Semiconductor device and method for manufacturing semiconductor device

By forming an aluminum oxide metal layer in a semiconductor device and performing planarization treatment, combined with oxidation annealing technology, the problems of defects in the insulating layer and oxygen deficiency in the oxide semiconductor layer are solved, and a semiconductor device with high reliability and high mobility is achieved.

CN118872076APending Publication Date: 2024-10-29JAPAN DISPLAY INC +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380028097.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-14
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The insulating layer formed under conditions containing more oxygen is prone to defects, which affects the reliability and characteristics of the semiconductor device. When the indium ratio in the oxide semiconductor layer is increased to increase mobility, oxygen defects are easily formed, making it difficult to maintain high reliability and high mobility.

Method used

By forming an oxide metal layer mainly composed of aluminum on the insulating surface, and performing planarization treatment to form an oxide semiconductor layer and a gate insulating layer, the supply of oxygen is controlled during the oxidation annealing process to ensure the flatness of the oxide semiconductor layer. and few defects.

Benefits of technology

Semiconductor devices that achieve high reliability and high field-effect mobility improve the flatness of the oxide metal layer through planarization to ensure the consistency of crystal growth of the oxide semiconductor layer, thereby improving mobility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872076A_ABST
    Figure CN118872076A_ABST
Patent Text Reader

Abstract

In a method for manufacturing a semiconductor device, an oxide metal layer having aluminum as a main component is formed on an insulating surface, a surface of the oxide metal layer is planarized, an oxide semiconductor layer is formed on the planarized surface, a gate insulating layer is formed on the oxide semiconductor layer, and a gate electrode is formed on the gate insulating layer. A gate electrode facing the oxide semiconductor layer is formed over the gate insulating layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device and a method for manufacturing the semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor as a channel and a method for manufacturing the semiconductor device. Background Art

[0002] In recent years, the development of semiconductor devices that use oxide semiconductors for channels instead of amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon has been continuously developed (for example, Patent Documents 1 to 6). Semiconductor devices that use oxide semiconductors in channels can be formed with simple structures and low-temperature processes, just like semiconductor devices that use amorphous silicon in channels. It is known that semiconductor devices that use oxide semiconductors in channels have higher mobility than semiconductor devices that use amorphous silicon in channels.

[0003] In order to make a semiconductor device using an oxide semiconductor in a channel operate stably, it is important to supply oxygen to the oxide semiconductor layer in its manufacturing process to reduce oxygen vacancies formed in the oxide semiconductor layer. For example, as one method of supplying oxygen to the oxide semiconductor layer, a technique of forming an insulating layer covering the oxide semiconductor layer under the condition that the insulating layer contains more oxygen is disclosed.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0007] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0008] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0009] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0010] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0011] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0012] Problems to be solved by the invention

[0013] However, the insulating layer formed under the condition of containing more oxygen will contain many defects. Under its influence, it is believed that the characteristics of the semiconductor device are abnormal due to the capture of electrons in the defects or the characteristics of the reliability test are changed. On the other hand, if an insulating layer with fewer defects is used, it is impossible to increase the oxygen contained in the insulating layer. Therefore, it is impossible to fully supply oxygen from the insulating layer to the oxide semiconductor layer. In this way, it is required to realize a structure that can reduce the defects in the insulating layer that cause the characteristics of the semiconductor device to change and at the same time repair the oxygen deficiency formed in the oxide semiconductor layer.

[0014] In addition, by relatively increasing the ratio of indium contained in the oxide semiconductor layer, a semiconductor device with high mobility can be obtained. However, when the ratio of indium contained in the oxide semiconductor layer is high, oxygen vacancies are easily formed in the oxide semiconductor layer. Therefore, in order to achieve high mobility while maintaining high reliability, it is necessary to work on the structure of the insulating layer around the oxide semiconductor layer.

[0015] An object of one embodiment of the present invention is to realize a semiconductor device having high reliability and high mobility.

[0016] Means for solving problems

[0017] In a method for manufacturing a semiconductor device involved in one embodiment of the present invention, a metal oxide layer mainly composed of aluminum is formed on an insulating surface, the surface of the metal oxide layer is planarized, an oxide semiconductor layer is formed on the planarized surface, a gate insulating layer is formed on the oxide semiconductor layer, and a gate electrode opposite to the oxide semiconductor layer is formed on the gate insulating layer.

[0018] A semiconductor device according to an embodiment of the present invention comprises: an oxide metal layer mainly composed of aluminum provided on an insulating surface; an oxide semiconductor layer provided on the oxide metal layer; a gate electrode opposed to the oxide semiconductor layer; and a gate insulating layer between the oxide semiconductor layer and the gate electrode, wherein the field effect mobility μ(cm 2 The relationship between the arithmetic mean roughness Ra (nm) of the oxidized metal layer is expressed by the following formula:

[0019] μ=-10.033Ra+48.23

[0020] (Among them, the arithmetic mean roughness Ra≤0.80nm). BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention.

[0022] Figure 2It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.

