Modified lithium-rich manganese-based positive electrode material and preparation method thereof, positive electrode plate, secondary battery and electric device

By using composite coating technology of rutile structural materials and amorphous carbon on lithium-rich manganese-based cathode materials, the problems of poor rate and cycle performance are solved, achieving higher battery performance and lower production costs.

CN118867166APending Publication Date: 2024-10-29NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410845849.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Lithium-rich manganese-based cathode materials have poor performance in rate performance and cycle performance, which limits their practical application in lithium-ion batteries.

Method used

A material with a rutile structure is used as the intermediate layer and amorphous carbon is used as the outer coating layer. The conductivity and structural stability of the material are improved through composite coating technology to form a modified lithium-rich manganese-based cathode material with a porous structure.

Benefits of technology

The cycle performance and rate performance of the modified lithium-rich manganese-based cathode material are significantly improved, the cycle life of the battery is extended, and the synthesis cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867166A_ABST
    Figure CN118867166A_ABST
Patent Text Reader

Abstract

The invention provides a modified lithium-rich manganese-based positive electrode material and a preparation method thereof, a positive electrode plate, a secondary battery and an electric device. The modified lithium-rich manganese-based positive electrode material comprises an inner core, a middle layer and an outer coating layer, wherein the middle layer coats at least part of the surface of the inner core; the outer coating layer coats at least part of the surface of the middle layer; the inner core comprises lithium-rich manganese-based oxide, the middle layer comprises a material with a rutile structure, the outer coating layer comprises amorphous carbon, and the outer coating layer has a pore structure. The material with a rutile structure contained in the middle layer of the modified lithium-rich manganese-based positive electrode material has a special bridge site oxygen atom (Obr) structure, so that the stability of the outer coating layer can be enhanced, permeation corrosion of an electrolyte to the core material is hindered, and meanwhile, the electron conductivity and the lithium ion transmission rate are improved; the porous structure of the outer coating layer can effectively improve the toughness of the material, so that the cracking of the positive electrode material caused by lattice distortion in the circulation process is effectively retarded, and the sustainability of lithium ion deintercalation is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to a modified lithium-rich manganese-based positive electrode material and a preparation method thereof, a positive electrode sheet, a secondary battery and an electrical device. Background Art

[0002] As new energy vehicles are gradually recognized and accepted by consumers, the most widely used cathode materials in the market include lithium iron phosphate, lithium cobalt oxide and ordinary ternary materials in response to the requirements of electric vehicle battery cost, safety and driving range. However, in order to achieve further growth and sustainable development of the market, it is inevitable to develop new lithium-ion battery cathode materials with high capacity, low cost and high safety.

[0003] In addition to high theoretical capacity, lithium-rich manganese-based cathode materials also have the advantages of high tap density, low cost, and high safety performance, and are considered to be the next generation of lithium-ion battery cathode materials. However, the rate performance and cycle performance of lithium-rich manganese-based cathode materials are poor, which seriously hinders their practical application. Summary of the invention

[0004] Based on this, the present application provides a modified lithium-rich manganese-based positive electrode material with excellent rate performance and cycle performance, and a preparation method thereof, a positive electrode plate, a secondary battery and an electrical device.

[0005] The first aspect of the present application provides a modified lithium-rich manganese-based positive electrode material, comprising:

[0006] a core comprising a lithium-rich manganese-based oxide;

[0007] an intermediate layer, coated on at least a portion of the surface of the inner core, wherein the intermediate layer comprises a material having a rutile structure;

[0008] The outer coating layer is coated on at least a portion of the surface of the intermediate layer, wherein the outer coating layer comprises amorphous carbon and has a pore structure.

[0009] In some embodiments, the intermediate layer has at least one of the following features (1)-(3):

[0010] (1) The material having a rutile structure includes one or more of TiO2, RuO2, IrO2 and SnO2;

[0011] (2) The mass of the intermediate layer accounts for 0.05% to 0.15% of the mass of the inner core;

[0012] (3) The intermediate layer further contains one or more doping elements selected from the group consisting of Al, Si, Zn, Zr and La.

[0013] In some embodiments, the pore structure has a pore size of 2 nm to 50 nm.

[0014] In some embodiments, the modified lithium-rich manganese-based positive electrode material has at least one of the following characteristics (1)-(3):

[0015] (1) The chemical formula of the lithium-rich manganese-based oxide is xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element includes one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S;

[0016] Optionally, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7);

[0017] Optionally, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%;

[0018] (2) The modified lithium-rich manganese-based positive electrode material includes secondary particles;

[0019] (3) The median particle size D50 of the modified lithium-rich manganese-based positive electrode material is 2.5 μm-3.5 μm;

[0020] (4) The specific surface area of ​​the modified lithium-rich manganese-based positive electrode material is 0.5 m 2 / g-8m 2 / g;

[0021] (5) The carbon content of the modified lithium-rich manganese-based positive electrode material is 0.1wt-0.4wt%.

[0022] The second aspect of the present application provides a method for preparing the modified lithium-rich manganese-based positive electrode material of the first aspect of the present application, comprising the following steps:

[0023] Performing a first sintering treatment on a mixture of a core and a material having a rutile structure, so as to coat at least a portion of the surface of the core with an intermediate layer, thereby preparing an intermediate;

[0024] preparing a mixed solution containing the intermediate and an organic carbon source, adjusting the pH of the mixed solution with an ammonia solution, separating the solid from the liquid, and drying;

[0025] The solid obtained after drying is subjected to a back-firing treatment to prepare the modified lithium-rich manganese-based positive electrode material;

[0026] Wherein, 500°C<the temperature of the back-firing treatment≤800°C.

[0027] In some embodiments, the organic carbon source comprises one or more of polyacrylic acid, polyimide and polypyrrole; and / or

[0028] The mass of the organic carbon source accounts for 2%-6% of the mass of the inner core, and can be 2-3%;

[0029] In some embodiments, the mass of NH4·H2O contained in the ammonia solution accounts for 2%-6% of the mass of the core, and can be 2-3%; and / or

[0030] The mass percentage concentration of the ammonia solution is 10%-50%; and / or

[0031] The pH of the mixed solution is adjusted to 7-10 using an ammonia solution.

[0032] In some embodiments, the temperature of the back-firing treatment is 600° C.-700° C.; and / or

[0033] The back-burning treatment time is 10h-20h; and / or

[0034] The atmosphere of the back-firing treatment includes nitrogen.

[0035] In some embodiments, the step of preparing a mixed solution containing the intermediate and an organic carbon source comprises:

[0036] The intermediate is mixed with a solvent and stirred, and then an organic carbon source is added to prepare the mixed solution;

[0037] Optionally, the solvent includes one of water and ethanol aqueous solution;

[0038] Optionally, the mass ratio of the solvent to the intermediate is (1-3):1;

[0039] Optionally, the temperature of the solvent is 0°C-10°C;

[0040] Optionally, the mass proportion of ethanol in the ethanol aqueous solution is 95%-99%.

