Semiconductor device

By introducing an oxide metal layer and an insulating layer into an oxide semiconductor device, and supplying oxygen through oxidation annealing technology, the problems of oxygen deficiency and insulating layer defects are solved, and a semiconductor device with high mobility and high reliability is achieved.

CN118872072APending Publication Date: 2024-10-29JAPAN DISPLAY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380021202.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing oxide semiconductor devices have difficulty balancing high mobility and reliability, and oxygen deficiency and insulating layer defects affect electronic properties and reliability.

Method used

Introducing an oxide metal layer and an insulating layer into an oxide semiconductor device, supplying oxygen on the upper surface and sides of the oxide semiconductor layer through oxidation annealing technology, repairing oxygen defects, and diffusing aluminum into the insulating layer to improve the barrier properties of the oxide metal layer .

Benefits of technology

A semiconductor device with high mobility and high reliability is realized, oxygen deficiency in the oxide semiconductor layer and insulating layer defects are reduced, and electronic characteristics and reliability test results are stabilized.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872072A_ABST
    Figure CN118872072A_ABST
Patent Text Reader

Abstract

A semiconductor device includes: an oxidized metal layer over an insulating surface; an oxide semiconductor layer over the oxide metal layer; and an insulating layer on the oxide semiconductor layer, in which the insulating layer includes a first region overlapping the oxide semiconductor layer, and the first region has a first aluminum concentration of 1 * 1017 atoms / cm3 or more. The first region may be a region 50 nm or less from the surface of the insulating layer located on the opposite side of the oxide semiconductor layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor as a channel. Background Art

[0002] In recent years, the development of semiconductor devices using oxide semiconductors for channels instead of amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon has been progressing (for example, see Patent Documents 1 to 6). Semiconductor devices using oxide semiconductors for channels can be formed with a simple structure and a low-temperature process, just like semiconductor devices using amorphous silicon for channels. It is known that semiconductor devices using oxide semiconductors for channels have higher mobility than semiconductor devices using amorphous silicon for channels.

[0003] In order to stably operate a semiconductor device using an oxide semiconductor for a channel, it is important to supply oxygen to the oxide semiconductor layer during its manufacturing process to reduce oxygen vacancies formed in the oxide semiconductor layer. For example, as one method of supplying oxygen to the oxide semiconductor layer, a technique of forming an insulating layer covering the oxide semiconductor layer under the condition that the insulating layer contains more oxygen is disclosed.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0008] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0009] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0010] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0011] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, the insulating layer formed under the condition of containing more oxygen contains more defects. Due to its influence, the characteristic abnormality of the semiconductor device or the characteristic variation in the reliability test occurs, which is believed to be caused by the electrons being captured by the defects. On the other hand, if an insulating layer with fewer defects is used, the oxygen contained in the insulating layer cannot be increased. As a result, oxygen cannot be fully supplied from the insulating layer to the oxide semiconductor layer. In this way, it is required to realize a structure that can reduce the defects in the insulating layer that cause the characteristic variation of the semiconductor device and repair the oxygen deficiency formed in the oxide semiconductor layer.

[0014] In addition, it is known that a semiconductor device with high mobility can be obtained by relatively increasing the ratio of indium contained in the oxide semiconductor layer. However, when the ratio of indium contained in the oxide semiconductor layer is high, oxygen vacancies are easily formed in the oxide semiconductor layer. Therefore, in order to achieve high mobility while maintaining high reliability, it is necessary to work on the formation of the insulating layer around the oxide semiconductor layer.

[0015] One object of one embodiment of the present invention is to provide a semiconductor device having high mobility and high reliability.

[0016] Means for solving problems

[0017] A semiconductor device according to one embodiment of the present invention comprises: an oxide metal layer on an insulating surface; an oxide semiconductor layer on the oxide metal layer; and an insulating layer on the oxide semiconductor layer, wherein the insulating layer comprises a first region overlapping the oxide semiconductor layer, and a first aluminum concentration in the first region is 1×10 17 atoms / cm 3 above. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] [ Figure 1 ] is a cross-sectional view showing an overview of a semiconductor device involved in one embodiment of the present invention.

[0019] [ Figure 2 ] is a top view showing an overview of a semiconductor device involved in one embodiment of the present invention.

[0020] [ Figure 3 ] is a flowchart showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0021] [ Figure 4 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0022] [ Figure 5 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0023] [ Figure 6 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0024] [ Figure 7 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0025] [ Figure 8 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0026] [ Fig. 9 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0027] [ Fig.10 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0028] [ Fig.11 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0029] [ Fig.12 ] is a cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0030] [ Fig.13 ] is a top view showing an overview of a display device involved in one embodiment of the present invention.

[0031] [ Fig.14 ] is a block diagram showing the circuit structure of a display device involved in one embodiment of the present invention.

[0032] [ Fig.15 ] is a circuit diagram showing a pixel circuit of a display device according to one embodiment of the present invention.

[0033] [ Fig.16 ] is a cross-sectional view showing an overview of a display device involved in one embodiment of the present invention.

[0034] [ Fig.17 ] is a top view showing a pixel electrode and a common electrode of a display device involved in one embodiment of the present invention.

[0035] [ Fig.18 ] is a circuit diagram showing a pixel circuit of a display device according to one embodiment of the present invention.

[0036] [ Fig.19 ] is a cross-sectional view showing an overview of a display device involved in one embodiment of the present invention.

[0037] [ Fig. 20 ] is a diagram showing the measurement results of SIMS analysis in the channel region of the oxide semiconductor layer of a semiconductor device.

[0038] [ Fig.21 ] is a diagram showing the measurement results of SIMS analysis in the source region or drain region of the oxide semiconductor layer of a semiconductor device.

[0039] [ Fig. 22 ] is a diagram showing the electrical characteristics of a semiconductor device.

[0040] [ Fig.23 ] is a diagram showing a reliability test of a semiconductor device. DETAILED DESCRIPTION

[0041] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. While maintaining the gist of the invention, the configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment is of course included in the scope of the present invention. In order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated in the accompanying drawings compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same configuration as that described previously with respect to the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.

[0042] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. On the contrary, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for the sake of convenience, the description is made using the phrases such as up or below, but for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a direction different from that shown in the figure. In the following description, for example, the description of the oxide semiconductor layer on the substrate is merely a description of the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may also be configured between the substrate and the oxide semiconductor layer. Up or down refers to the stacking order in a structure formed by stacking a plurality of layers, and in the case of a pixel electrode described as above the transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as vertically above the transistor, it refers to a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.

[0043] The so-called "display device" refers to a structure that uses an electro-optical layer to display an image. For example, the term display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure in which other optical components (such as polarization components, backlight sources, touch panels, etc.) are installed on the display unit. The "electro-optical layer" may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer as long as no technical contradiction arises. Therefore, in the embodiments described below, as display devices, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified for explanation, but the structure in this embodiment can be applied to a display device including the above-mentioned other electro-optical layers.