[0023] Figure 3 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0024] Figure 4 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0025] Figure 5 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0026] Figure 6 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0027] Figure 7 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0028] Figure 8 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0029] Fig. 9 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0030] Fig.10 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0031] Fig.11 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0032] Fig.12 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0033] Fig.13 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0034] Fig.14 It is a timing chart showing a method for manufacturing a semiconductor device according to a modification of one embodiment of the present invention.

[0035] Fig.15 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modification example of one embodiment of the present invention.

[0036] Fig.16It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modification example of one embodiment of the present invention.

[0037] Fig.17 It is a cross-sectional view schematically showing a semiconductor device according to a modified example of one embodiment of the present invention.

[0038] Fig.18 It is a timing chart showing a method for manufacturing a semiconductor device according to a modification of one embodiment of the present invention.

[0039] Fig.19 It is a cross-sectional view schematically showing a semiconductor device according to a modified example of one embodiment of the present invention.

[0040] Fig. 20 It is a plan view schematically showing a semiconductor device according to a modified example of one embodiment of the present invention.

[0041] Fig.21 It is a timing chart showing a method for manufacturing a semiconductor device according to a modification of one embodiment of the present invention.

[0042] Fig. 22 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modification example of one embodiment of the present invention.

[0043] Fig.23 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modification example of one embodiment of the present invention.

[0044] Fig.24 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0045] Fig.25 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0046] Fig.26 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0047] Fig. 27 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0048] Fig.28 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0049] Fig.29 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0050] Fig.30It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0051] Fig.31 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0052] Fig.32 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0053] Fig.33 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0054] Fig.34 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0055] Fig.35 It is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0056] Fig.36 It is a plan view schematically showing a display device according to one embodiment of the present invention.

[0057] Fig.37 This is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention.

[0058] Fig.38 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0059] Fig.39 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.

[0060] Fig.40 It is a plan view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention.

[0061] Fig.41 : is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention.

[0062] Fig.42 It is a cross-sectional view schematically showing a display device according to an embodiment of the present invention.

[0063] Fig.43 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0064] Fig.44 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0065] Fig.45 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0066] Fig.46 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0067] Fig.47 This is a diagram showing a box plot illustrating the variation in field-effect mobility of the semiconductor device according to the embodiment of the present invention.

[0068] Fig.48 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0069] Fig.49 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0070] Fig.50 This is a diagram showing the electrical characteristics of a semiconductor device according to an embodiment of the present invention.

[0071] Fig.51 This is a diagram showing a box plot illustrating the variation in field-effect mobility of the semiconductor device according to the embodiment of the present invention.

[0072] Fig.52A This is an AFM observation image of the aluminum oxide layer obtained by the planarization process (condition 1).

[0073] Fig.52B This is an AFM observation image of the aluminum oxide layer obtained by the flattening process (condition 2).

[0074] Fig.53 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (condition 1) and the field effect mobility of the semiconductor device.

[0075] Fig.54 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (condition 2) and the field effect mobility of the semiconductor device.

[0076] Fig.55 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (conditions 1 and 2) and the field effect mobility of the semiconductor device. DETAILED DESCRIPTION

[0077] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. The configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment while maintaining the gist of the invention is of course included in the scope of the present invention. With respect to the accompanying drawings, in order to make the description clearer, the width, thickness, shape, etc. of each part are sometimes schematically indicated compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and each figure, the same figure mark is marked for the same configuration as that described in the accompanying drawings that have appeared, and the detailed description is sometimes appropriately omitted.

[0078] The so-called "semiconductor device" refers to all devices that can function by utilizing semiconductor characteristics. Transistors and semiconductor circuits are a form of semiconductor devices. The semiconductor device of the embodiment shown below can also be a transistor used in an integrated circuit (IC) such as a display device, a microprocessor (MPU), or a memory circuit.

[0079] The so-called "display device" refers to a structure that uses an electro-optical layer to display an image. For example, the term display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure that is equipped with other optical components (such as polarization components, backlight sources, touch panels, etc.) relative to the display unit. As long as there is no technical contradiction, the "electro-optical layer" may include a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer. Therefore, with respect to the embodiments described later, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified as display devices for explanation, but the structure in this embodiment can be applied to a display device including the above-mentioned other electro-optical layers.

[0080] In each embodiment of the present invention, the direction from the substrate toward the oxide semiconductor layer is referred to as up or above. Conversely, the direction from the oxide semiconductor layer toward the substrate is referred to as down or below. Thus, for ease of explanation, the above or below phrases are used for explanation, but for example, the up-and-down relationship between the substrate and the oxide semiconductor layer may be configured in a different direction than that shown in the figure. In the following description, for example, the oxide semiconductor layer on the substrate is merely used to illustrate the up-and-down relationship between the substrate and the oxide semiconductor layer as described above, and other components may be configured between the substrate and the oxide semiconductor layer. Above or below refers to the stacking order in a structure having multiple layers stacked, and in the case of a pixel electrode described as above a transistor, it may also be a positional relationship in which the transistor and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as being vertically above a transistor, it refers to a positional relationship in which the transistor and the pixel electrode overlap when viewed from above.

[0081] In this specification, unless otherwise specified, expressions such as “α includes A, B, or C”, “α includes any one of A, B, and C”, and “α includes one selected from the group consisting of A, B, and C” do not exclude the case where α includes a plurality of combinations of A to C. In addition, the above expressions do not exclude the case where α includes other elements.