[0041] In some embodiments, the mass of the material having a rutile structure is 0.05%-0.15%, optionally 0.08%-0.1% of the mass of the core; and / or

[0042] The temperature of the first sintering treatment is 400° C.-950° C., and can be 500° C.-800° C.; and / or

[0043] The first sintering treatment time is 18h-30h; and / or

[0044] The mixed material further comprises an additive A, wherein the additive A comprises one or more elements selected from the group consisting of Al, Si, Zn, Zr and La.

[0045] In some embodiments, the method for preparing the inner core comprises:

[0046] After mixing the precursor, the lithium source and the optional additive B, a second sintering treatment is performed to prepare the core; the core comprises a lithium-rich manganese-based oxide with a chemical formula of xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element comprises one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S;

[0047] Optionally, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7);

[0048] Optionally, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%;

[0049] Optionally, the lithium source includes one or more of lithium carbonate, lithium hydroxide and lithium sulfate;

[0050] Optionally, the lithium source comprises lithium carbonate and lithium hydroxide in a molar ratio of (3-5):1;

[0051] Optionally, the lithium source comprises lithium carbonate and lithium sulfate in a molar ratio of ≥5:1;

[0052] Optionally, the temperature of the second sintering treatment is 700°C-1050°C, optionally 700°C-1000°C;

[0053] Optionally, the second sintering treatment time is 10h-28h;

[0054] Optionally, the elements contained in the precursor include Ni and Mn, and the molar ratio of Ni to Mn is 3:(2-7);

[0055] Further optionally, the elements contained in the precursor further include one or more of Na, Sr, Ta, Ga, Sn, Te and Ce;

[0056] Optionally, the elements contained in the additive B include one or more of Mg, Y, Ti, Zr, Nb, Cr, Mo, W, Co, Al, P, Sb, La, F and S.

[0057] The third aspect of the present application provides a positive electrode plate, comprising the modified lithium-rich manganese-based positive electrode material of the first aspect of the present application or the modified lithium-rich manganese-based positive electrode material prepared by the preparation method of the second aspect of the present application.

[0058] The fourth aspect of the present application provides a secondary battery, comprising the positive electrode sheet of the third aspect of the present application.

[0059] A fifth aspect of the present application provides an electrical device, comprising the secondary battery of the fourth aspect of the present application.

[0060] The modified lithium-rich manganese-based positive electrode material provided above, wherein the interlayer contains a material having a rutile structure, and the outer coating layer contains amorphous carbon and has a porous structure; compared with the unmodified lithium-rich manganese-based material, the material having a rutile structure contained in the interlayer of the modified lithium-rich manganese-based positive electrode material of the present application has a special bridging oxygen atom (O br ) structure, which can enhance the stability of the outer coating layer, hinder the penetration and corrosion of the electrolyte to the core material, and at the same time improve the electronic conductivity and lithium ion transmission rate; the pore structure of the outer coating layer can effectively improve the toughness of the material, thereby effectively slowing down the cracking of the positive electrode material caused by lattice distortion during the cycle process, and enhancing the sustainability of lithium ion deintercalation. Therefore, under the combined effect of the intermediate layer and the outer coating layer, the modified lithium-rich manganese-based positive electrode material has excellent cycle performance and rate performance.

[0061] In addition, when preparing the modified lithium-rich manganese-based positive electrode material in this application, the intermediate layer is directly coated by the solid phase method, and then the amorphous carbon is coated by the wet method. The mesopore size and distribution are adjusted by adjusting the amount of added NH4·H2O, thereby adjusting the specific surface area and morphology, and effectively improving the processing performance of the material. At the same time, the template required for the mesoporous structure is avoided, the synthesis steps are simplified, and the synthesis cost is reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0063] Figure 1 These are SEM images of the positive electrode materials prepared in Example 1, Examples 11-12 and Comparative Example 4. DETAILED DESCRIPTION

[0064] For ease of understanding of the present invention, the application will be described more fully below with reference to relevant embodiments. The following provides preferred embodiments of the application. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0065] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0066] The terms "and / or", "or / and", and "and / or" used herein include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. It should be noted that when at least three items are connected by at least two conjunctions selected from "and / or", "or / and", and "and / or", it should be understood that in the present application, the technical solution undoubtedly includes technical solutions connected by "logical and", and also undoubtedly includes technical solutions connected by "logical or".

[0067] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0068] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0069] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.

[0070] The temperature parameters in this application, unless otherwise specified, allow both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0071] In this application, unless otherwise specified, the size, particle size, and diameter generally refer to the average value. In this application, "particle size" and "particle size" have the same definition, both representing the average particle size of a sphere or a spheroid.

[0072] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the ability to implement the technical solution of this application, solve the technical problems of this application, and achieve the expected technical effects of this application.

[0073] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate differences in content, but should not be construed as limiting the scope of protection of the present application.

[0074] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.

[0075] In the description of the application, "plurality" means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0076] In this application, the terms "first", "second", etc. in "first sintering treatment", "second sintering treatment", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0077] If there is no special description, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present application can be combined with each other to form a new technical solution.

[0078] If there is no special explanation, all the steps of the present application can be performed sequentially or randomly, preferably sequentially.

[0079] Lithium-rich manganese-based cathode materials are considered to be the next generation of lithium-ion battery cathode materials. However, compared with traditional cathode materials, lithium-rich manganese-based materials have a unique phase structure, which makes them more difficult to be used in Li + The oxygen vacancies caused by the loss of lattice oxygen during the deintercalation process will cause the crystal structure to undergo an irreversible transformation from the outside to the inside; in addition, the positive electrode material also has problems such as mixing, segregation and reduction of the average valence state of transition metal elements during the cycle. Therefore, lithium-rich manganese-based materials have obvious defects, such as low initial Coulomb efficiency, fast voltage / capacity decay, poor rate performance, poor electronic conductivity, and slow lithium ion migration, which seriously hinder their practical application.

[0080] In order to improve the above defects, a lot of research has been done in the related technologies on bulk doping, surface coating and structural morphology. Among them, oxide or carbon coating of lithium-rich manganese-based materials can effectively improve their cycle performance, but the single coating structure design still has certain difficulties in improving the overall performance.

[0081] Based on the above problems, the present application uses a material with a rutile structure and an amorphous carbon to compositely coat the lithium-rich manganese-based positive electrode material. The material with a rutile structure is first coated on the surface of the lithium-rich manganese-based positive electrode material to form an intermediate layer, and then an amorphous carbon coating layer with a porous structure is formed on the outermost layer. The combined effect of the two improves the rate performance and cycle performance of the lithium-rich manganese-based positive electrode material.

[0082] One or more embodiments of the present application provide a modified lithium-rich manganese-based positive electrode material, including an inner core, an intermediate layer coated on at least a portion of the surface of the inner core, and an outer coating layer coated on at least a portion of the surface of the intermediate layer; the inner core comprises a lithium-rich manganese-based oxide, the intermediate layer comprises a material having a rutile structure, the outer coating layer comprises amorphous carbon, and the outer coating layer has a porous structure.

