Device and method for efficiently preparing hydrogel-based composite material under driving of electric field
The electric field driving method is used to process hydrogels and charged particles in the reaction tank, which solves the problems of long compounding time and unevenness in the preparation of bacterial nanocellulose composites, and achieves efficient and uniform preparation of hydrogel-based composites. , suitable for composites of multiple materials, and has industrial application prospects.
Patent Information
- Application Number
- CN202410829353.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, the preparation method of bacterial nanocellulose composite materials has problems such as long compounding time, small processing capacity, and poor uniformity. In particular, the impregnation adsorption method has a long compounding time and is uneven, and the chemical cross-linking method may introduce toxicity. substance.
Hydrogel-based composite materials are prepared using an electric field driving method. By setting a positive electrode and a negative electrode in a reaction tank, a DC power supply is used to process the hydrogel and charged particles under an electric field to form an efficient three-dimensional network structure composite material.
It achieves the preparation of hydrogel-based composite materials with short compounding time, large processing capacity, and good uniformity. The material contact surface is large and the load capacity is large. It is suitable for the compounding of various hydrogel matrix materials and has industrial prospects.
Smart Images

Figure CN118846196A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of composite material preparation, and particularly relates to a device and method for efficiently preparing a hydrogel-based composite material by electric field driving. Background Art
[0002] The selection of hemostatic materials is crucial for dealing with post-traumatic bleeding. The non-adjustable shape of traditional hemostatic gauze and gelatin sponge makes them unsuitable for irregularly shaped and incompressible bleeding wounds, while hemostatic powder cannot form a stable scab on the wound surface. Therefore, it is urgent to develop a new type of hemostatic material to deal with traumatic bleeding. Bacterial nanocellulose can be used to prepare hemostatic materials because of its three-dimensional network structure similar to the extracellular matrix and a microenvironment suitable for wound healing. However, due to its single function and limited coagulation effect, bacterial nanocellulose is often compounded with other substances to improve the biological functionality of bacterial nanocellulose.
[0003] There are many strategies for the composite of bacterial nanocellulose composites, but there are also many shortcomings, such as the impregnation adsorption method often takes a long time to composite and the composite is uneven, and the chemical cross-linking method may introduce toxic substances. Therefore, it is necessary to develop a preparation method with large processing volume and short composite time. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a device and method for efficiently preparing hydrogel-based composite materials by electric field drive, which effectively solves the problems of long composite time, small processing volume and poor uniformity of conventional impregnation adsorption method.
[0005] The present invention provides an electric field driven device for efficiently preparing a hydrogel-based composite material, comprising a reaction tank; positive terminal empty slots and negative terminal empty slots are arranged on both sides of the reaction tank; a plurality of vertically placed clamping plates are arranged in the reaction tank; the direct current power supply is connected to the positive terminal empty slot via a positive electrode rod, and is connected to the negative terminal empty slot via a negative electrode rod; and a cover plate is placed above the reaction tank.
[0006] Preferably, the hydrogel is a hydrophilic, water-soluble or water-swellable natural polymer, synthetic polymer or a polymer material in which a natural polymer and a synthetic polymer are hybridized to form a three-dimensional network structure through cross-linking, or an inorganic material hydrogel, or a hydrogel doped with an inorganic material and an organic material.
[0007] Preferably, the natural polymer is one or more of polysaccharide polymers, polypeptide polymers, and nucleic acid hydrogels; the synthetic polymer is one or more of polymer polymers of alcohol, acrylic acid or its derivatives, silica gel, and hydrophilic organic glass.
[0008] Most preferably, the hydrogel is a bacterial nanocellulose membrane.
[0009] Preferably, the clamping plate is connected to or not connected to the side walls of the positive terminal slot and the negative terminal slot.
[0010] Preferably, the splint is detachable.
[0011] Preferably, the splint is of snap-fit type, screw type or clip type.
[0012] Preferably, the reaction tank is further provided with a cooling device, and the cooling device is coil cooling, jacket cooling or plywood cooling.
[0013] The present invention also provides a method for efficiently preparing a hydrogel-based composite material by electric field driving, comprising the following steps:
[0014] Using the above device, the hydrogel is immersed in a conductive solution, and then the hydrogel is cut into the size of a splint and placed vertically in the splint. The conductive solution or charged particle solution is then injected into the positive terminal empty slot and the negative terminal empty slot on both sides of the reaction tank. The cover is closed, and a DC power supply is turned on to prepare a hydrogel-based composite material under the drive of an electric field.
[0015] Preferably, the conductive solution is one or more of acetic acid-sodium acetate buffer, phosphate buffer solution PBS, and citric acid-sodium citrate buffer.