[0082] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0083] <First Embodiment>

[0084] use Figures 1 to 13 A semiconductor device according to an embodiment of the present invention will be described.

[0085] [Configuration of Semiconductor Device 10]

[0086] use Figure 1 and Figure 2 Next, a configuration of a semiconductor device 10 according to an embodiment of the present invention will be described. Figure 1 It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention. Figure 2 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.

[0087] like Figure 1As shown, the semiconductor device 10 is provided on a substrate 100. The semiconductor device 10 includes a gate electrode 105, gate insulating layers 110 and 120, an oxide metal layer 130 (also referred to as a metal oxide layer), an oxide semiconductor layer 140, a gate insulating layer 150, a gate electrode 160, insulating layers 170 and 180, a source electrode 201, and a drain electrode 203. When the source electrode 201 and the drain electrode 203 are not particularly distinguished, they are sometimes collectively referred to as a source / drain electrode 200.

[0088] The gate electrode 105 is provided on the substrate 100. The gate insulating layer 110 and the gate insulating layer 120 are provided on the substrate 100 and the gate electrode 105. The metal oxide layer 130 is provided on the gate insulating layer 120. The metal oxide layer 130 is in contact with the gate insulating layer 120. The oxide semiconductor layer 140 is provided on the metal oxide layer 130. The oxide semiconductor layer 140 is in contact with the metal oxide layer 130. The surface of the main surface of the oxide semiconductor layer 140 that is in contact with the metal oxide layer 130 is referred to as a lower surface 142. The end of the metal oxide layer 130 is substantially consistent with the end of the oxide semiconductor layer 140.

[0089] In this embodiment, no semiconductor layer or oxide semiconductor layer is provided between the metal oxide layer 130 and the substrate 100 .

[0090] In this embodiment, the structure in which the metal oxide layer 130 is in contact with the gate insulating layer 120 and the oxide semiconductor layer 140 is in contact with the metal oxide layer 130 is exemplified, but the present invention is not limited to this structure. Other layers may be provided between the gate insulating layer 120 and the metal oxide layer 130. Other layers may also be provided between the metal oxide layer 130 and the oxide semiconductor layer 140.

[0091] exist Figure 1 In the embodiment, the side wall of the metal oxide layer 130 and the side wall of the oxide semiconductor layer 140 are arranged in a straight line, but the present invention is not limited to this configuration. The angle of the side wall of the metal oxide layer 130 relative to the main surface of the substrate 100 may be different from the angle of the side wall of the oxide semiconductor layer 140 relative to the main surface of the substrate 100. The cross-sectional shape of the side wall of at least one of the metal oxide layer 130 and the oxide semiconductor layer 140 may be curved.

[0092] The gate electrode 160 is opposite to the oxide semiconductor layer 140. The gate insulating layer 150 is provided between the oxide semiconductor layer 140 and the gate electrode 160. The gate insulating layer 150 is in contact with the oxide semiconductor layer 140. The surface in contact with the gate insulating layer 150 among the main surfaces of the oxide semiconductor layer 140 is referred to as an upper surface 141. The surface between the upper surface 141 and the lower surface 142 is referred to as a side surface 143. The insulating layers 170 and 180 are provided on the gate insulating layer 150 and the gate electrode 160. The insulating layers 170 and 180 are provided with openings 171 and 173 reaching the oxide semiconductor layer 140. The source electrode 201 is provided inside the opening 171. The source electrode 201 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 171. The drain electrode 203 is provided inside the opening 173. The drain electrode 203 is in contact with the oxide semiconductor layer 140 at the bottom of the opening 173.

[0093] The gate electrode 105 has a function as a bottom gate of the semiconductor device 10 and a function as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 110 has a function as a barrier film for shielding impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. The gate insulating layers 110 and 120 have a function as a gate insulating layer for the bottom gate. The metal oxide layer 130 is a layer containing a metal oxide having aluminum as a main component, and has a function as a gas barrier film for shielding gases such as oxygen and hydrogen.

[0094] The oxide semiconductor layer 140 is divided into a source region S, a drain region D, and a channel region CH. The channel region CH is a region vertically below the gate electrode 160 in the oxide semiconductor layer 140. The source region S is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the source electrode 201 than the channel region CH. The drain region D is a region of the oxide semiconductor layer 140 that does not overlap with the gate electrode 160, and is a region closer to the drain electrode 203 than the channel region CH. The oxide semiconductor layer 140 in the channel region CH has physical properties as a semiconductor. The oxide semiconductor layer 140 in the source region S and the drain region D has physical properties as a conductor.

[0095] The gate electrode 160 has the function of serving as the top gate of the semiconductor device 10 and as a light shielding film for the oxide semiconductor layer 140. The gate insulating layer 150 has the function of serving as a gate insulating layer for the top gate and has the function of releasing oxygen through heat treatment in the manufacturing process. The insulating layers 170 and 180 have the function of insulating the gate electrode 160 from the source / drain electrode 200 to reduce the parasitic capacitance therebetween. The operation of the semiconductor device 10 is mainly controlled by the voltage supplied to the gate electrode 160. An auxiliary voltage is supplied to the gate electrode 105. However, in the case where the gate electrode 105 is used only as a light shielding film, it is also possible to place the gate electrode 105 in a floating state instead of supplying a specific voltage to the gate electrode 105. That is, the gate electrode 105 may also be simply referred to as a "light shielding film".