[0083] It should be noted that the "lithium-rich manganese-based oxide" mentioned above is not limited to lithium manganese oxide. As long as it is an oxide containing lithium and manganese elements, for example, an oxide containing lithium and manganese elements doped with other metal elements (such as transition metal elements), it is within the scope of protection of this application.

[0084] The rutile structure is the ionic crystal structure of AB2 type compounds and belongs to the tetragonal crystal system.

[0085] The use of materials with a rutile structure to coat lithium-rich manganese-based oxides to form an intermediate layer can isolate the direct contact between the electrolyte and the active electrode material, reduce a series of side reactions, and improve the cycle performance of the positive electrode material; materials with a rutile structure can provide a fast lithium ion transmission channel and good electronic conductivity, which helps to improve the charge and discharge efficiency of the battery; but if only materials with a rutile structure are used for coating, capacity attenuation and structural damage are prone to problems during long-term cyclic use. The use of amorphous carbon coating to form an outer coating layer can effectively improve the conductivity and structural stability of the material, reduce the volume change and structural damage of the material during the charge and discharge process, and thus improve the cycle life and rate performance of the material.

[0086] At the same time, materials with rutile structure can promote Me-C bonding, and they have unique bridging oxygen atoms (O br ) can promote the dissociation of CH and reduce the activation barrier required for CC coupling reaction, which is conducive to the uniform coating of amorphous carbon layer on the surface of positive electrode materials. Among them, Me is a metal atom with unsaturated coordination in the rutile structure.

[0087] The mesoporous structure is introduced into the carbon coating layer, which is Li + The deintercalation of Li provides a three-dimensional channel to accelerate the + The pore structure can increase the contact area of ​​the active material, which is beneficial to improve the energy density and power density. Since the lithium ion deintercalation of the positive electrode material will cause volume changes, the pore structure can provide a certain amount of pore space to alleviate the volume expansion of the positive electrode material, reduce structural damage, and extend the cycle life of the battery.

[0088] It can be understood that the modified lithium-rich manganese-based positive electrode material provided by the present application, wherein the interlayer contains a material having a rutile structure, and the outer coating layer contains amorphous carbon and has a porous structure; compared with the unmodified lithium-rich manganese-based material, the material having a rutile structure contained in the interlayer of the modified lithium-rich manganese-based positive electrode material of the present application has a special bridging oxygen atom (O br ) structure, which can enhance the stability of the outer coating layer, hinder the penetration and corrosion of the electrolyte to the core material, and at the same time improve the electronic conductivity and lithium ion transmission rate; the pore structure of the outer coating layer can effectively improve the toughness of the material, thereby effectively slowing down the cracking of the positive electrode material caused by lattice distortion during the cycle process, and enhancing the sustainability of lithium ion deintercalation. Therefore, under the combined effect of the intermediate layer and the outer coating layer, the modified lithium-rich manganese-based positive electrode material has excellent cycle performance and rate performance.

[0089] In some embodiments, the material having a rutile structure includes one or more of TiO2, RuO2, IrO2, and SnO2.

[0090] In some embodiments, the mass of the intermediate layer is 0.05%-0.15% of the mass of the core; for example, it can be but not limited to 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.1%, 0.11%, 0.12%, 0.13%, 0.14%, 0.15% or the range between any two of the above values. The intermediate layer is a material with a rutile structure, which has a special O br The structure can promote C coating, hinder the penetration and corrosion of the electrolyte to the core material, and improve the electronic conductivity and lithium ion transmission rate. When the mass of the intermediate layer accounts for the mass of the core within the above range, it is conducive to the uniform and stable combination of the intermediate layer and the C coating to prevent the core from being corroded, and it can also prevent the intermediate layer and the C coating from being too close and dense, resulting in Li + Transmission is obstructed and rate performance is reduced.

[0091] In some optional embodiments, the mass of the intermediate layer is 0.08%-0.1% of the mass of the core.

[0092] In some embodiments, the pore structure of the outer coating layer has a pore size of 2nm-50nm; for example, it can be but not limited to 2nm, 5nm, 8nm, 10nm, 12nm, 15nm, 18nm, 20nm, 22nm, 25nm, 28nm, 30nm, 32nm, 35nm, 38nm, 40nm, 42nm, 45nm, 48nm, 50nm or the range between any two of the above pore sizes. When the pore size of the pore structure is in the above range, the material conductivity can be improved, and the porous structure can alleviate the stress concentration caused by the volume change of the material due to the deintercalation of Li during the cyclic charge and discharge process, thereby alleviating cracking. If the pore size is too small, the ability to alleviate the stress of volume change is limited, and the cycle optimization cannot be achieved; if the pore size is too large, the electrolyte is in direct contact with the rutile structure coating, which is easy to cause corrosion, and the material conductivity decreases. The amorphous porous carbon coating is too thin, and the stress relief effect is limited; if it is too thick, Li transmission is inhibited.

[0093] In some embodiments, the chemical formula of the lithium-rich manganese-based oxide is xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element includes one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S. When the lithium-rich manganese-based oxide is doped with the M element, it has at least the following beneficial effects:

[0094] (1) Li doping: Na, Mg and other elements replace Li, play a supporting role, widen the Li interlayer spacing, and increase Li +transmission efficiency.

[0095] (2) Transition metal doping: (a) Elements such as Y, Nb, and Co form MO bonds with O atoms, which have a high activation barrier and stabilize the lattice oxygen, inhibiting the oxygen evolution reaction; (b) Elements such as Co, Ti, and Zr have unstable electrons in 3d and 4d orbitals, which can provide charges for the redox reactions during the charging and discharging process, thereby increasing the battery capacity.

[0096] (3) O-site doping: P, S, F and other elements form polyanion doping, which has a higher MO bond, can stabilize the lattice oxygen, slow down the oxygen decomposition reaction, and improve the cycle performance.

[0097] In some optional embodiments, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7); for example, it can be, but is not limited to, 3:2, 3:2.3, 3:2.5, 3:2.7, 3:3, 3:3.3, 3:3.5, 3:3.7, 3:4, 3:4.3, 3:4.5, 3:4.7, 3:5, 3:5.3, 3:5.5, 3:5.7, 3:6, 3:6.3, 3:6.5, 3:6.7, 3:7 or a range between any two of the above ratios. When the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is within the above range, the molar ratio of Li2MnO3 in the synthesized lithium-rich manganese-based oxide can take into account the capacity and cycle stability of the modified lithium-rich manganese-based positive electrode material. In some optional embodiments, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(4-7).

[0098] In some optional embodiments, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(5-7).

[0099] In some optional embodiments, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%; for example, it can be but not limited to 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or the range between any two of the above values. When the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is within the above range, the capacity and cycle stability of the modified lithium-rich manganese-based positive electrode material can be taken into account.

[0100] In some of the embodiments, the modified lithium-rich manganese-based positive electrode material includes secondary particles.

