Refining agent for improving corrosion resistance and mechanical property of aluminum-copper alloy and application

By using refining agents prepared from raw materials such as MgCl2, KCl, YCl3, K2TiF6 and K2ZrF6, the existing aluminum alloy refining agent problems of large unit dosage, low purification efficiency and single function are solved, and the corrosion resistance and mechanics of aluminum-copper alloys are significantly improved. performance and achieves effective removal of oxides and impurities.

CN118854075APending Publication Date: 2024-10-29KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410905370.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing aluminum alloy refining agent has a large unit dosage, low purification efficiency, contains toxic odor components, and has a single function. It is difficult to effectively remove impurity elements such as Fe and Si, which affects the corrosion resistance and mechanical properties of the aluminum alloy.

Method used

The refining agent is formulated with raw materials such as MgCl2, KCl, YCl3, K2TiF6 and K2ZrF6. It is melted and stirred to form a molten salt. It is cooled into blocks and then broken into appropriate particle sizes. It is used in the smelting of aluminum and copper alloys to promote the removal of oxides and impurities. Separation and removal.

Benefits of technology

Significantly improves the tensile strength and elongation of aluminum-copper alloys, reduces intergranular corrosion depth, removes pores above 5 μm, enhances the corrosion resistance of aluminum alloys, and reduces the generation of pungent odors and smoke.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854075A_ABST
    Figure CN118854075A_ABST
Patent Text Reader

Abstract

The invention discloses a refining agent for improving corrosion resistance and mechanical properties of an aluminum-copper alloy and application, and belongs to the technical field of aluminum alloy smelting auxiliaries. The refining agent comprises the following raw materials in parts by weight: 10-20 parts of MgCl2, 20-30 parts of KCl, 35-15 parts of YCl, 5-20 parts of K2TiF6 and 5-20 parts of K2ZrF6, and the refining agent is obtained by mixing and drying the raw materials of the refining agent, then melting and preserving heat, finally cooling and solidifying, crushing and sieving. When the refining agent is in contact with the aluminum ash slag, the inclusions are separated from the molten aluminum through the comprehensive effects of dissolution, adsorption, chemical combination and the like on the inclusions, and through the good slag-aluminum separation effect, no pungent smell exists, and less smoke is generated. In addition, when the refining agent disclosed by the invention is used for refining the cast aluminum-copper alloy, on one hand, pores of more than 5 microns in the alloy are completely removed; on the other hand, the mechanical property and corrosion resistance of the aluminum alloy are greatly improved, and the tensile strength is improved by 10%; the ductility is improved by 495%; and the intergranular corrosion depth is reduced to 152 microns after refining from 182 microns after refining.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy smelting additives, and specifically relates to a refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloys and its application. Background Art

[0002] During the refining and transportation of molten metal, foreign matter such as oxide scale, intermetallic compounds, and furnace debris are easily brought into the molten metal to form non-metallic inclusions. These non-metallic inclusions are mainly oxide inclusions. According to the different formation periods during the melting and casting process, they can be divided into primary oxide inclusions and secondary oxide inclusions.

[0003] Primary oxide inclusions mainly refer to all oxide inclusions formed before aluminum liquid is poured. Primary oxide inclusions can be divided into two categories according to their shapes: the first type of oxides are large inclusions that are unevenly distributed in the macroscopic structure. Such inclusions make the alloy structure discontinuous, reduce the airtightness of the workpiece, become the source of corrosion, significantly reduce the strength and plasticity of the aluminum alloy, and often become the source of cracks in parts. The second type of oxide inclusions refers to small, dispersed inclusions that cannot be completely removed even after careful purification, which increases the viscosity of the molten metal, reduces the shrinkage compensation ability of the aluminum liquid during solidification, and easily causes shrinkage of the casting.

[0004] Secondary oxide inclusions, also known as endogenous inclusions, are mainly formed during the pouring process. Endogenous inclusions are generally evenly distributed and have relatively small particles. The splashing and turbulence of aluminum liquid during the pouring process are the main sources of secondary oxide inclusions. In the sand mold, aluminum liquid reacts with the water in the sand and decomposes into oxygen and hydrogen through water. Oxygen reacts with aluminum to form oxide inclusions, and hydrogen dissolves in the aluminum liquid.