[0096] In this embodiment, a dual-gate transistor in which gate electrodes are provided both above and below the oxide semiconductor layer is used as an example of the semiconductor device 10, but the present invention is not limited to this configuration. For example, a bottom-gate transistor in which the gate electrode is provided only below the oxide semiconductor layer or a top-gate transistor in which the gate electrode is provided only above the oxide semiconductor layer may be used as the semiconductor device 10. The above configuration is only one embodiment, and the present invention is not limited to the above configuration.

[0097] like Figure 2 As shown, in a top view, the planar pattern of the metal oxide layer 130 is substantially the same as the planar pattern of the oxide semiconductor layer 140. Figure 1 and Figure 2 , the lower surface 142 of the oxide semiconductor layer 140 is covered by the oxide metal layer 130. In particular, in the present embodiment, the entire lower surface 142 of the oxide semiconductor layer 140 is covered by the oxide metal layer 130. In the first direction D1, the width of the gate electrode 105 is greater than the width of the gate electrode 160. The first direction D1 is a direction connecting the source electrode 201 and the drain electrode 203, and is a direction indicating the channel length L of the semiconductor device 10. Specifically, the length in the first direction D1 of the region (channel region CH) where the oxide semiconductor layer 140 overlaps with the gate electrode 160 is the channel length L, and the width in the second direction D2 of the channel region CH is the channel width W.

[0098] In this embodiment, a configuration in which the entire lower surface 142 of the oxide semiconductor layer 140 is covered by the oxide metal layer 130 is exemplified, but the present invention is not limited to this configuration. For example, a portion of the lower surface 142 of the oxide semiconductor layer 140 may not be in contact with the oxide metal layer 130. For example, the entire lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may be covered by the oxide metal layer 130, and the entire or a portion of the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be covered by the oxide metal layer 130. That is, the entire or a portion of the lower surface 142 of the oxide semiconductor layer 140 in the source region S and the drain region D may not be in contact with the oxide metal layer 130. However, in the above configuration, a portion of the lower surface 142 of the oxide semiconductor layer 140 in the channel region CH may not be covered by the oxide metal layer 130, and the other portion of the lower surface 142 may be in contact with the oxide metal layer 130.

[0099] In this embodiment, a configuration in which the gate insulating layer 150 is formed on the entire surface and the openings 171 and 173 are provided in the gate insulating layer 150 is exemplified, but the present invention is not limited to this configuration. The gate insulating layer 150 may also be patterned. For example, the gate insulating layer 150 may be patterned in such a manner that the oxide semiconductor layer 140 in the source region S and the drain region D is exposed. That is, the gate insulating layer 150 in the source region S and the drain region D may be removed, and the oxide semiconductor layer 140 may be in contact with the insulating layer 170 in these regions.

[0100] exist Figure 2 , the structure in which the source / drain electrode 200 does not overlap with the gate electrode 105 and the gate electrode 160 in a plan view is illustrated, but the present invention is not limited to this structure. For example, the source / drain electrode 200 may overlap with at least one of the gate electrode 105 and the gate electrode 160 in a plan view. The above structure is only one embodiment, and the present invention is not limited to the above structure.

[0101] [Material of Each Component of Semiconductor Device 10]

[0102] As the substrate 100, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate is used. When the substrate 100 needs to be flexible, a substrate containing resin such as a polyimide substrate, an acrylic substrate, a siloxane-based substrate, or a fluororesin substrate is used as the substrate 100. When a substrate containing resin is used as the substrate 100, impurities may be introduced into the above-mentioned resin in order to improve the heat resistance of the substrate 100. In particular, when the semiconductor device 10 is a top-emitting display, since the substrate 100 does not need to be transparent, impurities that reduce the transparency of the substrate 100 may be used. When the semiconductor device 10 is used in an integrated circuit that is not a display device, a substrate that is not light-transmitting, such as a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, or a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate, is used as the substrate 100.

[0103] A common metal material is used as the gate electrode 105, the gate electrode 160, and the source / drain electrode 200. For example, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys thereof or compounds thereof are used as these members. The gate electrode 105, the gate electrode 160, and the source / drain electrode 200 may be used in a single layer or in a stacked layer.

[0104] As the gate insulating layers 110, 120 and the insulating layers 170, 180, a general insulating layer material is used. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), Silicon Nitride (SiN x ), silicon oxynitride (SiN x O y ), aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x ) and other inorganic insulating layers.

[0105] As the gate insulating layer 150, an insulating layer containing oxygen among the above insulating layers is used. For example, as the gate insulating layer 150, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), aluminum oxide (AlO x ), aluminum oxynitride (AlOx N y ) and other inorganic insulating layers.