[0101] As a possible implementation mode, the median particle size D50 of the modified lithium-rich manganese-based positive electrode material is 2.5μm-3.5μm; when the median particle size D50 of the modified lithium-rich manganese-based positive electrode material is within the above range, the compaction density can be increased to increase the energy density of the battery, while ensuring that the kinetic performance is not reduced.

[0102] In some exemplary embodiments, the specific surface area of ​​the modified lithium-rich manganese-based positive electrode material is 0.5 m 2 / g-8m 2 / g; for example, but not limited to 0.5m 2 / g, 1m 2 / g, 1.5m 2 / g, 2m 2 / g, 2.5m 2 / g, 3m 2 / g, 3.5m 2 / g, 4m 2 / g, 4.5m 2 / g, 5m 2 / g, 5.5m 2 / g, 6m 2 / g, 6.5m 2 / g, 7m 2 / g, 7.5m 2 / g, 8m 2 / g or the range between any two of the above specific surface areas, etc. When the specific surface area of ​​the modified lithium-rich manganese-based positive electrode material is within the above range, it is beneficial to further improve the rate performance of the material.

[0103] In some embodiments, the carbon content of the modified lithium-rich manganese-based positive electrode material is 0.1wt-0.4wt%; for example, it can be but not limited to 0.1wt%, 0.12wt%, 0.15wt%, 0.18wt%, 0.2wt%, 0.22wt%, 0.25wt%, 0.28wt%, 0.3wt%, 0.32wt%, 0.35wt%, 0.38wt%, 0.4wt% or the range between any two of the above values. Thus, the outer coating layer can be more evenly distributed and has sufficient ionic conductivity.

[0104] In some optional embodiments, the carbon content of the modified lithium-rich manganese-based positive electrode material is 0.1 wt%-0.3 wt%.

[0105] In some optional embodiments, the carbon content of the modified lithium-rich manganese-based positive electrode material is 0.15 wt%-0.25 wt%.

[0106] One or more embodiments of the present application further provide a method for preparing a modified lithium-rich manganese-based positive electrode material, which can prepare the aforementioned modified lithium-rich manganese-based positive electrode material, and the preparation method comprises the following steps:

[0107] A mixed material comprising an inner core and a material having a rutile structure is subjected to a first sintering treatment to coat at least a portion of the surface of the inner core with an intermediate layer to prepare an intermediate; a mixed solution containing the intermediate and an organic carbon source is prepared, the pH of the mixed solution is adjusted with an ammonia solution, the solid-liquid separation is performed, and the mixture is dried; and a solid obtained after drying is subjected to a back-firing treatment to prepare a modified lithium-rich manganese-based positive electrode material; wherein the back-firing treatment temperature is 500°C < ≤ 800°C.

[0108] As an example, the temperature of the back-firing treatment may be, but is not limited to, 510°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, or a range between any two of the above temperatures. When the temperature of the back-firing treatment is within the above range, it is beneficial to form an outer coating layer (amorphous carbon layer) with good toughness, which can effectively reduce the occurrence of cracking or separation of the outer coating layer from the substrate due to expansion and contraction of the positive electrode material during the charge and discharge process.

[0109] In some optional embodiments, the temperature of the back-firing treatment is 600°C-700°C.

[0110] It should be noted that when preparing the outer coating layer (amorphous carbon layer), the excessive Li + Washing with H + With Li + The interaction of the intermediates creates oxygen vacancies on the surface of the intermediates, thereby increasing the conductivity of the intermediate layer (rutile coating layer); and also partially controlling the Li + There is an activation effect, thereby increasing the capacity of the positive electrode material.

[0111] When preparing the amorphous carbon layer, an organic carbon source is added to the mixed solution, and then the mixture is carbonized by back-firing to obtain the amorphous carbon layer; before the mixed solution is separated into solid and liquid, the pH of the mixed solution is adjusted by adding an ammonia solution, and ammonia gas is generated during the back-firing process, so that the surface amorphous carbon layer has a mesoporous structure. The amorphous carbon layer with a mesoporous structure provides an effective way for charge transfer. Compared with the untreated rutile coating layer, the amorphous carbon layer has a lower charge transfer resistance and a higher lithium ion diffusion coefficient, so that the modified lithium-rich manganese-based positive electrode material finally obtained has a more stable cycle performance and a higher rate performance.

[0112] Understandably, when preparing the modified lithium-rich manganese-based positive electrode material, the intermediate layer is directly coated by the solid phase method, and then the amorphous carbon is coated by the wet method. The mesopore size and distribution are adjusted by adjusting the amount of added NH4·H2O, thereby adjusting the specific surface area and morphology, and effectively improving the processing performance of the material. At the same time, the template required for the mesoporous structure is avoided, the synthesis steps are simplified, and the synthesis cost is reduced.

[0113] In some embodiments, the organic carbon source includes one or more of polyacrylic acid, polyimide, and polypyrrole.

[0114] As a possible implementation, the mass of the organic carbon source accounts for 2%-6% of the mass of the inner core; for example, it can be but not limited to 2%, 2.3%, 2.5%, 2.8%, 3%, 3.3%, 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.8%, 5%, 5.3%, 5.5%, 5.8%, 6% or the range between any two of the above values. When the mass of the organic carbon source accounts for the mass of the inner core in the above range, the outer coating layer can be more evenly distributed and has sufficient ionic conductivity.

[0115] In some optional embodiments, the mass of the organic carbon source accounts for 2% to 3% of the mass of the inner core.

[0116] In some embodiments, the mass of NH4·H2O contained in the ammonia solution accounts for 2%-6% of the mass of the inner core; for example, it can be but not limited to 2%, 2.3%, 2.5%, 2.8%, 3%, 3.3%, 3.5%, 3.8%, 4%, 4.3%, 4.5%, 4.8%, 5%, 5.3%, 5.5%, 5.8%, 6% or the range between any two of the above values. When the mass of NH4 H2O contained in the ammonia solution accounts for the mass of the inner core within the above range, the porous distribution generated when the ammonia solution treats the surface of the material is more uniform.

[0117] In some optional embodiments, the mass of NH4·H2O contained in the aqueous ammonia solution accounts for 2%-4% of the mass of the inner core.

[0118] In some optional embodiments, the mass of NH4·H2O contained in the aqueous ammonia solution accounts for 2%-3% of the mass of the inner core.

[0119] In some embodiments, the mass percentage concentration of the ammonia solution is 10%-50%; for example, it can be but not limited to 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or the range between any two of the above mass percentage concentrations. When the concentration of the ammonia solution is lower than the above range, the reaction speed is slow, which easily leads to the precipitation of Li in the core of the material, resulting in internal lithium deficiency; when the concentration of the ammonia solution is higher than the above range, the reaction speed is too fast, resulting in a larger pore size of the amorphous porous carbon, so that the outermost layer cannot play a role in protecting the core.

[0120] In some optional embodiments, the mass percentage concentration of the ammonia solution is 20%-45%.