[0044] In this specification, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a combination of multiple elements of A to C unless otherwise specified. In addition, these expressions do not exclude the case where α includes other elements.

[0045] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0046] <First embodiment>

[0047] Reference Figures 1 to 12 , a semiconductor device according to an embodiment of the present invention is described. For example, the semiconductor device according to the embodiment described below can be used for an integrated circuit (IC) such as a microprocessor (Micro-Processing Unit: MPU) or a memory circuit in addition to a transistor used in a display device.

[0048] [Configuration of Semiconductor Device 10]

[0049] Reference Figure 1 and Figure 2 The configuration of a semiconductor device 10 according to one embodiment of the present invention will be described. Figure 1 It is a cross-sectional view schematically showing a semiconductor device according to one embodiment of the present invention. Figure 2 It is a plan view schematically showing a semiconductor device according to one embodiment of the present invention.

[0050] like Figure 1As shown, the semiconductor device 10 is provided on a substrate 100. The semiconductor device 10 includes a gate electrode 105, gate insulating layers 110 and 120, an oxide metal layer 130, an oxide semiconductor layer 140, a gate insulating layer 150, a gate electrode 160, insulating layers 170 and 180, a source electrode 201, and a drain electrode 203. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as a source / drain electrode 200.

[0051] The gate electrode 105 is provided on the substrate 100. The gate insulating layer 110 and the gate insulating layer 120 are provided on the substrate 100 and the gate electrode 105. The metal oxide layer 130 is provided on the gate insulating layer 120. The metal oxide layer 130 is in contact with the gate insulating layer 120. The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The oxide semiconductor layer 140 is in contact with the metal oxide layer 130. Among the main surfaces of the oxide semiconductor layer 140, the surface in contact with the metal oxide layer 130 is referred to as a lower surface 142. The end of the metal oxide layer 130 is substantially consistent with the end of the oxide semiconductor layer 140.

[0052] In this embodiment, no semiconductor layer or oxide semiconductor layer is provided between the metal oxide layer 130 and the substrate 100 .

[0053] In this embodiment, the structure in which the metal oxide layer 130 is in contact with the gate insulating layer 120 and the oxide semiconductor layer 140 is in contact with the metal oxide layer 130 is exemplified, but the present invention is not limited to this structure. Another layer may be provided between the gate insulating layer 120 and the metal oxide layer 130. Another layer may also be provided between the metal oxide layer 130 and the oxide semiconductor layer 140.

[0054] exist Figure 1 In the embodiment, the sidewalls of the metal oxide layer 130 and the sidewalls of the oxide semiconductor layer 140 are arranged in a straight line, but the present invention is not limited to this configuration. The angle of the sidewall of the metal oxide layer 130 relative to the main surface of the substrate 100 may be different from the angle of the sidewall of the oxide semiconductor layer 140. The cross-sectional shape of the sidewall of at least one of the metal oxide layer 130 and the oxide semiconductor layer 140 may be curved.

[0055] The gate electrode 160 is opposite to the oxide semiconductor layer 140. The gate insulating layer 150 is provided between the oxide semiconductor layer 140 and the gate electrode 160. The gate insulating layer 150 is in contact with the oxide semiconductor layer 140. Among the main surfaces of the oxide semiconductor layer 140, the surface in contact with the gate insulating layer 150 is referred to as the upper surface 141. The surface between the upper surface 141 and the lower surface 142 is referred to as the side surface 143. The insulating layers 170 and 180 are provided on the gate insulating layer 150 and the gate electrode 160. The insulating layers 170 and 180 are provided with openings 171 and 173 reaching the oxide semiconductor layer 140. The source electrode 201 is provided inside the opening 171. The source electrode 201 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 171. The drain electrode 203 is provided inside the opening 173. The drain electrode 203 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 173.

[0056] The gate electrode 105 has a function as a bottom gate of the semiconductor device 10 and a function as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 110 has a function as a barrier film for shielding impurities diffused from the substrate 100 to the oxide semiconductor layer 140. The gate insulating layers 110 and 120 have a function as a gate insulating layer for the bottom gate. The metal oxide layer 130 is a layer containing a metal oxide mainly composed of aluminum, and has a function as a gas barrier film for shielding gases such as oxygen and hydrogen.

[0057] The oxide semiconductor layer 140 is divided into a source region S, a drain region D, and a channel region CH. The channel region CH is a region vertically below the gate electrode 160 in the oxide semiconductor layer 140. The source region S is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160 and is closer to the source electrode 201 than the channel region CH. The drain region D is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160 and is closer to the drain electrode 203 than the channel region CH. The oxide semiconductor layer 140 in the channel region CH has physical properties as a semiconductor. The oxide semiconductor layer 140 in the source region S and the drain region D has physical properties as a conductor.

[0058] The gate electrode 160 has the function of serving as the top gate of the semiconductor device 10 and as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 150 has the function of serving as a gate insulating layer for the top gate, and has the function of releasing oxygen through heat treatment in the manufacturing process. The insulating layers 170 and 180 insulate the gate electrode 160 from the source / drain electrode 200, and have the function of reducing the parasitic capacitance therebetween. The operation of the semiconductor device 10 is mainly controlled by the voltage supplied to the gate electrode 160. An auxiliary voltage is supplied to the gate electrode 105. However, in the case where the gate electrode 105 is used only as a light shielding film, no specific voltage is supplied to the gate electrode 105, and the gate electrode 105 may also be in a floating state. That is, the gate electrode 105 may also be simply referred to as a "light shielding film".

[0059] In this embodiment, a configuration of a dual-gate transistor in which gate electrodes are provided both above and below an oxide semiconductor layer is exemplified as the semiconductor device 10, but the present invention is not limited to this configuration. For example, a bottom-gate transistor in which a gate electrode is provided only below an oxide semiconductor layer, or a top-gate transistor in which a gate electrode is provided only above an oxide semiconductor layer may be used as the semiconductor device 10. The above configuration is merely one embodiment, and the present invention is not limited to the above configuration.

[0060] like Figure 2 As shown in FIG. 1 , in a plan view, the planar pattern of the metal oxide layer 130 is substantially the same as the planar pattern of the oxide semiconductor layer 140. Figure 1 and Figure 2 , the lower surface 142 of the oxide semiconductor layer 140 is covered by the oxide metal layer 130. In particular, in the present embodiment, the lower surface 142 of the oxide semiconductor layer 140 is entirely covered by the oxide metal layer 130. In the D1 direction, the width of the gate electrode 105 is greater than the width of the gate electrode 160. The D1 direction is a direction connecting the source electrode 201 and the drain electrode 203, and is a direction indicating the channel length L of the semiconductor device 10. Specifically, the length in the D1 direction of the region (channel region CH) where the oxide semiconductor layer 140 overlaps with the gate electrode 160 is the channel length L, and the width in the D2 direction of the channel region CH is the channel width W.