[0106] An insulating layer having a function of releasing oxygen by heat treatment is used as the gate insulating layer 120. For example, the temperature of the heat treatment for releasing oxygen from the gate insulating layer 120 is, for example, 600° C. or less, 500° C. or less, 450° C. or less, or 400° C. or less. That is, for example, when a glass substrate is used as the substrate 100, the gate insulating layer 120 releases oxygen at the heat treatment temperature performed in the manufacturing process of the semiconductor device 10.

[0107] As the gate insulating layer 150, an insulating layer with few defects is used. For example, when the composition ratio of oxygen in the gate insulating layer 150 is compared with the composition ratio of oxygen in an insulating layer having the same composition as the gate insulating layer 150 (hereinafter referred to as "another insulating layer"), the composition ratio of oxygen in the gate insulating layer 150 is closer to the stoichiometric ratio of the insulating layer than the composition ratio of oxygen in the other insulating layer. Specifically, silicon oxide (SiO x ), the oxygen composition ratio of silicon oxide used as the gate insulating layer 150 is closer to the stoichiometric ratio of silicon oxide than the oxygen composition ratio of silicon oxide used as the insulating layer 180. For example, as the gate insulating layer 150, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) may be used.

[0108] The above SiO x N y and AlO x N y It is a silicon compound or aluminum compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). x O y and AlN x O y These are silicon compounds and aluminum compounds containing oxygen at a ratio smaller than that of nitrogen (x>y).

[0109] As the metal oxide layer 130, a metal oxide containing aluminum as a main component is used. For example, aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x) and other inorganic insulating layers. The so-called "metal oxide layer with aluminum as the main component" means that the ratio of aluminum contained in the metal oxide layer 130 is greater than 1% of the entire metal oxide layer 130. The ratio of aluminum contained in the metal oxide layer 130 may also be greater than 5% and less than 70%, greater than 10% and less than 60%, or greater than 30% and less than 50% of the entire metal oxide layer 130. The above ratio may be a mass ratio or a weight ratio.

[0110] As the oxide semiconductor layer 140, an oxide metal having semiconductor characteristics can be used. For example, as the oxide semiconductor layer 140, an oxide semiconductor containing two or more metals including indium (In) can be used. The ratio of indium to the whole of the oxide semiconductor layer 140 is 50% or more. As the oxide semiconductor layer 140, in addition to indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium oxide (Zr), and lanthanide elements can also be used. As the oxide semiconductor layer 140, other elements other than the above can also be used.

[0111] The oxide semiconductor layer 140 may be amorphous or crystalline. The oxide semiconductor layer 140 may also be a mixed phase of amorphous and crystalline. As described below, in the oxide semiconductor layer 140 where the ratio of indium is 50% or more, oxygen vacancies are easily formed. Crystalline oxide semiconductors are less likely to form oxygen vacancies than amorphous oxide semiconductors. Therefore, it is preferred that the oxide semiconductor layer 140 as described above has crystallinity.

[0112] [Problems Newly Recognized in the Process of Implementing the Invention]

[0113] The ratio of indium in the oxide semiconductor layer 140 is set to 50% or more, thereby realizing a semiconductor device 10 with high mobility. On the other hand, in such an oxide semiconductor layer 140 , oxygen contained in the oxide semiconductor layer 140 is easily reduced, so that oxygen vacancies are easily formed in the oxide semiconductor layer 140 .

[0114] In the semiconductor device 10, hydrogen is released from a layer (e.g., gate insulating layers 110 and 120) disposed on the substrate 100 side relative to the oxide semiconductor layer 140 during a heat treatment process in the manufacturing process. Since the hydrogen reaches the oxide semiconductor layer 140, oxygen vacancies are generated in the oxide semiconductor layer 140. The generation of the oxygen vacancies is more significant when the pattern size of the oxide semiconductor layer 140 is larger. In order to suppress the generation of such oxygen vacancies, it is necessary to suppress the hydrogen from reaching the lower surface 142 of the oxide semiconductor layer 140. The above content is the first subject.

[0115] In addition to the above-mentioned problems, there is a second problem as shown below. The upper surface 141 of the oxide semiconductor layer 140 is affected by the process (e.g., patterning process or etching process) after the oxide semiconductor layer 140 is formed. On the other hand, the lower surface 142 of the oxide semiconductor layer 140 (the surface of the oxide semiconductor layer 140 on the substrate 100 side) is not affected as described above.

[0116] Therefore, the oxygen vacancies formed near the upper surface 141 of the oxide semiconductor layer 140 are more than the oxygen vacancies formed near the lower surface 142 of the oxide semiconductor layer 140. That is, the oxygen vacancies in the oxide semiconductor layer 140 are not uniformly present in the thickness direction of the oxide semiconductor layer 140, but are unevenly distributed in the thickness direction of the oxide semiconductor layer 140. Specifically, the oxygen vacancies in the oxide semiconductor layer 140 are less toward the lower surface 142 of the oxide semiconductor layer 140, and more toward the upper surface 141 of the oxide semiconductor layer 140.