[0121] In some exemplary embodiments, an ammonia solution is used to adjust the pH of the mixed solution to 7-10; for example, it may be but is not limited to 7, 7.5, 8, 8.5, 9, 9.5, 10 or a range between any two of the above pH values.

[0122] In some optional embodiments, the temperature of the back-firing treatment is 600°C to 700°C.

[0123] As a possible implementation manner, the time for the back-burning treatment is 10h-20h; for example, it can be but not limited to 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h or a range between any two of the above times.

[0124] In some optional embodiments, the back-burning treatment time is 12h-18h.

[0125] It should be noted that the temperature and time of the back-firing treatment can be combined in any appropriate manner, and both can be selected from any temperature and time of the back-firing treatment described in this article.

[0126] In some optional embodiments, the atmosphere of the backfiring treatment includes nitrogen.

[0127] In some embodiments, the step of preparing a mixed solution containing an intermediate and an organic carbon source comprises: mixing and stirring the intermediate with a solvent, and then adding the organic carbon source to prepare a mixed solution.

[0128] In some optional embodiments, the solvent includes one of water and ethanol aqueous solution.

[0129] In some embodiments, the mass ratio of the solvent to the intermediate is (1-3):1; for example, it can be, but is not limited to, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3:1 or a range between any two of the above mass ratios. When the mass ratio of the solvent to the intermediate is within the above range, it is beneficial to wash away the rich Li on the surface of the material, save costs, and reduce pollution.

[0130] In some exemplary embodiments, the mass percentage of ethanol in the ethanol aqueous solution is 95%-99%; for example, it can be but not limited to 95%, 96%, 97%, 98%, 99% or a range between any two of the above values.

[0131] In some embodiments, the temperature of the first sintering treatment is 400°C-950°C; for example, it can be but not limited to 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or a range between any two of the above temperatures. When the temperature of the first sintering treatment is within the above range, it is beneficial for the intermediate layer to be combined with the core structure.

[0132] In some optional embodiments, the temperature of the first sintering process is 500°C-800°C.

[0133] In some embodiments, the first sintering treatment time is 18h-30h; for example, it can be but not limited to 18h, 19h, 20h, 21h, 22h, 23h, 24h, 25h, 26h, 27h, 28h, 29h, 30h or a range between any two of the above times. When the first sintering treatment time is within the above range, it is beneficial to combine the intermediate layer with the core structure.

[0134] In some optional embodiments, the first sintering treatment lasts for 12 hours to 15 hours.

[0135] It should be noted that the temperature and time of the first sintering treatment may be combined in any appropriate manner, and both may be selected from any temperature and time of the first sintering treatment described herein.

[0136] As a possible implementation manner, the mixed material further includes an additive A, and the elements contained in the additive A include one or more of Al, Si, Zn, Zr and La.

[0137] In some embodiments, the method for preparing the inner core includes: mixing a precursor, a lithium source and an optional additive B, and then performing a second sintering treatment to prepare the inner core; the inner core includes a lithium-rich manganese-based oxide with a chemical formula of xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element includes one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S.

[0138] In some optional embodiments, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7); for example, it can be but is not limited to 3:2, 3:2.3, 3:2.5, 3:2.7, 3:3, 3:3.3, 3:3.5, 3:3.7, 3:4, 3:4.3, 3:4.5, 3:4.7, 3:5, 3:5.3, 3:5.5, 3:5.7, 3:6, 3:6.3, 3:6.5, 3:6.7, 3:7 or a range between any two of the above ratios.

[0139] In some optional embodiments, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%; for example, it can be but not limited to 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or the range between any two of the above values.

[0140] In some optional embodiments, the lithium source includes one or more of lithium carbonate, lithium hydroxide and lithium sulfate.

[0141] As a possible embodiment, the lithium source includes lithium carbonate and lithium hydroxide in a molar ratio of (3-5): 1; the molar ratio of lithium carbonate and lithium hydroxide can be, but is not limited to, 3: 1, 3.1: 1, 3.2: 1, 3.3: 1, 3.4: 1, 3.5: 1, 3.6: 1, 3.7: 1, 3.8: 1, 3.9: 1, 4: 1, 4.1: 1, 4.2: 1, 4.3: 1, 4.4: 1, 4.5: 1, 4.6: 1, 4.7: 1, 4.8: 1, 4.9: 1, 5: 1 or a range between any two of the above ratios. When the molar ratio of lithium carbonate and lithium hydroxide is within the above range, lithium hydroxide can be better dispersed into the polycrystalline matrix due to its low melting point, promoting internal matrix reaction and grain growth, and improving the material structure stability and cycle stability.

[0142] In some exemplary embodiments, the lithium source includes lithium carbonate and lithium sulfate in a molar ratio of ≥5:1; the molar ratio of lithium carbonate to lithium sulfate can be, but is not limited to, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1, 12:1, 12.5:1, 13:1, 13.5:1, 14:1, 14.5:1, 15:1 or a range between any two of the above ratios. When the molar ratio of lithium carbonate to lithium sulfate is within the above range, lithium sulfate, as a co-solvent, can promote the growth and fusion of primary particles, increase the compaction density of the positive electrode, and thus achieve the purpose of increasing the energy density.

[0143] In some optional embodiments, the lithium source includes lithium carbonate and lithium sulfate in a molar ratio of (8-13):1.

[0144] In some embodiments, the temperature of the second sintering treatment is 700°C-1050°C; for example, it can be but not limited to 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C or a range between any two of the above temperatures.

[0145] In some optional embodiments, the temperature of the second sintering process is 700°C-1000°C.

[0146] In some exemplary embodiments, the time of the second sintering treatment is 10 hours to 28 hours; for example, it can be but is not limited to 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 23 hours, 25 hours, 28 hours or a range between any two of the above times.

[0147] It should be noted that the temperature and time of the second sintering treatment may be combined in any appropriate manner, and both may be selected from any temperature and time of the second sintering treatment described herein.

[0148] As a possible embodiment, the elements contained in the precursor include Ni and Mn, and the molar ratio of Ni to Mn is 3:(2-7); for example, it can be but not limited to 3:2, 3:2.3, 3:2.5, 3:2.7, 3:3, 3:3.3, 3:3.5, 3:3.7, 3:4, 3:4.3, 3:4.5, 3:4.7, 3:5, 3:5.3, 3:5.5, 3:5.7, 3:6, 3:6.3, 3:6.5, 3:6.7, 3:7 or a range between any two of the above ratios.

[0149] As an example, the precursor may be one or more of carbonate, hydroxide, and oxalate.

[0150] In some optional embodiments, the elements contained in the precursor further include one or more of Na, Sr, Ta, Ga, Sn, Te and Ce.

[0151] In some exemplary embodiments, the additive B contains one or more elements of Mg, Y, Ti, Zr, Nb, Cr, Mo, W, Co, Al, P, Sb, La, F, and S.

[0152] One or more embodiments of the present application provide a positive electrode plate, including the modified lithium-rich manganese-based positive electrode material provided by one or more embodiments of the present application or the modified lithium-rich manganese-based positive electrode material prepared by the preparation method provided by one or more embodiments of the present application.