[0061] In this embodiment, a configuration in which the lower surface 142 of the oxide semiconductor layer 140 is entirely covered by the oxidized metal layer 130 is illustrated, but the configuration is not limited thereto. For example, a portion of the lower surface 142 of the oxide semiconductor layer 140 may not be in contact with the oxidized metal layer 130. For example, the lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may be entirely covered by the oxidized metal layer 130, and the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be entirely or partially covered by the oxidized metal layer 130. That is, the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be entirely or partially in contact with the oxidized metal layer 130. However, in the above configuration, a portion of the lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may not be covered by the oxidized metal layer 130, and the other portion of the lower surface 142 may be in contact with the oxidized metal layer 130.

[0062] In this embodiment, a configuration in which the gate insulating layer 150 is formed on the entire surface and the openings 171 and 173 are provided in the gate insulating layer 150 is exemplified, but the present invention is not limited to this configuration. The gate insulating layer 150 may be patterned. For example, the gate insulating layer 150 may be patterned to expose the oxide semiconductor layer 140 in the source region S and the drain region D. That is, the gate insulating layer 150 in the source region S and the drain region D may be removed, and the oxide semiconductor layer 140 and the insulating layer 170 may be in contact with each other in these regions.

[0063] exist Figure 2 , a configuration in which the source / drain electrode 200 does not overlap with the gate electrode 105 and the gate electrode 160 in a plan view is illustrated, but the present invention is not limited to this configuration. For example, in a plan view, the source / drain electrode 200 may overlap with at least one of the gate electrode 105 and the gate electrode 160. The above configuration is merely one embodiment, and the present invention is not limited to the above configuration.

[0064] [Material of Each Component of Semiconductor Device 10]

[0065] As the substrate 100, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate can be used. When the substrate 100 needs to be flexible, a substrate containing resin, such as a polyimide substrate, an acrylic substrate, a siloxane-based substrate, or a fluororesin substrate can be used as the substrate 100. When a substrate containing resin is used as the substrate 100, impurities can be introduced into the resin in order to improve the heat resistance of the substrate 100. In particular, when the semiconductor device 10 is a top-emitting display, since the substrate 100 does not need to be transparent, impurities that reduce the transparency of the substrate 100 can also be used. When the semiconductor device 10 is used in an integrated circuit that is not a display device, as the substrate 100, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, or a compound semiconductor substrate, or a substrate that is not light-transmitting, such as a conductive substrate such as a stainless steel substrate, can be used.

[0066] As the gate electrode 105, the gate electrode 160, and the source / drain electrode 200, a common metal material can be used. For example, as these members, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys thereof or compounds thereof can be used. As the gate electrode 105, the gate electrode 160, and the source / drain electrode 200, the above materials can be used as a single layer or as a stacked layer.

[0067] It should be noted that the gate electrode 160 and the source / drain electrode 200 may be made of the same metal material or different metal materials. For example, the gate electrode 160 may not contain aluminum, while the source / drain electrode 200 may contain aluminum.

[0068] As the gate insulating layers 110, 120 and the insulating layers 170, 180, a common insulating material can be used. For example, silicon oxide (SiO x ), silicon oxide nitride (SiO x N y ), Silicon Nitride (SiN x ), silicon oxide nitride (SiN x O y ), aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ), aluminum nitride (AlN x O y ), aluminum nitride (AlN x ) and other inorganic insulating layers.

[0069] The above SiO x N y and AlOx N y It is a silicon compound and an aluminum compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). x O y and AlN x O y These are silicon compounds and aluminum compounds containing oxygen at a ratio smaller than that of nitrogen (x>y).

[0070] As the gate insulating layer 150, an insulating layer containing oxygen among the above insulating layers can be used. For example, as the gate insulating layer 150, silicon oxide (SiOx), silicon nitride oxide (SiO x N y ) and other inorganic insulating layers.

[0071] An insulating layer having a function of releasing oxygen by heat treatment is used as the gate insulating layer 120. For example, the temperature of the heat treatment for releasing oxygen from the gate insulating layer 120 is 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, for example, when a glass substrate is used as the substrate 100, the gate insulating layer 120 releases oxygen at the heat treatment temperature performed in the manufacturing process of the semiconductor device 10.

[0072] As the gate insulating layer 150, an insulating layer with few defects is used. For example, when the composition ratio of oxygen in the gate insulating layer 150 is compared with the composition ratio of oxygen in an insulating layer having the same composition as the gate insulating layer 150 (hereinafter referred to as "another insulating layer"), the composition ratio of oxygen in the gate insulating layer 150 is closer to the stoichiometric ratio with respect to the insulating layer than the composition ratio of oxygen in the other insulating layer. Specifically, in silicon oxide (SiO x ) is used for each of the gate insulating layer 150 and the insulating layer 180, the composition ratio of oxygen in the silicon oxide used for the gate insulating layer 150 is closer to the stoichiometric ratio of silicon oxide than the composition ratio of oxygen in the silicon oxide used for the insulating layer 180. For example, as the gate insulating layer 150, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) may be used.

[0073] As the metal oxide layer 130 and the metal oxide layer 190 used in the manufacturing process described later, a metal oxide containing aluminum as a main component can be used. For example, aluminum oxide (AlO x ), aluminum oxide nitride (AlO x N y ), aluminum nitride (AlN x O y ), aluminum nitride (AlN x) or the like. “A metal oxide layer mainly composed of aluminum” means that the ratio of aluminum contained in the metal oxide layer 130 (or metal oxide layer 190) is greater than 1% of the total metal oxide layer 130 (or metal oxide layer 190). The ratio of aluminum contained in the metal oxide layer 130 (or metal oxide layer 190) may be greater than 5% and less than 70%, greater than 10% and less than 60%, or greater than 30% and less than 50% of the total metal oxide layer 130. The above ratios may be either mass ratios or weight ratios.

[0074] When the metal oxide layer 190 is formed on the gate insulating layer 150 and an oxidation annealing is performed, the aluminum contained in the metal oxide layer 190 diffuses into the gate insulating layer 150, as described in detail later. Therefore, in the region near the surface of the gate insulating layer 150 (near the surface on the opposite side of the oxide semiconductor layer 140), the diffused aluminum can be detected by, for example, SIMS (Secondary Ion Mass Spectrometry) analysis. In the semiconductor device 10 manufactured by the manufacturing method described later, the aluminum concentration detected in the region below 50 nm from the surface of the gate insulating layer 150 is preferably 1×10 17 atoms / cm 3 Since the metal oxide layer 190 is removed during the manufacturing process, the semiconductor device 10 does not include the metal oxide layer 190. However, since aluminum diffused from the metal oxide layer 190 remains in the gate insulating layer 150, by measuring the aluminum concentration in the gate insulating layer 150, it can be inferred that the semiconductor device 10 is manufactured by the manufacturing method described later. In particular, the aluminum concentration in the gate insulating layer 150 is 1×10 17 atoms / cm 3 In the above case, it can be inferred that oxidation annealing using the oxidized metal layer 190 is effectively performed.