[0117] In the case where the oxygen supply treatment is uniformly performed on the oxide semiconductor layer 140 having the above-described oxygen vacancy distribution, if the amount of oxygen required to repair the oxygen vacancy formed on the upper surface 141 side of the oxide semiconductor layer 140 is supplied, oxygen will be excessively supplied to the lower surface 142 side of the oxide semiconductor layer 140. As a result, on the lower surface 142 side, a defect energy level different from the oxygen vacancy is formed due to the excess oxygen. As a result, phenomena such as characteristic changes in reliability tests or a decrease in field effect mobility occur. Therefore, in order to suppress such a phenomenon, it is necessary to supply oxygen to the upper surface 141 side of the oxide semiconductor layer 140 while suppressing the oxygen supply to the lower surface 142 side of the oxide semiconductor layer 140.

[0118] The above-mentioned problems are newly recognized problems in the process of reaching the present invention, and are not problems that have been recognized in the past. In the previous structure and manufacturing method, even if the initial characteristics of the semiconductor device are improved by oxygen supply treatment to the oxide semiconductor layer, the characteristics change in the reliability test, and there is a trade-off relationship between the initial characteristics and the reliability test. However, the structure involved in this embodiment can solve the above-mentioned problems, and can obtain good initial characteristics and high reliability of the semiconductor device 10.

[0119] In addition, the flatness of the surface on which the oxide semiconductor layer 140 is formed affects the crystallinity of the oxide semiconductor layer 140. In the present embodiment, the metal oxide layer 130 for forming the oxide semiconductor layer 140 is usually formed by sputtering. The surface roughness (arithmetic mean roughness Ra) of the metal oxide layer 130 just after the film is formed by sputtering is about 1nm to 4nm. If surface irregularities are generated on the surface of the metal oxide layer 130, even if they are about 1nm to 4nm, when the oxide semiconductor layer 140 formed on the metal oxide layer 130 is crystallized by heat treatment, the crystal growth in the thickness direction of the oxide semiconductor layer 140 will also be hindered. That is, the direction of crystal growth of the oxide semiconductor layer 140 becomes random due to the surface irregularities. In a semiconductor device using such an oxide semiconductor layer, further improvement of the field effect mobility cannot be expected. Therefore, there is room for improvement in order to improve the field effect mobility of the semiconductor device.

[0120] In the semiconductor device 10 according to one embodiment of the present invention, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0121] μ=-10.033Ra+48.23

[0122] (Among which, the arithmetic mean roughness Ra≤0.80nm)

[0123] In one embodiment of the present invention, at the interface between the metal oxide layer 130 and the oxide semiconductor layer 140, the upper surface of the metal oxide layer 130 has flatness. The oxide semiconductor layer 140 is formed on a surface with reduced surface irregularities, which will be described later. When the oxide semiconductor layer 140 formed on the metal oxide layer 130 is heat treated, the direction and growth rate of the crystal growth of the oxide semiconductor layer 140 can be made consistent. By using the oxide semiconductor layer 140 having such crystallinity, the field effect mobility of the semiconductor device 10 can be further improved. Specifically, the field effect mobility of the semiconductor device 10 can be 40 cm 2 / V·s or more.

[0124] [Method of Manufacturing Semiconductor Device 10]

[0125] use Figure 3 to Figure 13 A method for manufacturing a semiconductor device according to an embodiment of the present invention will be described. Figure 3 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Figures 4 to 132 is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. In the following description of the manufacturing method, a method for manufacturing the semiconductor device 10 using aluminum oxide as the metal oxide layer 130 will be described.

[0126] like Figure 3 and Figure 4 As shown, a gate electrode 105 is formed on the substrate 100 as a bottom gate, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Figure 3 The "bottom GI / GE formation" of step S1001). For example, silicon nitride is formed as the gate insulating layer 110. For example, silicon oxide is formed as the gate insulating layer 120. The gate insulating layers 110 and 120 are formed by CVD (Chemical Vapor Deposition).

[0127] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.

[0128] like Figure 3 and Figure 5 As shown, a metal oxide layer 130 is formed on the gate insulating layer 120 ( Figure 3 The metal oxide layer 130 is formed by a sputtering method or an atomic layer deposition method (ALD: Atomic Layer Deposition).

[0129] For example, the thickness of the metal oxide layer 130 during film formation is 6 nm to 60 nm, 6 nm to 50 nm, 6 nm to 25 nm, or 6 nm to 15 nm. The thickness of the metal oxide layer 130 can also be appropriately set according to the planarization method to be described later. In this embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has a high barrier property against gases such as oxygen or hydrogen. The metal oxide layer 130 is formed by sputtering. In this embodiment, aluminum oxide used as the metal oxide layer 130 blocks hydrogen and oxygen released from the gate insulating layer 120, and inhibits the released hydrogen and oxygen from reaching the oxide semiconductor layer 140.

[0130] The surface of the metal oxide layer 130 has a surface unevenness of about 1 nm to 4 nm just after film formation. When the oxide semiconductor layer 140 formed on the metal oxide layer 130 is crystallized, if there is a surface unevenness, even if it is about 1 nm to 4 nm, the direction of crystal growth becomes random. However, it is difficult to form a film by sputtering in a manner that the surface unevenness of the metal oxide layer 130 is less than 1 nm. Therefore, it is preferred to flatten the surface of the metal oxide layer 130 so that the surface unevenness of the metal oxide layer 130 is less than 1 nm.