[0153] One or more embodiments of the present application provide a secondary battery, including the positive electrode sheet provided by one or more embodiments of the present application.

[0154] The secondary battery of the present application comprises the above-mentioned modified lithium-rich manganese-based positive electrode material and has excellent cycle performance and rate performance.

[0155] One or more embodiments of the present application provide an electric device, including a secondary battery provided by one or more embodiments of the present application. The electric device can be an electric car, an electric bicycle, an electric two-wheeled vehicle, an electric car power system, an energy storage system, or a mobile storage device, etc., without limitation.

[0156] The electric device of the present application includes the secondary battery provided by the present application, and thus has at least the same advantages as the secondary battery.

[0157] The technical scheme of the present invention is described in detail below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods for which specific conditions are not specified in the following embodiments are preferably referred to the guidance given in the present invention, and can also be based on the experimental manuals or conventional conditions in the art, or can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0158] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.

[0159] 1. Preparation of modified lithium-rich manganese-based cathode materials

[0160] S1. Preparation of core: Ni 0.36 Mn 0.64(OH)2 (as precursor), Li2CO3 (as lithium source), LiOH (as lithium source), WO3 (as additive) and AlF3 (as additive) were mixed and placed in a sagger, and then placed in a muffle furnace, and dry air was introduced. The temperature was raised to 450°C at a rate of 2°C / min, sintered for 4h, and then continued to be raised to 900°C and sintered for 15h; then the core (lithium-rich manganese-based oxide, chemical formula Li 1.3 Ni 0.35 Mn 0.65 O 2.3 ). The average particle size D50 of the inner core is 3.45 μm.

[0161] Among them, the theoretical amount of Li2CO3 is calculated according to the ratio of the molar amount of lithium to the molar sum of other metal elements except lithium, which is 1.34. The actual weighed amount of Li2CO3 is 1.03wt% of the theoretical amount of Li2CO3. The actual weighed amount of lithium hydroxide is 0.05wt% of the theoretical amount of Li2CO3. The theoretical amount of the core finally obtained is (precursor + lithium salt) × 0.91, the mass of W contained in WO3 accounts for 1% of the theoretical amount of the core, and the mass of Al in AlF3 accounts for 0.8% of the theoretical amount of the core.

[0162] S2. The core and TiO2 (as a material having a rutile structure) are mixed uniformly, and then sintered in an air atmosphere at 825°C for 15 hours to coat the surface of the core with an intermediate layer, and after cooling to room temperature, an intermediate is obtained. The amount of TiO2 used is 0.1% of the mass of the core.

[0163] S3. The intermediate is mixed with deionized water at a temperature of 0°C in a mass ratio of 1:2, stirred for 5 minutes, and then a polyacrylic acid (PAA) solution with a mass percentage concentration of 30% is added; after stirring for 5 minutes, a 25% ammonia solution with a mass percentage concentration is added, stirred for 10 minutes, and then filtered. The resulting filter cake is dried at 80°C and then sintered at 600°C in a nitrogen atmosphere for 13 hours to form an outer coating layer on the surface of the intermediate, with a heating rate of 2°C / min. After sintering, the final product is sieved. Among them, the mass of polyacrylic acid (PAA) is 2% of the mass of the core; the mass of NH4·H2O in the ammonia solution is 2% of the mass of the core.

[0164] Example 2

[0165] The difference between Example 2 and Example 1 is that RuO2 is used to replace TiO2 in step S2, and the rest are the same.

[0166] Example 3

[0167] The difference between Example 3 and Example 1 is that IrO2 is used to replace TiO2 in step S2, and the rest are the same.

[0168] Example 4

[0169] The difference between Example 4 and Example 1 is that SnO2 is used to replace TiO2 in step S2, and the rest are the same.

[0170] Example 5

[0171] The difference between Example 5 and Example 1 is that the amount of TiO2 used in step S2 is 0.05% of the mass of the core; the rest are the same.

[0172] Example 6

[0173] The difference between Example 6 and Example 1 is that the amount of TiO2 used in step S2 is 0.15% of the mass of the core; the rest are the same.

[0174] Example 7

[0175] The difference between Example 7 and Example 1 is that polyimide (PI) is used to replace polyacrylic acid (PAA) in step S3, and the rest are the same.

[0176] Example 8

[0177] The difference between Example 8 and Example 1 is that in step S3, polypyrrole (PPy) is used to replace polyacrylic acid (PAA), and 95% ethanol aqueous solution is used to replace deionized water, and the other aspects are the same.

[0178] Example 9

[0179] The difference between Example 9 and Example 1 is that the mass of polyacrylic acid (PAA) in step S3 is 4% of the mass of the core; the others are the same.

[0180] Example 10

[0181] The difference between Example 10 and Example 1 is that the mass of polyacrylic acid (PAA) in step S3 is 6% of the mass of the core; the others are the same.

[0182] Embodiment 11

[0183] The difference between Example 11 and Example 1 is that the mass of NH4·H2O in the ammonia solution in step S3 is 4% of the mass of the core, and the other parts are the same.

[0184] Example 12

[0185] The difference between Example 12 and Example 1 is that the mass of NH4·H2O in the ammonia solution in step S3 is 6% of the mass of the core, and the other parts are the same.

[0186] Embodiment 13

[0187] The difference between Example 13 and Example 1 is that the temperature of the back-firing treatment in step S3 is 800° C., and the others are the same.

[0188] Comparative Example 1

[0189] The difference between Comparative Example 1 and Example 1 is that after the lithium-rich manganese-based positive electrode oxide is prepared by the method of step S1, the intermediate layer and the outer coating layer are not further coated.

[0190] Comparative Example 2

[0191] The difference between Comparative Example 2 and Example 1 is that only the preparations of step S1 and step S2 are performed, and the preparation of step S3 is not performed.

[0192] Comparative Example 3

[0193] The difference between Comparative Example 3 and Example 1 is that the core prepared in step S1 is directly wet treated and back-fired using a solution containing polyacrylic acid (PAA), and the other parts are the same; the specific process is as follows:

[0194] The core was mixed with deionized water at a temperature of 0°C in a mass ratio of 1:2, stirred for 5 minutes, and then a polyacrylic acid (PAA) solution with a mass percentage concentration of 30% was added; after stirring for 10 minutes, suction filtration was performed, and the obtained filter cake was dried at 80°C and then calcined at 600°C in a nitrogen atmosphere for 13 hours to form an outer coating layer on the surface of the intermediate, with a heating rate of 2°C / min, and the final product was obtained by sintering and sieving. Among them, the mass of polyacrylic acid (PAA) is 2% of the mass of the core.