[0075] In addition, since the aluminum remaining in the gate insulating layer 150 is not a main component, the aluminum concentration in the gate insulating layer 150 is at an impurity level. That is, the aluminum concentration in the gate insulating layer 150 is, for example, 1×10 21 atoms / cm 3 Below, preferably 1×10 20 atoms / cm 3 Below, more preferably 1×10 19 atoms / cm 3 the following.

[0076] It should be noted that since aluminum remaining in the gate insulating layer 150 does not degrade electrical characteristics and reliability, the semiconductor device 10 has high mobility and high reliability.

[0077] As the oxide semiconductor layer 140, an oxide metal having semiconductor properties can be used. For example, as the oxide semiconductor layer 140, an oxide semiconductor containing two or more metals including indium (In) can be used. In the oxide semiconductor layer 140, the ratio of indium to the two or more metals is 50% or more. As the oxide semiconductor layer 140, in addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium oxide (Zr), and lanthanide elements can also be used. As the oxide semiconductor layer 140, elements other than the above can also be used.

[0078] The oxide semiconductor layer 140 may be amorphous or crystalline. The oxide semiconductor layer 140 may be a mixed phase of amorphous and crystalline. As described below, in the oxide semiconductor layer 140 where the ratio of indium is 50% or more, oxygen vacancies are easily formed. Crystalline oxide semiconductors are less likely to form oxygen vacancies than amorphous oxide semiconductors. Therefore, the oxide semiconductor layer 140 as described above is preferably crystalline.

[0079] [Problems Newly Recognized in the Process of Implementing the Invention]

[0080] When the ratio of indium in the oxide semiconductor layer 140 is 50% or more, a semiconductor device 10 with high mobility can be realized. On the other hand, in such an oxide semiconductor layer 140 , oxygen contained in the oxide semiconductor layer 140 is easily reduced, so that oxygen vacancies are easily formed in the oxide semiconductor layer 140 .

[0081] In the semiconductor device 10, during the heat treatment process of the manufacturing process, hydrogen is released from a layer (e.g., gate insulating layers 110, 120) disposed closer to the substrate 100 than the oxide semiconductor layer 140. The hydrogen reaches the oxide semiconductor layer 140, thereby causing oxygen vacancies in the oxide semiconductor layer 140. The larger the pattern size of the oxide semiconductor layer 140, the more significant the occurrence of the oxygen vacancies. In order to suppress the occurrence of such oxygen vacancies, it is necessary to suppress hydrogen from reaching the lower surface 142 of the oxide semiconductor layer 140. The above is the first subject.

[0082] In addition to the above-mentioned problems, there is a second problem as shown below. The upper surface 141 of the oxide semiconductor layer 140 is affected by the process (e.g., patterning process or etching process) after forming the oxide semiconductor layer 140. On the other hand, the lower surface 142 of the oxide semiconductor layer 140 (the surface of the oxide semiconductor layer 140 on the substrate 100 side) is not affected by the above-mentioned process.

[0083] Therefore, the oxygen vacancies formed near the upper surface 141 of the oxide semiconductor layer 140 are more than the oxygen vacancies formed near the lower surface 142 of the oxide semiconductor layer 140. That is, the oxygen vacancies in the oxide semiconductor layer 140 are not uniformly present in the thickness direction of the oxide semiconductor layer 140, but are present in a non-uniform distribution in the thickness direction of the oxide semiconductor layer 140. Specifically, the oxygen vacancies in the oxide semiconductor layer 140 are less as they are closer to the lower surface 142 of the oxide semiconductor layer 140, and are more as they are closer to the upper surface 141 of the oxide semiconductor layer 140.

[0084] In the case where the oxide semiconductor layer 140 having the above-mentioned oxygen vacancy distribution is uniformly subjected to oxygen supply treatment, if the amount of oxygen required to repair the oxygen vacancy formed on the upper surface 141 side of the oxide semiconductor layer 140 is supplied, oxygen is excessively supplied to the lower surface 142 side of the oxide semiconductor layer 140. As a result, on the lower surface 142 side, a defect energy level different from that of the oxygen vacancy is formed due to the excess oxygen. As a result, phenomena such as characteristic changes in reliability tests or a decrease in field effect mobility occur. Therefore, in order to suppress this phenomenon, it is necessary to supply oxygen to the upper surface 141 side of the oxide semiconductor layer 140 while suppressing the supply of oxygen to the lower surface 142 side of the oxide semiconductor layer 140.

[0085] The above-mentioned problems are newly recognized problems in the process of realizing the present invention, rather than problems that have been recognized in the past. In the existing structure and manufacturing method, even if the initial characteristics of the semiconductor device are improved by oxygen supply treatment of the oxide semiconductor layer, characteristic changes caused by reliability tests will occur, and there is a trade-off relationship between the initial characteristics and the reliability test. However, according to the structure involved in this embodiment, the above-mentioned problems can be solved, and good initial characteristics and reliability tests of the semiconductor device 10 can be obtained.

[0086] [Method of Manufacturing Semiconductor Device 10]

[0087] Reference Figure 3 to Figure 12 , a method for manufacturing a semiconductor device according to an embodiment of the present invention is described. Figure 3 It is a flowchart showing a method for manufacturing a semiconductor device according to one embodiment of the present invention. Figures 4 to 12 This is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. In the following description of the manufacturing method, a method for manufacturing the semiconductor device 10 using aluminum oxide as the metal oxide layers 130 and 190 will be described.

[0088] like Figure 3 and Figure 4As shown, a gate electrode 105 is formed on the substrate 100 as a bottom gate, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Figure 3 The bottom GI / GE is formed in step S2001. For example, silicon nitride is formed as the gate insulating layer 110. For example, silicon oxide is formed as the gate insulating layer 120. The gate insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition). Sometimes, one or both of the gate insulating layers 110 and 120 are referred to as the "first insulating layer".

[0089] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 side toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.

[0090] like Figure 3 and Figure 5 As shown, a metal oxide layer 130 and an oxide semiconductor layer 140 are formed on the gate insulating layer 120 ( Figure 3 In this process, gate insulating layers 110 and 120 are sometimes formed on the substrate 100, and a metal oxide layer 130 is formed on the gate insulating layers 110 and 120. Alternatively, a metal oxide layer 130 is sometimes formed on the substrate 100, and an oxide semiconductor layer 140 is formed on the metal oxide layer 130. Specifically, the oxide semiconductor layer 140 is formed in contact with the metal oxide layer 130. The metal oxide layer 130 and the oxide semiconductor layer 140 are formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).