[0016] Preferably, the charged particles are one or more of polyelectrolytes, polyethyleneimine hydrochloride, polyvinyl pyridine, polyvinyl amine, chitosan or its derivatives, proteins, collagen, gelatin, polypeptides, polyamino acids, nucleotides, DNA, RNA, carboxylic acid pyridine copolymers, carboxymethyl chitosan, hyaluronic acid, and sodium polyacrylate.
[0017] Preferably, the charged particles are injected into the same electrode end slot according to their charge properties.
[0018] Preferably, when the charged particles are multi-component, charged particles with the same charge are mixed and injected into the same electrode end slot.
[0019] Furthermore, when bacterial nanocellulose aerogel and sponge need to be prepared, they can be obtained by using traditional freeze-drying technology and processes.
[0020] Beneficial Effects
[0021] (1) Compared with the conventional impregnation adsorption method, the present invention has the advantages of short recombination time, large processing volume and good uniformity.
[0022] (2) Compared with the composite material driven by the horizontal electric field, the present invention has the advantages of large material contact surface, large load capacity and good industrialization prospect.
[0023] (3) The device and preparation method of the present invention can be used for the composite of various hydrogel matrix materials and have universal applicability. At the same time, due to its unique vertical processing method, it can process multiple materials at a time, with a large processing volume, and the number of splints in the device can be increased or decreased arbitrarily according to the size of the processing volume. It is easy to operate and has broad prospects for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is a side view of the device of the present invention;
[0025] Figure 2 It is a front view of the device of the present invention;
[0026] Figure 3 It is a top view of the device of the present invention.
[0027] Figure 4 This is a diagram of the snap-fitting splint components of the device of the present invention.
[0028] Figure 5 It is a diagram of the screw-type clamping plate component of the device of the present invention.
[0029] Figure 6 This is a diagram of the clip-type clamping plate component of the device of the present invention.
[0030] Figure 7 This is a three-view drawing of the coil cooling device of the present invention.
[0031] Figure 8 This is a three-view drawing of the jacket cooling of the device of the present invention.
[0032] Fig. 9 Three views of the cooling plate of the device of the present invention.
[0033] Fig.10 The SEM micrographs are of the bacterial cellulose / collagen composite film of Example 1, the bacterial cellulose / collagen / chitosan composite film of Example 2, the bacterial cellulose of Comparative Example 1, and the bacterial cellulose / collagen / chitosan composite film of Comparative Example 2. Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0034] Fig.11 The mechanical properties of the bacterial cellulose / collagen composite film of Example 1, the bacterial cellulose / collagen / chitosan composite film of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite film of Comparative Example 2 are shown in the figure, including stress-strain curve (A), maximum breaking force (B), Young's modulus (C) and elongation at break (D). Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0035] Fig.12 The water control performance results of the bacterial cellulose / collagen composite membrane of Example 1, the bacterial cellulose / collagen / chitosan composite membrane of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite membrane of Comparative Example 2 are shown, including the water content (A) and the water absorption rate (B). Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0036] Fig.13 The blood test results of the bacterial cellulose / collagen composite film of Example 1, the bacterial cellulose / collagen / chitosan composite film of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite film of Comparative Example 2 are shown, including the hemolysis rate (A) and the whole blood coagulation curve (B). Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0037] Fig.14 The antibacterial effect results of the bacterial cellulose / collagen composite film of Example 1, the bacterial cellulose / collagen / chitosan composite film of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite film of Comparative Example 2 are shown. Including the Escherichia coli inhibition zone (A), the Staphylococcus aureus inhibition zone (B), the Escherichia coli inhibition rate (C) and the Staphylococcus aureus inhibition rate (D). Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0038] Fig.15 The cell experiment results of the bacterial cellulose / collagen composite film of Example 1, the bacterial cellulose / collagen / chitosan composite film of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite film of Comparative Example 2 are shown. Including the cell fluorescence staining results (A), the CCK-8 value of the direct contact method (B) and the cytotoxicity of the 100% extract method (C). Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2.
