citations
Rearview mirror
CN110901540A
Liquid crystal display panel and display
CN112445020A
Dimming assembly, preparation method thereof and vehicle
CN114834111A
Dimming assembly, preparation method thereof and vehicle
CN115257116A
Dimming device and dimming device
CN217543619U
Cited By
Dimming assembly and preparation method therefor, and vehicle
WO2026032395A1
Dimming assembly, manufacturing method therefor and use thereof
WO2026097404A1
Light-regulating assembly, preparation method therefor, and use thereof
WO2026097809A1