[0005] If the unpurified aluminum liquid is used to produce castings directly, the gas dissolved in the aluminum liquid will float up as the solubility decreases during the solidification process. In addition, the oxide inclusions inside the casting will cause casting defects such as pores and cracks, which will seriously affect the quality of the casting and even make the product scrapped. Therefore, it is necessary to purify the aluminum and aluminum alloy melt to remove the gas, metal oxides, non-metallic inclusions and other harmful elements in it, purify the alloy melt, and thus improve the quality of the alloy.

[0006] Refining agent purification method is a commonly used melt purification method in the production of aluminum and aluminum alloys. It is widely used in actual production due to its advantages of easy operation and good purification effect. Refining agent plays an important role in the purification of aluminum alloy melts. The quality of refining agent is related to the improvement of aluminum alloy quality and performance. At present, there are no performance index requirements for refining agents, and no unified evaluation standards have been formed. The quality of refining agents on the market is uneven, and the prices are also quite different, which has affected the promotion and use of refining agents to a certain extent.

[0007] At present, the disclosed refining agent products generally contain one or more of sodium salts such as sodium chloride, sodium fluoroaluminate, sodium fluorosilicate, sodium fluoride, etc. For example, Chinese invention patent application CN101343699A discloses an aluminum silicon alloy refining agent, which is mainly composed of potassium chloride, sodium chloride, zinc chloride, sodium fluoroaluminate, sodium fluorosilicate, sodium nitrate, graphite powder, charcoal powder, hexachloroethane, sodium fluoroborate, potassium fluorotitanate, and is suitable for casting aluminum silicon alloys. Chinese invention patent application CN101423910A discloses a refining agent for aluminum and low-magnesium aluminum alloys, which is mainly composed of sodium chloride, sodium sulfate, calcium fluoride, potassium chloride, magnesium chloride, sodium fluorosilicate, and is suitable for refining aluminum alloys with aluminum and magnesium content less than 2%. Chinese invention patent application CN101967565A discloses a refining agent for aluminum and aluminum alloys, which is mainly composed of sodium chloride, sodium fluorosilicate, sodium sulfate, calcium fluoride, and hexachloroethane. The refining agent may also include one or more of calcium magnesium carbonate, sodium fluoroaluminate, sodium thiosulfate, and sodium fluoride. The refining agent does not contain potassium salts and has little corrosion to the electrolytic cell. The aluminum ash produced after refining aluminum and aluminum alloys with the refining agent can be recycled back to the electrolytic cell. Chinese invention patent application CN201810331113.8 discloses a refining agent, preparation method, and refining process for aluminum alloys, which is mainly composed of potassium chloride, sodium chloride, sodium tetrachloroaluminate, sodium sulfate, sodium fluorosilicate, and a promoter. The promoter can promote the decomposition of sodium tetrachloroaluminate in the refining agent, and at the same time, reduce the interfacial tension between the refining agent and the oxidized inclusions, so that the oxidized inclusions can float smoothly on the liquid surface and then be removed, thereby improving the product quality.

[0008] The currently disclosed patents have one or more of the following defects: ① The unit dosage is large, generally above 2-3‰, and the purification efficiency is low. ② It contains toxic and unpleasant hexachloroethane, which is harmful to human health and the environment. ③ Hexachloroethane, sodium sulfate and other ingredients release irritating gases such as chlorine and sulfur dioxide during use, polluting the environment. ④ The function is single and can only remove oxidized inclusions, and the removal ability of impurity elements such as Fe and Si is insufficient. Summary of the invention

[0009] In view of the above-mentioned shortcomings of the prior art, the present invention proposes a refining agent and application for improving the corrosion resistance and mechanical properties of aluminum-copper alloy.

[0010] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy, comprising the following raw materials in parts by weight: 10-20 parts of MgCl2, 20-30 parts of KCl, 35-15 parts of YCl, 5-20 parts of K2TiF6, and 5-20 parts of K2ZrF6.

[0011] The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy comprises the following steps:

[0012] (1) The raw materials of the refining agent are fully mixed, and then dried until the moisture content of the materials is ≤ 0.05%; finally, they are melted and stirred at a temperature-insulated state to obtain molten salt;

[0013] (2) pouring the molten salt into a mold to cool and solidify into a block flux;

[0014] (3) crushing and sieving the bulk flux into particles with an average particle size of 0.10 to 0.40 cm;

[0015] (4) The sieved particles are sealed and packaged with aluminum foil to obtain a finished product, thereby obtaining a refining agent.