[0039] Fig.16The graphs show the hemostasis results of the bacterial cellulose / collagen composite membrane of Example 1, the bacterial cellulose / collagen / chitosan composite membrane of Example 2, the bacterial cellulose of Comparative Example 1 and the bacterial cellulose / collagen / chitosan composite membrane of Comparative Example 2 in rats. Including the hemostasis time (A) of the rat liver trauma model, the blood loss (B) of the rat liver trauma model, the hemostasis time (C) of the rat tail amputation model and the blood loss (D) of the rat tail amputation model. Among them, BNC: Comparative Example 1; E-BNC / COL: Example 1; E-BNC / COL / CS: Example 2; S-BNC / COL / CS: Comparative Example 2. DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0041] like Figure 1-Figure 3 As shown, a device for efficiently preparing hydrogel-based composite materials driven by electric field is provided, including a reaction tank 7; positive terminal empty slots 5 and negative terminal empty slots 6 are provided on both sides of the reaction tank 7; a plurality of vertically placed clamping plates 4 are provided in the reaction tank 7; the DC power supply 1 is connected to the positive terminal empty slot 5 through the positive terminal electrode rod 2, and is connected to the negative terminal empty slot 6 through the negative terminal electrode rod 3; and a cover plate 8 is placed above the reaction tank 7.
[0042] Preferably, the clamping plate 4 is connected to or not connected to the side walls of the positive terminal slot 5 and the negative terminal slot 6 .
[0043] Preferably, the clamping plate 4 is detachable.
[0044] Preferably, Figure 4-Figure 6 As shown, the splint 4 is of a snap-fit type, a screw type or a clip type. The snap-fit type splint buckles the hydrogel in the splint by means of a snap-fit key; the screw type splint fixes the hydrogel in the splint by means of screws; the clip type splint squeezes the hydrogel in the splint by force.
[0045] Preferably, Figure 7-Figure 9 As shown, the reaction tank 7 is also provided with a cooling device, which is coil cooling, jacket cooling or splint cooling. Coil cooling is embedded in the wall of the reaction tank 7, and the coil is cooled by entering and exiting from the bottom; jacket cooling is to wrap a jacket around the outer periphery of the reaction tank 7, and cool by entering and exiting from the bottom; splint cooling is to cool by a cooling pipe in the shape of a splint.
[0046] Example 1
[0047] (1) After Acetobacter xylinum was cultured in a liquid medium at 30°C for 3 days, the membrane was repeatedly purified in a 1% (w / v) sodium hydroxide solution, rinsed with deionized water, and sterilized by high pressure to obtain a bacterial cellulose membrane.
[0048] (2) Take the purified bacterial cellulose hydrogel, cut it into 3×3 cm pieces, and immerse it in 0.4 M acetic acid-sodium acetate buffer for 1 h.
[0049] (3) Dissolve 0.5 g collagen in 0.4 M acetic acid-sodium acetate solution at pH 5.5 to obtain a 0.5 mg / mL collagen solution.
[0050] (4) The bacterial cellulose membrane obtained in step (1) is vertically placed in the clamping plate 4 of the reaction tank 7, and 60 mL of the collagen solution is injected into the negative terminal empty tank 6.
[0051] (5) Cover the cover plate 8, set the voltage to 20 V, take out the bacterial cellulose hydrogel after treating for 3 min, and wash it with PBS three times to obtain the bacterial cellulose / collagen composite hydrogel.
[0052] Example 2
[0053] (1) After Acetobacter xylinum was cultured in a liquid medium at 30°C for 3 days, the membrane was repeatedly purified in a 1% (w / v) sodium hydroxide solution, rinsed with deionized water, and sterilized by high pressure to obtain a bacterial cellulose membrane.
[0054] (2) Take the purified bacterial cellulose hydrogel, cut it into 3×3 cm pieces, and immerse it in 0.4 M acetic acid-sodium acetate buffer for 1 h.
[0055] (3) Dissolve 0.5 g collagen in a 0.4 M acetic acid-sodium acetate solution at pH 5.5 to obtain a 0.5 mg / mL collagen solution. Dissolve 0.5 g chitosan in a 0.4 M acetic acid-sodium acetate solution at pH 5.5 to obtain a 0.5 mg / mL chitosan solution. (4) Place the bacterial cellulose membrane obtained in step (1) vertically in the clamping plate 4 of the reaction tank 7, take 60 mL of the collagen solution and inject it into the negative terminal empty slot 6, and then take 60 mL of the chitosan solution and inject it into the positive terminal empty slot 5.
[0056] (5) Cover the cover plate 8, set the voltage to 20 V, take out the bacterial cellulose hydrogel after treating for 3 min, and wash it with PBS three times to obtain the bacterial cellulose / collagen / chitosan composite hydrogel.
[0057] Example 3
[0058] (1) A 10% PVA hydrogel solution was prepared and repeatedly frozen and thawed at -20°C to obtain a PVA hydrogel film.
[0059] (2) The PVA hydrogel film was cut into 3×3 cm pieces and immersed in 0.4 M phosphate buffer for 1 h. HA was dissolved in 0.4 M phosphate buffer to prepare a 2% HA solution.