[0091] For example, the thickness of the metal oxide layer 130 is 1 nm to 100 nm, 1 nm to 50 nm, 1 nm to 30 nm, or 1 nm to 10 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has a high barrier property against gas. In this embodiment, aluminum oxide used as the metal oxide layer 130 blocks hydrogen and oxygen released from the gate insulating layer 120, and inhibits the released hydrogen and oxygen from reaching the oxide semiconductor layer 140.

[0092] For example, the thickness of the oxide semiconductor layer 140 is greater than or equal to 10 nm and less than or equal to 100 nm, greater than or equal to 15 nm and less than or equal to 70 nm, or greater than or equal to 20 nm and less than or equal to 40 nm. In this embodiment, an oxide containing indium (In) and gallium (Ga) is used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 before the heat treatment (OS annealing) described later is amorphous.

[0093] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, it is preferable that the oxide semiconductor layer 140 after film formation and before OS annealing is in an amorphous state (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 immediately after film formation is as little crystallized as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed while controlling the temperature of the film formation object (the substrate 100 and the structure formed thereon).

[0094] If a film is formed on the film-forming object by sputtering, the ions generated in the plasma and the atoms recoiled by the sputtering target collide with the film-forming object. Therefore, as the film is formed, the temperature of the film-forming object rises. If the temperature of the film-forming object rises during the film-forming process, the oxide semiconductor layer 140 contains microcrystals in the state just after the film is formed. The crystallization caused by the subsequent OS annealing is hindered by the microcrystals. As described above, in order to control the temperature of the film-forming object, for example, the film can be formed while the film is cooled. For example, the film-forming object can be cooled from the surface opposite to the film-forming surface in such a manner that the temperature of the film-forming surface (surface) of the film-forming object (hereinafter referred to as "film-forming temperature") is below 100°C, below 70°C, below 50°C or below 30°C. As described above, by forming the oxide semiconductor layer 140 while cooling the film-forming object, the oxide semiconductor layer 140 with a small crystalline component can be formed in the state just after the film is formed.

[0095] like Figure 3 and Figure 6 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Figure 3 (“OS pattern formation” in step S2003 of FIG. 1 ) Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask. The oxide semiconductor layer 140 may be etched by wet etching or dry etching. As wet etching, an acidic etchant may be used for etching. For example, oxalic acid or hydrofluoric acid may be used as the etchant.

[0096] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Figure 3 In the present embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing.

[0097] like Figure 3 and Figure 7 As shown, the pattern of the oxidized metal layer 130 is formed ( Figure 3 The oxide semiconductor layer 140 patterned in the above process is used as a mask to etch the oxidized metal layer 130. As the etching of the oxidized metal layer 130, wet etching can be used, or dry etching can be used. For example, as wet etching, diluted hydrofluoric acid (DHF) can be used. As described above, by etching the oxidized metal layer 130 using the oxide semiconductor layer 140 as a mask, the photolithography process can be omitted.

[0098] like Figure 3 and Figure 8 As shown, a gate insulating layer 150 is formed on the oxide semiconductor layer 140 ( Figure 3 The gate insulating layer 150 is formed by a CVD method. For example, in order to form the above-mentioned insulating layer with few defects as the gate insulating layer 150, the gate insulating layer 150 may be formed at a film forming temperature of 350°C or higher. For example, the thickness of the gate insulating layer 150 is between 50nm and 300nm, between 60nm and 200nm, or between 70nm and 150nm. After the gate insulating layer 150 is formed, a process of injecting oxygen into a portion of the gate insulating layer 150 may be performed. The gate insulating layer 150 is sometimes referred to as a "second insulating layer". A metal oxide layer 190 is formed on the gate insulating layer 150 ( Fig. 22 The metal oxide layer 190 is formed by a sputtering method. Oxygen is injected into the gate insulating layer 150 by the formation of the metal oxide layer 190.

[0099] For example, the thickness of the metal oxide layer 190 is 5 nm to 100 nm, 5 nm to 50 nm, 5 nm to 30 nm, or 7 nm to 15 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 190. Aluminum oxide has a high barrier property against gas. In this embodiment, aluminum oxide used as the metal oxide layer 190 suppresses the outward diffusion of oxygen injected into the gate insulating layer 150 when the metal oxide layer 190 is formed.

[0100] For example, when the metal oxide layer 190 is formed by sputtering, the process gas used in sputtering may remain in the film of the metal oxide layer 190. For example, when Ar is used as the process gas for sputtering, Ar may remain in the film of the metal oxide layer 190. The remaining Ar can be detected by SIMS analysis of the metal oxide layer 190.

[0101] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140 and the metal oxide layer 190 is formed on the gate insulating layer 150, a heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Figure 3 In other words, the metal oxide layer 130 and the oxide semiconductor layer 140 patterned as described above are subjected to heat treatment (oxidation annealing). In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Through the above-mentioned oxidation annealing, the oxygen released from the gate insulating layers 120 and 150 is supplied to the oxide semiconductor layer 140, and the oxygen vacancies are repaired.

[0102] Oxygen released from the gate insulating layer 120 by the oxidation annealing is blocked by the oxidized metal layer 130. Therefore, it is not easy to supply oxygen to the lower surface 142 of the oxide semiconductor layer 140. The oxygen released from the gate insulating layer 120 diffuses from the region where the oxidized metal layer 130 is not formed to the gate insulating layer 150 provided on the gate insulating layer 120, and reaches the oxide semiconductor layer 140 through the gate insulating layer 150. As a result, the oxygen released from the gate insulating layer 120 is not easily supplied to the lower surface 142 of the oxide semiconductor layer 140, but is mainly supplied to the side surface 143 and the upper surface 141 of the oxide semiconductor layer 140. In addition, by the oxidation annealing, the oxygen released from the gate insulating layer 150 is supplied to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. By the above-mentioned oxidation annealing, hydrogen is sometimes released from the gate insulating layers 110 and 120, but the hydrogen is blocked by the oxidized metal layer 130.

[0103] As described above, the oxidation annealing step can suppress supply of oxygen to the lower surface 142 of the oxide semiconductor layer 140 having a small amount of oxygen vacancies, and can supply oxygen to the upper surface 141 and side surfaces 143 of the oxide semiconductor layer 140 having a large amount of oxygen vacancies.

[0104] Similarly, in the oxidation annealing, oxygen injected into the gate insulating layer 150 is blocked by the oxidized metal layer 190. Therefore, it is possible to suppress the oxygen from being released into the atmosphere. Therefore, through the oxidation annealing, the oxygen is efficiently supplied to the oxide semiconductor layer 140, and the oxygen deficiency is repaired.