[0195] Comparative Example 4

[0196] The difference between Comparative Example 4 and Example 1 is that no ammonia solution is added in step S3, and the other steps are the same; specifically, as follows:

[0197] The intermediate was mixed with deionized water at a temperature of 0°C in a mass ratio of 1:2, stirred for 5 minutes, and then a polyacrylic acid (PAA) solution with a mass percentage concentration of 30% was added; after stirring for 10 minutes, suction filtration was performed, and the obtained filter cake was dried at 80°C and then calcined at 600°C in a nitrogen atmosphere for 13 hours to form an outer coating layer on the surface of the intermediate, with a heating rate of 2°C / min, and the final product was obtained by sintering and sieving. Among them, the mass of polyacrylic acid (PAA) is 2% of the mass of the core.

[0198] Comparative Example 5

[0199] The difference between Comparative Example 5 and Example 1 is that the temperature of the back-firing treatment in step S3 is 450° C., and the others are the same.

[0200] The parameter settings of the above embodiments and comparative examples are shown in Table 1.

[0201] Table 1

[0202]

[0203] 2. Physical and Chemical Properties Test of Cathode Materials

[0204] 1. The SEM images of the positive electrode materials prepared in Example 1, Examples 11-12 and Comparative Example 4 are as follows: Figure 1 As shown by Figure 1 It can be seen that the size and structure of the pores contained in the outer coating layer (amorphous carbon layer) can be adjusted by adjusting the amount of NH4·H2O added.

[0205] 2. Specific surface area test (BET test method)

[0206] The BET test method, namely the BET specific surface area test method, is based on the multi-molecular layer adsorption formula derived by Brunauer, Emmett and Teller. In the BET test, nitrogen is usually used as the adsorbate, and the specific surface area and pore structure of the material are calculated by measuring the amount of nitrogen adsorbed on the surface of the material. First, the sample is degassed by heating and vacuuming to remove moisture and other impurities on the surface and pores of the material; then the sample is weighed and recorded; the sample is placed in liquid nitrogen, and the nitrogen adsorption of the sample is measured at different pre-set pressure points at liquid nitrogen temperature to obtain the adsorption isotherm.

[0207] 3. Carbon content test (C%)

[0208] The working principle of the high-frequency infrared carbon and sulfur analyzer is based on the infrared absorption method. The sample is heated together with the solvent, and the sample is burned at high temperature in a high-frequency induction furnace, so that the carbon and sulfur elements in the sample react with oxygen to generate carbon dioxide and sulfur dioxide gas. Driven by the carrier gas, these gases enter the detection chamber through the gas path processing system. CO2 and SO2 gases are absorbed under specific wavelengths of infrared light, which are 4.26μm and 7.40μm respectively. The detector converts the received light signal into an electrical signal, which is normalized, calibrated and integrated by a microcomputer to finally obtain the percentage content of carbon and sulfur elements.

[0209] 4. Median particle size D50 test

[0210] The particle size is measured using Mastersizer 3000 with laser beam technology. When the laser beam passes through the dispersed particle sample, the particle size measurement is completed by measuring the intensity of the scattered light. The data is then used to analyze and calculate the particle size distribution that forms the scattering spectrum. After turning on the machine, the particle size test is performed after alignment with the standard sample. Immerse the laser head in deionized water, add dispersant to the cup, and stabilize the solution by ultrasound. Add the finished cathode material to the solution, and after the first test is completed, test it again by ultrasound for 60s. The final D50 is the data after ultrasound.

[0211] The test results of the above embodiments and comparative examples are shown in Table 2.

[0212] Table 2

[0213] Group <![CDATA[BET / m 2 / g]]> C / wt% D50 / μm Example 1 1.0160 0.1639 3.49 Example 2 1.0338 0.1643 3.39 Example 3 1.0184 0.1635 3.36 Example 4 1.0186 0.1529 3.66 Example 5 1.0793 0.1635 3.45 Example 6 1.0537 0.1610 3.46 Example 7 1.0796 0.2010 3.47 Example 8 0.9281 0.2126 3.42 Example 9 0.9570 0.2989 3.31 Example 10 0.9081 0.3229 3.28 Embodiment 11 1.1751 0.2549 3.34 Example 12 1.3321 0.2367 3.49 Embodiment 13 1.0300 0.1374 3.23 Comparative Example 1 1.0677 / 3.21 Comparative Example 2 1.2212 / 3.23 Comparative Example 3 1.0097 0.1096 3.23 Comparative Example 4 1.0635 0.1699 3.27 Comparative Example 5 1.0922 0.1608 3.38

[0214] In Table 2, “C” represents the carbon content of the positive electrode material.

[0215] 3. Preparation and performance testing of secondary batteries

[0216] The positive electrode materials prepared in the above embodiments and comparative examples were mixed with the conductive agent Super-P and the binder PVDF in a mass ratio of 92:4:4, and an appropriate amount of NMP solution was added to form a slurry, which was coated on the double-layer surface of the aluminum foil, dried and baked in a vacuum oven at 150°C for 12 hours. After that, the secondary battery was assembled in an Ar atmosphere glove box, with metallic lithium as the negative electrode and 1 mol / L LiPF6 dissolved in a mixed organic solvent with a volume ratio of EC:EMC=3:7 as the electrolyte, and assembled into a button CR2032 battery.

[0217] Using constant current and constant voltage charging + constant current discharge charging and discharging mode, with a current density of 1C=230mAh / g, at a rate of 0.1C, the first cycle of charge and discharge activation and rate test were performed in the voltage window of 2.5V-4.6V, followed by a 50-week cycle test at 2.5V-4.55V and 0.33C. The results are shown in Table 3.

[0218] Table 3

[0219]

[0220] From the comparison of the results of Examples 1-11 and Comparative Examples 1-5 in Table 3, it can be seen that by composite coating the lithium-rich manganese-based positive electrode material with an intermediate layer (rutile coating layer) and an outer coating layer (amorphous carbon), the discharge capacity, rate performance and cycle performance of the positive electrode material can be effectively improved as a whole.

[0221] Although carbon coating was performed in Examples 7 and 8, the carbon source and Li +Without complex reaction, the excess Li is washed away by water, resulting in low capacity; PI and PPy have large molecular weights and are adsorbed on the surface of the material. Even if there are porous results after carbonization, the surface carbon layer is thick, resulting in Li + The transmission is hindered and the rate performance is reduced. In Example 10, the carbon coating layer is too thick, resulting in Li + The transmission is blocked and the rate performance is reduced. In Example 13, the sintering temperature is high, resulting in the formation of LiO x In Comparative Example 5, due to the low backfiring temperature, the carbonized layer is not strong enough and the cycle performance is poor.

[0222] Compared with the capacity and rate performance in Example 12, the cycle performance is improved less, which may be due to the large amount of ammonia solution used, and the amorphous carbon layer finally obtained has more pores and larger pores, resulting in less improvement in cycle stability.

[0223] The difference between Example 1, Example 13 and Comparative Example 5 is the different back-firing temperatures. Comparison of the results of Example 1, Example 13 and Comparative Example 5 shows that when the back-firing temperature is 500°C < ≤ 800°C, it is conducive to the formation of an outer coating layer (amorphous carbon layer) with good toughness, which can effectively reduce the occurrence of cracking or separation of the outer coating layer from the substrate due to expansion and contraction of the positive electrode material during the charge and discharge process. When the back-firing temperature is lower than the above range, a large amount of organic matter exists on the surface of the obtained positive electrode material, and Li + Diffusion is hindered, capacity cannot be fully utilized, and rate performance is reduced.