[0060] (3) The PVA hydrogel film obtained in step (1) is vertically placed in the clamping plate 4 of the reaction tank 7, and the prepared HA solution is injected into the negative terminal empty tank 6.
[0061] (4) Cover the cover plate 8, set the voltage to 20 V, take out the PVA hydrogel film after treating for 3 min, and wash it with PBS three times to obtain the PVA / HA composite hydrogel.
[0062] Comparative Example 1
[0063] After Acetobacter xylinum was cultured in a liquid medium at 30°C for 3 days, the membrane was repeatedly purified in a 1% (w / v) sodium hydroxide solution, rinsed with deionized water, and sterilized by high pressure to obtain a bacterial cellulose membrane.
[0064] Comparative Example 2
[0065] (1) After Acetobacter xylinum was cultured in a liquid medium at 30°C for 3 days, the membrane was repeatedly purified in a 1% (w / v) sodium hydroxide solution, rinsed with deionized water, and sterilized by high pressure to obtain a bacterial cellulose membrane.
[0066] (2) Dissolve 0.5 g collagen in a pH 5.5, 0.4 M acetic acid-sodium acetate solution to obtain a 0.5 mg / mL collagen solution. Dissolve 0.5 g chitosan in a pH 5.5, 0.4 M acetic acid-sodium acetate solution to obtain a 0.5 mg / mL chitosan solution. (3) Take the purified bacterial cellulose hydrogel, cut it into 3×3 cm, and place it in 100 mL of 5 mg / mL COL solution and CS solution, and stir at 100 rpm for 24 hours at room temperature to obtain bacterial nanocellulose / collagen / chitosan composite hydrogel.
[0067] Depend on Fig.10 It can be seen that the comparative example 1 has a three-dimensional irregular network structure, while the polymer is stably attached to the surface and inside of the BNC fiber network in Examples 1 and 2. In contrast, the polymer material in comparative example 2 is only attached to the surface of the BNC nanonetwork, and there is almost no CS and COL inside. This is because the polymer material is unevenly distributed on the surface of the BNC membrane using the impregnation adsorption method and blocks the porous structure of the BNC membrane.
[0068] Depend on Fig.11It can be seen that after COL is introduced into the BNC three-dimensional network by the electric field driving method, the tensile properties of E-BNC / COL are relatively improved, because the addition of COL can adhere to the BNC network and increase the binding force between BNC fibers. On this basis, the Young's modulus and tensile strength of the BNC composite hydrogel are further improved after the introduction of CS. However, there is no significant difference in the elongation at break, because the composite hydrogels prepared by the electric field driving method and the immersion method do not destroy the natural structure of BNC, ensuring that the good mechanical properties of BNC are fully retained, so there is no significant effect on the elongation at break of the BNC hydrogel.
[0069] Depend on Fig.12 It can be seen that the moisture content of the four membranes is higher than 90%, and the water absorption rate is higher than 50%, which means that they have good liquid absorption performance and can quickly and effectively absorb a large amount of wound exudate in a short time. Not only can they keep the wound surface clean, but they can also create a moist environment around the wound in the later stage to facilitate wound healing.
[0070] Depend on Fig.13 It can be seen that the hemolysis rates of Comparative Example 1, Comparative Example 2, Example 1 and Example 2 are all lower than 1.5%, which are insoluble materials. The absorbance values of the four hydrogels gradually decrease with time after contact with blood. The order of procoagulant effect is E-BNC / COL / CS>S-BNC / COL / CS>E-BNC / COL>BNC. At 5 minutes, the absorbance values of BNC, E-BNC / COL, E-BNC / COL / CS, and S-BNC / COL / CS were 1.59, 1.25, 0.53, and 0.73, respectively, indicating that a large amount of blood has been coagulated on the surface of the E-BNC / COL / CS hydrogel at this time, and the procoagulant effect is the best among the four samples, while the coagulation effect on the surface of the BNC hydrogel is poor. This is because the combined hemostatic effect of collagen and chitosan makes E-BNC / COL / CS and S-BNC / COL / CS show better procoagulant properties than E-BNC / COL, and the procoagulant property of E-BNC / COL / CS is the best.
[0071] Depend on Fig.14 It can be seen that no antibacterial zone appears around Comparative Example 1 and Example 1. After adding chitosan, Example 2 and Comparative Example 2 show good antibacterial performance. This is because the interaction between the positive charge carried by the CS molecule and the negative charge carried by the microbial cell membrane causes CS to adsorb on the surface of the bacterial cell and destroy its structure. The bacterial activity of Escherichia coli in Example 2 is 13.9% and the bacterial activity of Staphylococcus aureus is only 6.4%, while the bacterial activity of Escherichia coli in Comparative Example 2 is 24% and the bacterial activity of Staphylococcus aureus is 17%, which shows that the overall antibacterial performance of Example 2 is better.