[0016] As a preferred embodiment of the present invention, in the step (1), the raw materials of the refining agent are mixed by a mixer, and the mixing time is 20-40 minutes.

[0017] As a preferred embodiment of the present invention, the drying temperature is 200°C.

[0018] As a preferred embodiment of the present invention, the melting temperature is 700-900°C.

[0019] The present invention also claims to protect the use of the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy in the smelting of aluminum-copper alloy.

[0020] The aluminum-copper alloy is any aluminum-copper alloy.

[0021] As a preferred embodiment of the present invention, the application includes the following steps: heating the cast aluminum-copper alloy to 720°C and keeping it warm for melting; then heating it to 760°C, adding a refining agent that improves the corrosion resistance and mechanical properties of the aluminum-copper alloy, stirring for 3-5 minutes, standing and cooling to 720°C, keeping it warm at 720°C for 20 minutes, and then performing slag removal and pouring to obtain an aluminum alloy ingot.

[0022] As a preferred embodiment of the present invention, the mass of the refining agent for improving the corrosion resistance and mechanical properties of the aluminum-copper alloy is 1.3% of the mass of the cast aluminum-copper alloy.

[0023] The refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy is used in the smelting process of casting aluminum-copper alloy. The beneficial chemical reaction formula is as follows:

[0024] 3K2TiF6+4Al=4AlF3+6KF+3Ti

[0025] Ti+Al=Al3Ti

[0026] 3K2ZrF6+4Al=4AlF3+6KF+3Zr

[0027] 2Zr+Al2O3=2Al+Zr2O3

[0028] [Zr] + 2[H] = [ZrH2]

[0029] The AlF3 produced by the above reaction is a gas that can generate bubbles, stir the aluminum alloy melt, and thus bring out inclusions, oxides and gases in the aluminum alloy melt, thereby achieving a refining effect on the aluminum alloy melt.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] (1) When the refining agent of the present invention contacts aluminum ash slag, the inclusions are separated from the aluminum liquid through the comprehensive effects of dissolution, adsorption, and combination of the inclusions, and the inclusions sink to the bottom of the crucible for removal. Due to the good slag-aluminum separation effect, there is no irritating odor and less smoke is generated.

[0032] (2) The refining agent of the present invention is used in the refining of cast aluminum-copper alloy. On the one hand, the pores larger than 5 microns in the refined aluminum and aluminum alloy are almost completely removed. On the other hand, the mechanical properties and corrosion resistance of the aluminum alloy are greatly improved, among which the tensile strength is increased from 300Mpa of unrefined to 330Mpa, and the tensile strength is increased by 10%; the elongation is increased from 4.4% of unrefined to 26.2% of refined, and the elongation is increased by 495%; the intergranular corrosion depth is reduced from 182 microns of unrefined to 152 microns of refined. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the pore distribution diagram of aluminum-copper alloy refined without adding refining agent.

[0034] Figure 2 This is the pore distribution diagram of the aluminum-copper alloy refined by adding the refining agent in Example 1.

[0035] Figure 3 1 is a stress-strain curve diagram of the aluminum-copper alloy after refining without adding a refining agent and a stress-strain curve diagram of the aluminum-copper alloy after refining with adding a refining agent in Example 1.

[0037] Figure 4 a is the cross-sectional view of intergranular corrosion of aluminum-copper alloy after refining without adding refining agent.

[0038] Figure 4 b is a cross-sectional view of intergranular corrosion of the aluminum-copper alloy after refining with the addition of a refining agent in Example 1.

[0039] Figure 5 a is the morphology of the Al3Y phase in the aluminum-copper alloy after refining with the addition of refining agent in Example 1.

[0040] Figure 5 b is the diffraction spot pattern of the Al3Y phase in the aluminum-copper alloy after refining with the refining agent in Example 1.

[0041] Figure 6 a is the morphology of the Al3Ti phase in the aluminum-copper alloy after refining with the addition of refining agent in Example 1.