[0224] By comparing the results of Comparative Example 3 and Comparative Example 4, it can be seen that the carbon content of the positive electrode material obtained in Comparative Example 4 is significantly higher than the carbon content of the positive electrode material obtained in Comparative Example 3, indicating that by coating the material with a rutile structure, the adsorption and reaction of carbon can be promoted, thereby increasing the carbon content of the positive electrode material.

[0225] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0226] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A modified lithium-rich manganese-based positive electrode material, characterized in that: include: a core comprising a lithium-rich manganese-based oxide; an intermediate layer, coated on at least a portion of the surface of the inner core, wherein the intermediate layer comprises a material having a rutile structure; The outer coating layer is coated on at least a portion of the surface of the intermediate layer, wherein the outer coating layer comprises amorphous carbon and has a pore structure.

2. The modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The intermediate layer has at least one of the following characteristics (1)-(3): (1) The material having a rutile structure includes one or more of TiO2, RuO2, IrO2 and SnO2; (2) The mass of the intermediate layer accounts for 0.05% to 0.15% of the mass of the inner core; (3) The intermediate layer further contains one or more doping elements selected from the group consisting of Al, Si, Zn, Zr and La.

3. The modified lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The pore structure has a pore diameter of 2nm-50nm.

4. The modified lithium-rich manganese-based positive electrode material according to any one of claims 1 to 3, characterized in that: The modified lithium-rich manganese-based positive electrode material has at least one of the following characteristics (1)-(3): (1) The chemical formula of the lithium-rich manganese-based oxide is xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element includes one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S; Optionally, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7); Optionally, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%; (2) The modified lithium-rich manganese-based positive electrode material includes secondary particles; (3) The median particle size D50 of the modified lithium-rich manganese-based positive electrode material is 2.5 μm-3.5 μm; (4) The specific surface area of ​​the modified lithium-rich manganese-based positive electrode material is 0.5 m 2 / g-8m 2 / g; (5) The carbon content of the modified lithium-rich manganese-based positive electrode material is 0.1wt-0.4wt%.

5. A method for preparing a modified lithium-rich manganese-based positive electrode material according to any one of claims 1 to 4, characterized in that: The steps include: Performing a first sintering treatment on a mixture of a core and a material having a rutile structure, so as to coat at least a portion of the surface of the core with an intermediate layer, thereby preparing an intermediate; preparing a mixed solution containing the intermediate and an organic carbon source, adjusting the pH of the mixed solution with an ammonia solution, separating the solid from the liquid, and drying; The solid obtained after drying is subjected to a back-firing treatment to prepare the modified lithium-rich manganese-based positive electrode material; Wherein, 500°C<the temperature of the back-firing treatment≤800°C.

6. The preparation method according to claim 5, characterized in that: The organic carbon source comprises one or more of polyacrylic acid, polyimide and polypyrrole; and / or The mass of the organic carbon source accounts for 2%-6% of the mass of the inner core, and can be optionally 2%-3%.

7. The preparation method according to claim 5, characterized in that: The mass of NH4·H2O contained in the ammonia solution accounts for 2%-6% of the mass of the core, and can be 2%-3%; and / or The mass percentage concentration of the ammonia solution is 10%-50%; and / or The pH of the mixed solution is adjusted to 7-10 using an ammonia solution.

8. The preparation method according to claim 5, characterized in that: The temperature of the back-firing treatment is 600°C-700°C; and / or The back-burning treatment time is 10h-20h; and / or The atmosphere of the back-firing treatment includes nitrogen.

9. The preparation method according to claim 5, characterized in that: The steps of preparing a mixed solution containing the intermediate and an organic carbon source include: The intermediate is mixed with a solvent and stirred, and then an organic carbon source is added to prepare the mixed solution; Optionally, the solvent includes one of water and ethanol aqueous solution; Optionally, the mass ratio of the solvent to the intermediate is (1-3):1; Optionally, the temperature of the solvent is 0°C-10°C; Optionally, the mass proportion of ethanol in the ethanol aqueous solution is 95%-99%.

10. The preparation method according to claim 5, characterized in that: The mass of the material having a rutile structure is 0.05%-0.15% of the mass of the core, and can be 0.08%-0.1%; and / or The temperature of the first sintering treatment is 400° C.-950° C., and can be 500° C.-800° C.; and / or The first sintering treatment time is 18h-30h; and / or The mixed material further comprises an additive A, wherein the additive A comprises one or more elements selected from the group consisting of Al, Si, Zn, Zr and La.

11. The preparation method according to any one of claims 5 to 10, characterized in that: The preparation method of the inner core comprises: After mixing the precursor, the lithium source and the optional additive B, a second sintering treatment is performed to prepare the core; the core comprises a lithium-rich manganese-based oxide with a chemical formula of xLi2MnO3·(1-x)LiMnNiMO2, 0.1≤x≤0.4, and the M element comprises one or more of Na, Mg, Sr, Y, Ti, Zr, Nb, Ta, Cr, Mo, W, Co, Al, Ga, Sn, P, Sb, Te, La, Ce, F and S; Optionally, the molar ratio of nickel to manganese in the lithium-rich manganese-based oxide is 3:(2-7); Optionally, the molar proportion of Li2MnO3 in the lithium-rich manganese-based oxide is 10%-30%; Optionally, the lithium source includes one or more of lithium carbonate, lithium hydroxide and lithium sulfate; Optionally, the lithium source comprises lithium carbonate and lithium hydroxide in a molar ratio of (3-5):1; Optionally, the lithium source comprises lithium carbonate and lithium sulfate in a molar ratio of ≥5:1; Optionally, the temperature of the second sintering treatment is 700°C-1050°C, optionally 700°C-1000°C; Optionally, the second sintering treatment time is 10h-28h; Optionally, the elements contained in the precursor include Ni and Mn, and the molar ratio of Ni to Mn is 3:(2-7); Further optionally, the elements contained in the precursor further include one or more of Na, Sr, Ta, Ga, Sn, Te and Ce; Optionally, the elements contained in the additive B include one or more of Mg, Y, Ti, Zr, Nb, Cr, Mo, W, Co, Al, P, Sb, La, F and S.

12. A positive electrode sheet, characterized in that: It comprises the modified lithium-rich manganese-based positive electrode material as described in any one of claims 1 to 4 or the modified lithium-rich manganese-based positive electrode material prepared by the preparation method as described in any one of claims 5 to 11.

13. A secondary battery, characterized in that: Comprising the positive electrode sheet as described in claim 12.

14. An electrical device, characterized in that: Comprising the secondary battery as claimed in claim 13.

Citation Information

Cited By

  • Lithium ion secondary battery, positive electrode active material, preparation method and electric equipment

    CN121215860A