[0072] Depend on Fig.15It can be seen that Comparative Example 1, Comparative Example 2, Example 1 and Example 2 did not produce cytotoxicity, and the fluorescent staining diagram showed that each material could promote cell proliferation, and Example 1 showed better cell compatibility.
[0073] Depend on Fig.16 It can be seen that compared with Comparative Example 1, the hemostasis time of the liver trauma model of Example 1 is reduced from 212s to 170s, and the blood loss is reduced from 329mg to 305mg. The hemostasis time of the tail-broken trauma model is reduced from 180s to 158s, and the blood loss is reduced from 462.9mg to 300mg, while the hemostasis time of the liver trauma of Example 2 and Comparative Example 2 is reduced to 126s and 147s, respectively, and the blood loss is reduced to 186mg and 217mg, respectively, and the hemostasis time of the tail-broken trauma model is 113s and 140s, respectively, and the blood loss is 165mg and 180.8mg, respectively. The hemostasis time and blood loss of the liver trauma model and the tail-broken trauma model show the same trend. In summary, Example 2 has better hemostatic performance than Comparative Example 2 because the electric field driven composite method can compound more polymer substances compared to the conventional immersion adsorption method, so there are more effective molecules that can act on the wound, and the hemostatic effect is better.
[0074] It can be seen from the above results that the present invention has the advantages of large material loading, short time consumption, high uniformity, etc., and the effect is obviously better than the conventional immersion adsorption method and the horizontal electric field driving method.
Claims
1. A device for efficiently preparing hydrogel-based composite materials driven by electric field, Features: The invention comprises a reaction tank (7); a positive terminal empty slot (5) and a negative terminal empty slot (6) are arranged on both sides of the reaction tank (7); a plurality of vertically placed clamping plates (4) are arranged in the reaction tank (7); the direct current power source (1) is connected to the positive terminal empty slot (5) through a positive terminal electrode rod (2), and is connected to the negative terminal empty slot (6) through a negative terminal electrode rod (3); and a cover plate (8) is placed above the reaction tank (7).
2. The device according to claim 1, Features: The hydrogel is a hydrophilic, water-soluble or water-swellable natural polymer, synthetic polymer or a polymer material formed by cross-linking a natural polymer and a synthetic polymer to form a three-dimensional network structure, or an inorganic material hydrogel, or a hydrogel doped with an inorganic material and an organic material.
3. The method according to claim 2, Features: The natural polymer is one or more of polysaccharide polymer, polypeptide polymer, and nucleic acid hydrogel; the synthetic polymer is one or more of polymer polymer of alcohol, acrylic acid or its derivatives, silica gel, and hydrophilic organic glass.
4. The device according to claim 1, Features: The hydrogel is a bacterial nanocellulose membrane.
5. The device according to claim 1, Features: The clamping plate (4) is connected or not connected to the side walls of the positive terminal slot (5) and the negative terminal slot (6).
6. The device according to claim 1, Features: The clamping plate (4) is detachable.
7. The device according to claim 1, Features: The clamping plate (4) is of a snap-fit type, a screw type or a clip type.
8. The device according to claim 1, Features: The reaction tank (7) is also provided with a cooling device, which is coil cooling, jacket cooling or clamp plate cooling.
9. A method for efficiently preparing a hydrogel-based composite material by electric field driving, comprising the following steps: Using the device as described in claim 1, the hydrogel is immersed in a conductive solution, and then the hydrogel is cut into the size of a clamp (4) and placed vertically in the clamp (4), and then the conductive solution or charged particle solution is injected into the positive terminal empty slot (5) and the negative terminal empty slot (6) on both sides of the reaction tank, and the cover plate (8) is covered, and the DC power supply (1) is turned on to prepare the hydrogel-based composite material under the drive of the electric field.
10. The method according to claim 9, Features: The conductive solution is one or more of acetic acid-sodium acetate buffer, phosphate buffer solution PBS, and citric acid-sodium citrate buffer.
11. The method according to claim 9, Features: The charged particles are one or more of polyelectrolytes, polyethyleneimine hydrochloride, polyvinyl pyridine, polyvinyl amine, chitosan or its derivatives, proteins, collagen, gelatin, polypeptides, polyamino acids, nucleotides, DNA, RNA, carboxylic acid pyridine copolymers, carboxymethyl chitosan, hyaluronic acid, and sodium polyacrylate.
12. The method according to claim 9, Features: The charged particles are injected into the same electrode end slot according to their charge properties.