[0105] like Figure 3 and Fig. 9 As shown, after the oxidation annealing, the oxide metal layer 190 is etched (removed) ( Figure 3 As for etching of the metal oxide layer 190, wet etching or dry etching can be used. For example, as wet etching, diluted hydrofluoric acid (DHF) can be used. By this etching, the metal oxide layer 190 formed on the entire surface is removed. In other words, the removal of the metal oxide layer 190 is performed without using a mask. In other words, by this etching, at least when viewed from above, the entire metal oxide layer 190 in the area overlapping with the oxide semiconductor layer 140 formed into a certain pattern is removed.

[0106] When the oxidation annealing is performed, aluminum contained in the oxidized metal layer 190 diffuses into the gate insulating layer 150. Therefore, even if the oxidized metal layer 190 is removed, aluminum diffused from the oxidized metal layer 190 remains in the gate insulating layer 150.

[0107] like Figure 3 and Fig.10 As shown, a gate electrode 160 is formed on the gate insulating layer 150 ( Figure 3 The gate electrode 160 is formed by sputtering or atomic layer deposition and patterned by photolithography. As described above, the gate electrode 160 is formed to contact the gate insulating layer 150 exposed by removing the oxidized metal layer 190.

[0108] When etching the gate electrode 160, a portion of the gate insulating layer 150 is sometimes also etched. That is, the gate insulating layer 150 includes regions with different film thicknesses. Specifically, the gate insulating layer 150 includes a first region overlapping with the gate electrode 160 and a second region not overlapping with the gate electrode 160. The first region overlaps with the channel region CH of the oxide semiconductor layer 140. The second region overlaps with the source region S or the drain region D of the oxide semiconductor layer 140. The film thickness of the second region is smaller than that of the first region. In this case, in the second region, since a portion of the region containing aluminum diffused from the metal oxide layer 190 is etched, even if the aluminum concentration in the first region is 1×10 17 atoms / cm 3 As described above, the aluminum concentration in the second region is also lower than the aluminum concentration in the first region.

[0109] In the state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Figure 3Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. For example, argon (Ar), phosphorus (P), and boron (B) are implanted into the oxide semiconductor layer 140 by ion implantation. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the semiconductor device 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.

[0110] like Figure 3 and Fig.11 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Figure 3 The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used for the insulating layers 170 and 180 are not limited to the above materials. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.

[0111] like Figure 3 and Fig.12 As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Figure 3 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrode 200 is formed on the oxide semiconductor layer 140 exposed through the openings 171 and 173 and on the insulating layer 180 ( Figure 3 Step S2014 of "SD formation"), thereby completing Figure 1 A semiconductor device 10 is shown.

[0112] The semiconductor device 10 manufactured by the above manufacturing method can obtain a mobility of 50 cm-1 within the range where the channel length L of the channel region CH is 2 μm to 4 μm and the channel width of the channel region CH is 2 μm to 25 μm. 2 / Vs or above, 55cm 2 / Vs or above or 60cm 2 / Vs or more electrical characteristics. The mobility in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10. Specifically, the mobility refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the semiconductor device 10 from the voltage (Vg) supplied to the gate electrode.

[0113] <Second embodiment>

[0114] Reference Figure 13 to Figure 17 In the following embodiment, a display device using a semiconductor device according to an embodiment of the present invention is described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device is described.

[0115] [Overview of Display Device 20]

[0116] Fig.13 FIG. 1 is a top view showing an overview of a display device according to an embodiment of the present invention. Fig.13 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. In the liquid crystal region 22 surrounded by the sealing portion 310, a plurality of pixel circuits 301 are arranged in a matrix. The liquid crystal region 22 is a region that overlaps with a liquid crystal element 311 described later in a plan view.

[0117] The sealing region 24 provided with the sealing portion 310 is the region around the liquid crystal region 22. The FPC 330 is provided in the terminal region 26. The terminal region 26 is the region where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 24. The outside of the sealing region 24 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.

[0118] [Circuit Configuration of Display Device 20]

[0119] Fig.14 FIG. 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. Fig.14As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 22 where the pixel circuit 301 is configured along the D1 direction (column direction), and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the D2 direction (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 24. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 24, and any region may be provided as long as it is outside the region where the pixel circuit 301 is provided.

[0120] The source wiring 304 extends from the source driving circuit 302 in the direction D1 and is connected to the plurality of pixel circuits 301 arranged in the direction D1. The gate wiring 305 extends from the gate driving circuit 303 in the direction D2 and is connected to the plurality of pixel circuits 301 arranged in the direction D2.

[0121] The terminal region 26 is provided with a terminal portion 306. The terminal portion 306 and the source driver circuit 302 are connected by a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected by the connection wiring 307. The FPC 330 is connected to the terminal portion 306, so that an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0122] The semiconductor device 10 described in the first embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .

[0123] [Pixel Circuit 301 of Display Device 20]

[0124] Fig.15 FIG. 2 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.15 As shown, the pixel circuit 301 includes a semiconductor device 10, a holding capacitor 350, and a liquid crystal element 311. The semiconductor device 10 has a gate electrode 160, a source electrode 201, and a drain electrode 203. The gate electrode 160 is connected to the gate wiring 305. The source electrode 201 is connected to the source wiring 304. The drain electrode 203 is connected to the holding capacitor 350 and the liquid crystal element 311. In this embodiment, for the sake of convenience, the electrode shown by the reference numeral "201" is called a source electrode, and the electrode shown by the reference numeral "203" is called a drain electrode, but the electrode shown by the reference numeral "201" may function as a drain electrode, and the electrode shown by the reference numeral "203" may function as a source electrode.

[0125] [Cross-sectional structure of display device 20]

[0126] Fig.16 FIG. 1 is a cross-sectional view of a display device according to an embodiment of the present invention. Fig.16 As shown in FIG. 1 , the display device 20 is a display device using the semiconductor device 10. In this embodiment, the semiconductor device 10 is used in the pixel circuit 301, but the semiconductor device 10 can also be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303. In the following description, the semiconductor device 10 is used in the pixel circuit 301. Figure 1 The semiconductor devices 10 shown are the same, and therefore description thereof will be omitted.

[0127] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 provided in common to a plurality of pixels is provided on the insulating layer 360. An insulating layer 380 is provided on the common electrode 370. An opening 381 is provided in the insulating layers 360 and 380. A pixel electrode 390 is provided on the insulating layer 380 and in the opening 381. The pixel electrode 390 is connected to the drain electrode 203.