[0042] Figure 6 b is the diffraction spot pattern of the Al3Ti phase in the aluminum-copper alloy after refining with the refining agent in Example 1. DETAILED DESCRIPTION

[0043] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0044] Example 1

[0045] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, YCl3, K2TiF6 and K2ZrF6, and the raw material ratios meet the following requirements: 15 parts of MgCl2, 25 parts of KCl, 10 parts of YCl3, 12 parts of K2TiF6, and 15 parts of K2ZrF6, and all the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0046] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0047] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 800° C. and stirred to obtain a uniform molten salt;

[0048] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0049] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0050] (5) Finally, the particles with qualified particle size are sealed and packaged with aluminum foil to form a refining agent.

[0051] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0052] (7) After complete melting, the temperature is raised to 760° C., and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720° C. After being kept at 720° C. for 20 minutes, slag removal and pouring are performed to obtain an aluminum-copper alloy.

[0053] Figure 1 , 2 These are the industrial CT pore distribution diagrams of the ingot samples before and after refining. It can be seen from the figure that after refining, the pores larger than 5um in the sample are basically removed and the porosity is greatly reduced. Figure 3 The stress-strain curve of aluminum-copper alloy before and after refining. It can be seen from the figure that the ultimate tensile strength and elongation of the refined sample increased by 10% and 495% respectively; Figure 4 , 5 The intergranular corrosion diagrams before and after refining are shown. It can be seen from the figure that the intergranular corrosion depth is reduced by 30um after refining. This is because the element Zr will inhibit the recrystallization of the alloy and the formation of the non-precipitation zone at the grain boundary, thereby improving the corrosion resistance of the alloy;

[0054] The above refining agent is used for the refining of aluminum-copper alloy, according to Figure 1 and 2 It can be seen that when the refining agent addition amount is 1.3%, the slag aluminum separation effect is good, the ash slag is loose, and the pores larger than 5um in the aluminum-copper alloy are almost removed. Figure 3 It can be seen that compared with the refining without adding refining agent, the tensile strength of the aluminum-copper alloy refined with adding refining agent increased from 300Mpa to 330Mpa after refining, and the tensile strength increased by 10%; the elongation increased from 4.4% to 26.2%, and the elongation increased by 495%. Figure 4-5 It can be seen that the intergranular corrosion depth is reduced from 182um without refining agent to 152um after refining agent. And the impurity elements Fe and Si are reduced from 407.00mg / Kg and 0.51mg / Kg without refining agent to 371.22mg / Kg and 0.18mg / Kg respectively. Figure 5 , 6 It can be seen that Al3Y is pinned at the grain boundary, thereby hindering dislocation movement and improving mechanical properties. On the other hand, Al3Ti can serve as the core of α-Al heterogeneous nucleation and refine α-Al grains through peritectic reaction.

[0055] Example 2

[0056] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, YCl3, K2TiF6 and K2ZrF6, and the raw material ratios meet the following requirements: 10 parts of MgCl2, 30 parts of KCl, 35 parts of YCl, 20 parts of K2TiF6, and 20 parts of K2ZrF6, and all the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0057] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0058] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 900° C. and stirred to obtain a uniform molten salt;

[0059] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0060] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0061] (5) Finally, the particles with qualified particle size are sealed and packaged with aluminum foil to form a refining agent.

[0062] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0063] (7) After complete melting, the temperature is raised to 760°C, and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720°C. After being kept at 720°C for 20 minutes, slag removal and pouring are performed to obtain an aluminum alloy ingot.

[0064] The above refining agent is used for the refining of aluminum-copper alloy, and the slag-aluminum separation effect is good, the ash slag is loose, and the pores above 5um in the aluminum-copper alloy are almost removed. Compared with the refining without adding the refining agent, the tensile strength of the aluminum-copper alloy refined with the refining agent is increased from 300Mpa to 318Mpa after refining, and the tensile strength is increased by 6%; the elongation is increased from 4.4% to 24.5%, and the elongation is increased by 456%. The intergranular corrosion depth is reduced from 182um without adding the refining agent to 158um after adding the refining agent. And the impurity elements Fe and Si are significantly reduced compared with the aluminum-copper alloy refined without adding the refining agent.