[0131] like Figure 3 and Figure 6 As shown, the metal oxide layer 130 is planarized ( Figure 3 As the AlOx planarization process, wet etching process or plasma treatment is used.

[0132] In the case of performing a planarization treatment by wet etching, as a chemical liquid, for example, an alkaline chemical liquid such as a developer for removing resist materials is used. As an alkaline chemical liquid, a solution such as tetramethylammonium hydroxide (TMAH) or potassium hydroxide (KOH) is used. In addition, an acidic chemical liquid such as phosphoric acid, nitric acid, hydrofluoric acid, hydrochloric acid, sulfuric acid, acetic acid, oxalic acid, or a mixture thereof may be used. As an acidic chemical liquid, for example, a mixed acid containing phosphoric acid, nitric acid, and acetic acid may be used. In addition, by wet etching, it is preferred to remove more than 5 nm from the surface of the metal oxide layer 130, and more preferably to remove more than 40 nm. When the thickness of the metal oxide layer 130 when formed is 6 nm to 25 nm or 6 nm to 15 nm, by performing a planarization treatment, the thickness of the metal oxide layer 130 becomes 1 nm to 20 nm, preferably 1 nm to 10 nm. The arithmetic mean roughness of the metal oxide layer 130 measured by observing the surface of the metal oxide layer 130 with a square of 1000 nm and a height of 10 nm (fixed) using an AFM is set to Ra<1 nm, preferably Ra≤0.80, and more preferably Ra≤0.73 nm. When wet etching is performed as the planarization process, a cleaning process before the oxide semiconductor layer 140 is formed can also be taken into account.

[0133] In the case of planarization by plasma treatment, the treatment is performed by reverse sputtering or etching. In the case of plasma treatment by reverse sputtering, an inactive gas such as argon, helium, nitrogen, etc. can be used. In addition, in the case of plasma treatment by reverse sputtering, oxygen can be used, or a mixed gas of oxygen and an inactive gas can be used. In addition, in the case of plasma treatment by etching, a halogen-based gas such as a chlorine-based gas and a fluorine-based gas can be used. It is preferred to remove more than 5nm of the surface of the metal oxide layer 130 by plasma treatment. In the case where the thickness of the metal oxide layer 130 when formed is 6nm to 60nm or 6nm to 50nm, by performing a planarization treatment, the thickness of the metal oxide layer 130 becomes 1nm to 20nm, preferably 1nm to 10nm. The arithmetic mean roughness of the oxidized metal layer 130 measured by observing the surface of the oxidized metal layer 130 with an AFM in a 1000 nm square and a 10 nm height (fixed) is set to Ra < 1 nm, preferably Ra ≤ 0.73 nm, and more preferably Ra ≤ 0.67. When plasma treatment is performed as a flattening treatment, particles attached to the surface can also be removed.

[0134] Here, a method for evaluating the flatness of the surface of the oxidized metal layer 130 is described. The flatness of the oxidized metal layer 130 can be evaluated using an atomic force microscope (AFM). A roughness curve is obtained by AFM analysis. Based on the roughness curve, the arithmetic mean roughness (Ra), the root mean square roughness (Rq), the maximum height difference (Rmax), etc. are obtained as roughness curve parameters.

[0135] The arithmetic mean roughness (Ra) is the average of the absolute values ​​of the ordinate values ​​Z(X) within the reference length. The smaller the arithmetic mean roughness (Ra), the higher the flatness of the film. It should be noted that the ordinate value Z(X) is the height of the roughness curve at an arbitrary position X. The root mean square height (Rq) represents the root mean square within the reference length. It refers to the standard deviation of the surface roughness.

[0136] The above-mentioned roughness curve parameters are defined in accordance with JIS B 0601-2001 (equivalent to ISO 4287-1997).

[0137] The roughness curve parameter of the oxidized metal layer 130 can also be calculated by using the contrast of the cross-sectional TEM image obtained by photographing the semiconductor device instead of the atomic force microscope. In the cross-sectional TEM image, the contrast (brightness) of the oxidized metal layer 130 and the oxide semiconductor layer 140 is different. Therefore, the boundary of the contrast between the oxidized metal layer 130 and the oxide semiconductor layer 140 can also be approximated as the roughness curve of the surface of the oxidized metal layer 130. Based on the approximated roughness curve, the arithmetic mean roughness (Ra) and the root mean square roughness (Rq) can also be calculated according to JIS B 0601-2001 as roughness curve parameters.

[0138] The thickness of the metal oxide layer after the planarization treatment is 1 nm to 20 nm, preferably 1 nm to 10 nm.

[0139] like Figure 3 and Figure 7 As shown, an oxide semiconductor layer 140 is formed on the planarized metal oxide layer 130 ( Figure 3 of step S1004 (“OS film formation”).

[0140] For example, the thickness of the oxide semiconductor layer 140 is greater than or equal to 10 nm and less than or equal to 100 nm, greater than or equal to 15 nm and less than or equal to 70 nm, or greater than or equal to 20 nm and less than or equal to 40 nm. In this embodiment, an oxide containing indium (In) and gallium (Ga) is used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 before the heat treatment (OS annealing) described later is amorphous.