[0128] In the display device 20, a wiring layer 162 is provided as the same layer as the gate electrode 160. The wiring layer 162 is made of the same material as the gate electrode 160. The wiring layer 162 is provided on an insulating layer corresponding to the gate insulating layer 150. The oxidized metal layer 190 is also formed on the insulating layer and oxidized annealed. Therefore, the aluminum concentration of the region of the insulating layer overlapping the wiring layer 162 is preferably 1×10 17 atoms / cm 3 In addition, the aluminum concentration in a region of the insulating layer that does not overlap with the wiring layer 162 is lower than the aluminum concentration in a region of the insulating layer that overlaps with the wiring layer 162 .

[0129] Fig.17 FIG. 1 is a top view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention. Fig.17 As shown, the common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 in a plan view, and a non-overlapping region that does not overlap with the pixel electrode 390. If a voltage is supplied between the pixel electrode 390 and the common electrode 370, a transverse electric field is formed from the pixel electrode 390 in the overlapping region toward the common electrode 370 in the non-overlapping region. The liquid crystal molecules included in the liquid crystal element 311 are moved by the transverse electric field, thereby determining the grayscale of the pixel.

[0130] <Third embodiment>

[0131] Reference Fig.18 and Fig.19, a display device using a semiconductor device according to an embodiment of the present invention is described. In this embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to an organic EL display device is described. The overview and circuit configuration of the display device 20 are similar to Fig.13 and Fig.14 The outline and structure shown are the same, so the description is omitted.

[0132] [Pixel Circuit 301 of Display Device 20]

[0133] Fig.18 FIG. 2 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.18 As shown, the pixel circuit 301 includes components such as a driving transistor 11, a selection transistor 12, a holding capacitor 210 and a light-emitting element DO. The driving transistor 11 and the selection transistor 12 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 12 is connected to the signal line 211, and the gate electrode of the selection transistor 12 is connected to the gate line 212. The source electrode of the driving transistor 11 is connected to the anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 11 is connected to the drain electrode of the selection transistor 12. The holding capacitor 210 is connected to the gate electrode and the drain electrode of the driving transistor 11. A grayscale signal that determines the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row in which the grayscale signal is written is supplied to the gate line 212.

[0134] [Cross-sectional structure of display device 20]

[0135] Fig.19 This is a cross-sectional view of a display device according to one embodiment of the present invention. Fig.19 The display device 20 shown in FIG. Fig.16 The display device 20 shown is similar, but Fig.19 The structure of the display device 20 above the insulating layer 360 and Fig.16 The structure of the display device 20 above the insulating layer 360 is different. Fig.19 In the configuration of the display device 20, Fig.16 The description of the same structure as the display device 20 is omitted, and the differences between the two are described.

[0136] like Fig.19As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 (light-emitting element DO) above the insulating layer 360. The pixel electrode 390 is arranged on the insulating layer 360 and inside the opening 381. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. In other words, the insulating layer 362 divides the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are respectively arranged for each pixel. On the other hand, the common electrode 394 is commonly arranged for a plurality of pixels. The light-emitting layer 392 uses different materials depending on the display color of the pixel.

[0137] In the second and third embodiments, the semiconductor device described in the first embodiment is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device can also be applied to other display devices other than these display devices (for example, a self-luminous display device or an electronic paper display device other than an organic EL display device). In addition, the semiconductor device can be applied to a variety of display devices from small to medium-sized to large display devices without particular limitation.

[0138] Example

[0139] As an example, the semiconductor device 10 described in the first embodiment was manufactured and evaluated. Furthermore, as a comparative example, a semiconductor device in which the metal oxide layer 130 in contact with the oxide semiconductor layer 140 was not provided was manufactured.

[0140] Furthermore, in the embodiment, before forming the gate electrode GE, an aluminum oxide layer is formed by sputtering as the metal oxide layer 190, and the aluminum oxide layer is removed after oxidation annealing. On the other hand, in the comparative example, the metal oxide layer 190 is not formed and the oxidation annealing is not performed.

[0141] [1.SIMS analysis]

[0142] Fig. 20 : is a diagram showing the measurement results of SIMS analysis in the channel region of the oxide semiconductor layer of the semiconductor device. Fig.21 : is a diagram showing the measurement results of SIMS analysis in the source region or drain region of the oxide semiconductor layer of the semiconductor device. Fig. 20 and Fig.21 In FIG. 1 , the vertical axis represents the aluminum concentration (Al concentration), and the horizontal axis represents the depth in the stacking direction of the semiconductor device. Fig. 20 and Fig.211 and 2 show the stacking structures of the embodiments and comparative examples in the stacking direction. The reference numerals SiNx, SiOx, GI, GE, OS and MO represent a silicon nitride layer, a silicon oxide layer, a gate insulating layer, a gate electrode, an oxide semiconductor layer and a metal oxide layer, respectively. The silicon nitride layer SiNx and the silicon oxide layer SiOx in contact with the silicon oxide layer SiOx correspond to the gate insulating layers 110 and 120, respectively. The metal oxide layer MO, the oxide semiconductor layer OS, the gate insulating layer GI and the gate electrode GE correspond to the metal oxide layer 130, the oxide semiconductor layer 140, the gate insulating layer 150 and the gate electrode 160, respectively. It should be noted that, similarly to the silicon oxide layer SiOx, silicon oxide is used for the gate insulating layer GI.

[0143] SIMS analysis uses so-called SSDP-SIMS that measures from the substrate side. Fig. 20 and Fig.21 In the example, the SiO2 standard sample is used to quantify the aluminum concentration in the silicon oxide layer SiOx and the gate insulating layer GI (quantitative range in the figure). Fig. 20 and Fig.21 In the embodiment, the aluminum concentrations in the silicon oxide layer SiOx and the gate insulating layer GI can be compared by absolute values. On the other hand, the aluminum concentrations in other layers can be compared by magnitude, but cannot be compared by absolute values.

[0144] like Fig. 20 As shown in FIG. 1 , in the channel region, the aluminum concentration of the gate insulating layer GI of the embodiment (solid line) is higher than that of the gate insulating layer GI of the comparative example (dashed line). Near the interface between the gate electrode GE and the gate insulating layer GI, the aluminum concentrations of the gate insulating layer GI of the embodiment and the comparative example are 2×10 17 atoms / cm 3 and 6×10 16 atoms / cm 3 In addition, if Fig.21 As shown in FIG. 1 , in the source region or the drain region, the aluminum concentration of the gate insulating layer GI of the embodiment is also higher than that of the gate insulating layer GI of the comparative example. Near the interface between the silicon nitride layer SiNx and the gate insulating layer GI, the aluminum concentrations of the gate insulating layer GI of the embodiment and the comparative example are 1.5×10 17 atoms / cm 3 and 6×10 16 atoms / cm 3 Therefore, in the embodiment, aluminum in aluminum oxide formed as the metal oxide layer 190 is diffused into the gate insulating layer GI by the heat treatment of oxidation annealing.