[0065] Example 3

[0066] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, YCl3, K2TiF6 and K2ZrF6, and the raw material ratios meet the following requirements: 20 parts of MgCl2, 20 parts of KCl, 15 parts of YCl3, 5 parts of K2TiF6, and 5 parts of K2ZrF6, and all the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0067] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0068] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 700° C. and stirred to obtain a uniform molten salt;

[0069] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0070] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0071] (5) Finally, the particles with qualified particle size are sealed and packaged with aluminum foil to form a refining agent.

[0072] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0073] (7) After complete melting, the temperature is raised to 760°C, and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720°C. After being kept at 720°C for 20 minutes, slag removal and pouring are performed to obtain an aluminum alloy ingot.

[0074] The above refining agent is used for the refining of aluminum-copper alloy, and the slag-aluminum separation effect is good, the ash slag is loose, and the pores above 5um in the aluminum-copper alloy are almost removed. Compared with the refining without adding the refining agent, the tensile strength of the aluminum-copper alloy refined with the refining agent is increased from 300Mpa to 323Mpa after refining, and the tensile strength is increased by 7.6%; the elongation is increased from 4.4% to 23.6%, and the elongation is increased by 436%. The intergranular corrosion depth is reduced from 182um without adding the refining agent to 163um after adding the refining agent. And the impurity elements Fe and Si are significantly reduced compared with the aluminum-copper alloy refined without adding the refining agent.

[0075] Comparative Example 1

[0076] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, YCl3 and K2TiF6, and the raw material ratios meet the following requirements: 15 parts of MgCl2, 25 parts of KCl, 10 parts of YCl3, and 12 parts of K2TiF6. All the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0077] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0078] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 800° C. and stirred to obtain a uniform molten salt;

[0079] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0080] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0081] (5) Finally, the particles with qualified particle size are sealed and packaged into refining agent using aluminum foil.

[0082] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0083] (7) After complete melting, the temperature is raised to 760°C, and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720°C. After being kept at 720°C for 20 minutes, slag removal and pouring are performed to obtain an aluminum alloy ingot.

[0084] The above refining agent is used for the refining of aluminum-copper alloy, and the slag-aluminum separation effect is better, the ash slag is loose, and some pores above 5um are not completely removed. Compared with the refining without adding the refining agent, the tensile strength of the aluminum-copper alloy refined with the refining agent is increased from 300Mpa to 320Mpa after refining, and the tensile strength is increased by 6%; the elongation is increased from 4.4% to 23.5%, and the elongation is increased by 434%; but there is no obvious change in the depth of intergranular corrosion.

[0085] Compared with Comparative Example 1, the pores of the aluminum-copper alloy with a diameter of more than 5 μm after refining by adding the refining agent in Examples 1-3 are almost completely removed, and the depth of intergranular corrosion is significantly reduced, mainly because K2ZrF6 reacts with aluminum to form Zr element, which reacts with H in the melt to form rare earth hydride, thereby removing H in the melt and avoiding the formation of multiple and large pores. At the same time, Zr element can inhibit the recrystallization of the alloy, promote the formation of precipitation zones at the grain boundaries, and significantly improve the corrosion resistance of the alloy.

[0086] Comparative Example 2

[0087] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, YCl3 and K2ZrF6, and the raw material ratios meet the following requirements: 15 parts of MgCl2, 25 parts of KCl, 10 parts of YCl3, and 15 parts of K2ZrF6, and all the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0088] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0089] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 800° C. and stirred to obtain a uniform molten salt;

[0090] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0091] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0092] (5) Finally, the particles with qualified particle size are sealed and packaged with aluminum foil to form a refining agent.

[0093] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0094] (7) After complete melting, the temperature is raised to 760°C, and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720°C. After being kept at 720°C for 20 minutes, slag removal and pouring are performed to obtain an aluminum alloy ingot.

[0095] When the above refining agent is used for the refining of aluminum-copper alloy, the slag-aluminum separation effect is better, the ash is loose, and the pores above 5um are basically removed. Compared with the refining without adding the refining agent, the tensile strength of the aluminum-copper alloy refined with the refining agent is basically not improved; the elongation is increased from 4.4% to 25.5%, and the elongation is increased by 479%; the intergranular corrosion depth is reduced from 182um to 165um.

[0096] The comparative example lacks K2TiF6 in the refining agent raw material, resulting in the failure to refine the alloy grains, which results in no improvement in alloy strength compared with refining without adding the refining agent.

[0097] Comparative Example 3

[0098] A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy and a preparation method thereof, characterized in that the raw materials include the following components: MgCl2, KCl, K2TiF6 and K2ZrF6, and the raw material ratios meet the following requirements: 15 parts of MgCl2, 25 parts of KCl, 12 parts of K2TiF6, and 15 parts of K2ZrF6, and all the raw materials meet the following requirements: purity ≥ 98%. The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy with the composition and its application include the following steps:

[0099] (1) Prepare the raw materials according to the above ratio, put the materials into a mixer for mixing, and the mixing time is 20 minutes;

[0100] (2) Then, the mixed material is dried in a dryer at 200° C. for 2 hours, and the moisture content of the refining agent is measured to be 0.03%. Then, the mixed material is melted in a resistance furnace, heated to 800° C. and stirred to obtain a uniform molten salt;

[0101] (3) pouring the obtained molten salt into a mold to cool and solidify into a block flux;

[0102] (4) crushing and sieving the bulk flux into particles with an average particle size of 0.10 cm to 0.40 cm;

[0103] (5) Finally, the particles with qualified particle size are sealed and packaged into refining agent using aluminum foil.

[0104] (6) heating the cast aluminum-copper alloy to 720° C. and melting the alloy;

[0105] (7) After complete melting, the temperature is raised to 760°C, and a refining agent treated in step (5) is added in an amount of 1.3% by mass of the cast aluminum-copper alloy. The mixture is stirred for 3-5 minutes, allowed to stand and cooled to 720°C. After being kept at 720°C for 20 minutes, slag removal and pouring are performed to obtain an aluminum alloy ingot.

[0106] The above refining agent is used for the refining of aluminum-copper alloy, and the slag-aluminum separation effect is better, the ash is loose, and the pores above 5um are basically removed. The tensile strength is increased from 300Mpa to 310Mpa after refining, and the tensile strength is increased by 3%. This is because there is no YCl3 in the refining agent, and no Al3Y phase is generated at the grain boundary, which cannot pin the grain boundary to hinder the dislocation movement, so the mechanical properties have no obvious change. The elongation is increased from 4.4% to 20.5%, and the elongation is increased by 365%; the intergranular corrosion depth is reduced from 182um before refining to 170um after refining.

[0107] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy, characterized in that: The invention comprises the following raw materials in parts by weight: 10-20 parts of MgCl2, 20-30 parts of KCl, 35-15 parts of YCl, 65-20 parts of K2TiF6, and 65-20 parts of K2ZrF6; The method for preparing the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy comprises the following steps: (1) The raw materials of the refining agent are fully mixed, and then dried until the moisture content of the materials is ≤ 0.05%; finally, they are melted and stirred at a temperature-insulated state to obtain molten salt; (2) pouring the molten salt into a mold to cool and solidify into a block flux; (3) crushing and sieving the bulk flux into particles with an average particle size of 0.10 to 0.40 cm; (4) The sieved particles are sealed and packaged with aluminum foil to form a refining agent.

2. The refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy according to claim 1, characterized in that: In the step (1), the raw materials of the refining agent are mixed by a mixer, and the mixing time is 20-40 minutes.

3. The refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy according to claim 1, characterized in that: The drying temperature is 200°C.

4. The refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy according to claim 1, characterized in that: The melting temperature is 700-900°C.

5. Use of the refining agent for improving the corrosion resistance and mechanical properties of aluminum-copper alloy as described in any one of claims 1 to 4 in the smelting of aluminum-copper alloy.

6. The use according to claim 5, characterized in that The method comprises the following steps: heating the cast aluminum-copper alloy to 720°C and melting it; then heating it to 760°C, adding a refining agent for improving the corrosion resistance and mechanical properties of the aluminum-copper alloy, stirring it for 3-5 minutes, standing it and cooling it to 720°C, and after keeping it at 720°C for 20 minutes, performing slag removal and pouring treatment to obtain an aluminum alloy ingot.

7. The use according to claim 6, characterized in that The mass of the refining agent for improving the corrosion resistance and mechanical properties of the aluminum-copper alloy is 1.3% of the mass of the cast aluminum-copper alloy.

Citation Information

Cited By

  • Wear-resistant manganese brass alloy material and processing method thereof

    CN119464830A