[0145] [2. Electrical characteristics]

[0146] Fig. 22It is a diagram showing the electrical characteristics of the semiconductor device 10 . Fig. 22 The measurement conditions of the electrical characteristics are shown in Table 1.

[0147] [Table 1]

[0148] The size of the channel area W / L=3.0μm / 3.0μm Source-drain voltage 0.1V (dashed line), 10V (solid line) Gate voltage -15V~+15V Measurement environment room temperature, dark room

[0149] Fig. 22 The electrical characteristics (Id-Vg characteristics) and mobility of the semiconductor device 10 are shown in FIG. Fig. 22 As shown by the arrow in , the vertical axis for the drain current (Id) is shown on the left side of the figure, and the vertical axis for the mobility calculated based on the drain current is shown on the right side of the figure.

[0150] like Fig. 22 As shown, the electrical characteristics of the semiconductor device 10 show so-called normally off (enhancement mode) characteristics in which the drain current Id starts to flow when the gate voltage Vg is higher than 0 V. The mobility calculated from the electrical characteristics is about 59 cm 2 / Vs.

[0151] [3. Reliability test]

[0152] Fig.23 1 is a diagram showing a reliability test of the semiconductor device 10 . Fig.23 The measurement conditions of the reliability test are shown in Table 2. That is, as the reliability test, reliability evaluation using Positive Bias Temperature Stress (PBTS) and Negative Bias Temperature Illumination Stress (NBTIS) was performed.

[0153] [Table 2]

[0154]

[0155] like Fig.23 As shown in FIG. 1 , the results of evaluating the electrical characteristics of the semiconductor device 1 v before stress application (0 seconds (sec)) and after stress application (3600 seconds) are overlapped and shown. Fig.23 In FIG. 1 , the electrical characteristics before stress application (0 seconds) are represented by a dotted line, and the electrical characteristics after stress application (3600 seconds) are represented by a solid line.

[0156] Table 3 shows the measurement conditions of the electrical characteristics of the semiconductor device 10 before and after stress application.

[0157] [Table 3]

[0158] The size of the channel area W / L=3.oμm / 3.0μm Source-drain voltage 0.1V, 10V Gate voltage -15V~+15V Measurement environment 60℃, dark room

[0159] like Fig.23 As shown, in the semiconductor device 10 , the electrical characteristics before and after stress application hardly change in the NBTIS test and the PBTS test.

[0160] As described above, from the electrical characteristics and reliability tests of the semiconductor device 10, it can be seen that the semiconductor device 10 not only has high mobility but also has stable reliability. Such a semiconductor device 10 having high mobility and high reliability can be obtained by crystallizing the oxide semiconductor layer 140 and supplying sufficient oxygen to the oxide semiconductor layer 140. Therefore, in the manufacturing method of the semiconductor device 10, OS annealing and oxidation annealing are important. In particular, in the oxidation annealing, the oxide metal layer 130 is provided below the oxide semiconductor layer 140, and then the oxide metal layer 190 is heat-treated in a film-forming state on the gate insulating layer 150. The oxide metal layers 130 and 190 can prevent hydrogen from invading the oxide semiconductor layer 140. In addition, the side surfaces 143 and the upper surface 141 of the oxide semiconductor layer 140 are in contact with the gate insulating layer 150 , and oxygen from the gate insulating layer 150 is efficiently supplied to the side surfaces 143 and the upper surface 141 of the oxide semiconductor layer 140 having a large amount of oxygen deficiencies, thereby being able to repair the oxygen deficiencies in the oxide semiconductor layer 140 .

[0161] The oxidized metal layer 190 is removed in the subsequent AlOx removal process, but the aluminum contained in the oxidized metal layer 190 diffuses into the gate insulating layer 150 through oxidation annealing and remains. Therefore, aluminum can be detected by analyzing the composition of the gate insulating layer 150 of the manufactured semiconductor device 10. Fig. 22 and Fig.23 As can be understood from the diagram, the aluminum remaining in the gate insulating layer 150 does not degrade the electrical characteristics and reliability.

[0162] As the embodiments of the present invention, the embodiments described above can be appropriately combined and implemented as long as they are not contradictory. In addition, based on the embodiments, the scheme obtained by the technicians in this field by appropriately adding, deleting or changing the design of the components, or the scheme obtained by adding, omitting or changing the conditions of the process, as long as they have the gist of the present invention, is included in the scope of the present invention.

[0163] Even if there are other effects different from the effects brought about by the above-mentioned embodiments, it can be understood that the effects that are clear from the description of this specification or the effects that can be easily predicted by those skilled in the art are the effects brought about by the present invention.

[0164] Description of Reference Numerals

[0165] 10: semiconductor device, 11: driving transistor, 12: selecting transistor, 20: display device, 22: liquid crystal region, 24: sealing region, 26: terminal region, 100: substrate, 105, 160: gate electrode, 110, 120, 150: gate insulating layer, 130, 190: oxide metal layer, 140: oxide semiconductor layer, 141: upper surface, 142: lower surface, 143: side surface, 162: wiring layer, 170, 180: insulating layer, 171, 173: opening, 200: source / drain electrode, 201: source electrode, 203: drain electrode, 210: holding capacitor, 211: signal line, 212: gate line, 21 3: anode power line, 214: cathode power line, 220: resist mask, 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connection wiring, 310: sealing portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate (FPC), 340: IC chip, 350: holding capacitor, 360, 362: insulating layer, 363, 381: opening, 370: common electrode, 380: insulating layer, 390: pixel electrode, 392: light-emitting layer, 394: common electrode

Claims

1. A semiconductor device comprising: an oxidized metal layer above an insulating surface; an oxide semiconductor layer on the oxide metal layer; and an insulating layer on the oxide semiconductor layer, in, The insulating layer includes a first region overlapping with the oxide semiconductor layer, The first aluminum concentration of the first region is 1×10 17 atoms / cm 3 above.

2. The semiconductor device according to claim 1, wherein: The first region is a region that is 50 nm or less from the surface of the insulating layer located on the opposite side to the oxide semiconductor layer.

3. The semiconductor device according to claim 1 or 2, further comprising a gate electrode on the insulating layer, The first region overlaps with the gate electrode.

4. The semiconductor device according to claim 3, wherein: The insulating layer further includes a second region that does not overlap with the gate electrode. A second aluminum concentration in the second region is lower than the first aluminum concentration.

5. The semiconductor device according to claim 3 or 4, further comprising a wiring layer provided on the insulating layer as the same layer as the gate electrode, The insulating layer includes a third region overlapping the wiring layer, The third aluminum concentration of the third region is 1×10 17 atoms / cm 3 above.

6. The semiconductor device according to any one of claims 3 to 5, wherein: The gate electrode does not contain aluminum.

7. The semiconductor device according to any one of claims 1 to 6, wherein: The metal oxide layer includes aluminum oxide.