[0141] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably in an amorphous state (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 immediately after film formation is not crystallized as much as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed under a state in which the temperature of the object to be formed (the substrate 100 and the structure formed thereon) is controlled.

[0142] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target will collide with the object to be formed. Therefore, the temperature of the object to be formed will rise along with the film forming process. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor layer 140 contains microcrystals in the state just after the film is formed. Due to the microcrystals, the subsequent crystallization caused by OS annealing is hindered. In order to control the temperature of the object to be formed as described above, the film can also be formed while cooling the object to be formed. For example, the object to be formed can also be cooled from the surface opposite to the film forming surface in such a way that the temperature of the film forming surface of the object to be formed (hereinafter referred to as the "film forming temperature") is below 100°C, below 70°C, below 50°C or below 30°C. By forming the oxide semiconductor layer 140 while cooling the object to be formed as described above, an oxide semiconductor layer 140 with a small crystalline component in the state just after the film is formed can be formed.

[0143] like Figure 3 and Figure 8 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Figure 3 Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask. The oxide semiconductor layer 140 can be etched by wet etching or dry etching. As wet etching, an acidic etchant can also be used for etching. For example, oxalic acid or hydrofluoric acid can be used as an etchant.

[0144] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Figure 3 In the present embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing. In the present embodiment, the arithmetic mean roughness Ra of the metal oxide layer 130 is reduced to less than 1 nm, preferably to less than 0.80 nm, and more preferably to less than 0.73 nm. The oxide semiconductor layer 140 is formed on the flat surface of the metal oxide layer 130 with suppressed surface irregularities. Therefore, when the oxide semiconductor layer 140 is crystallized by the OS annealing, the direction of crystal growth can be suppressed from becoming random, and the direction and growth speed of crystal growth can be made consistent. Thus, the oxide semiconductor layer 140 having such a crystalline state that the direction of crystal growth is consistent can be formed.

[0145] like Figure 3 and Fig. 9 As shown, the pattern of the oxidized metal layer 130 is formed ( Figure 3The oxide semiconductor layer 140 patterned in the above process is used as a mask to etch the oxidized metal layer 130. As the etching of the oxidized metal layer 130, wet etching or dry etching can be used. As the wet etching, for example, diluted hydrofluoric acid (DHF) can be used. As described above, by etching the oxidized metal layer 130 with the oxide semiconductor layer 140 as a mask, the photolithography process can be omitted.

[0146] like Figure 3 and Fig.10 As shown, the gate insulating layer 150 ( Figure 3 ("GI formation" in step S1008 of the present invention). For example, silicon oxide is formed as the gate insulating layer 150. The gate insulating layer 150 is formed by a CVD method. For example, in order to form an insulating layer with few defects as the gate insulating layer 150 as described above, the gate insulating layer 150 may be formed at a film forming temperature of 350° C. or higher. For example, the thickness of the gate insulating layer 150 is between 50 nm and 300 nm, between 60 nm and 200 nm, or between 70 nm and 150 nm. After the gate insulating layer 150 is formed, a process of injecting oxygen into a portion of the gate insulating layer 150 may be performed.

[0147] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140, heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Figure 3 In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. The oxygen released from the gate insulating layers 120 and 150 by the above-mentioned oxidation annealing is supplied to the oxide semiconductor layer 140 to repair the oxygen vacancies.

[0148] Oxygen released from the gate insulating layer 120 by the oxidation annealing is blocked by the oxidized metal layer 130. Therefore, it is difficult to supply oxygen to the lower surface 142 of the oxide semiconductor layer 140. Oxygen released from the gate insulating layer 120 diffuses from the region where the oxidized metal layer 130 is not formed to the gate insulating layer 150 provided on the gate insulating layer 120, and reaches the oxide semiconductor layer 140 via the gate insulating layer 150. As a result, oxygen released from the gate insulating layer 120 is not easily supplied to the lower surface 142 of the oxide semiconductor layer 140, but is mainly supplied to the side surface 143 and the upper surface 141 of the oxide semiconductor layer 140. In addition, oxygen released from the gate insulating layer 150 by the oxidation annealing is supplied to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Hydrogen may be released from the gate insulating layers 110 and 120 by the above-mentioned oxidation annealing, but the hydrogen is blocked by the oxidized metal layer 130.

[0149] As described above, the oxidation annealing step can suppress oxygen supply to the lower surface 142 of the oxide semiconductor layer 140 having a small amount of oxygen vacancies, while supplying oxygen to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140 having a large amount of oxygen vacancies.

[0150] like Figure 3 and Fig.11 As shown, the film-forming gate electrode 160 ( Figure 3 The gate electrode 160 is formed by sputtering or atomic layer deposition and patterned by a photolithography process.

[0151] In the state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Figure 3 Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. For example, argon (Ar), phosphorus (P), and boron (B) are injected into the oxide semiconductor layer 140 by ion implantation. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the semiconductor device 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.

[0152] like Figure 3 and Fig.12 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Figure 3The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used as the insulating layers 170 and 180 are not limited to the above. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.

[0153] like Figure 3 and Fig.13 As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Figure 3 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrodes 200 ( Figure 3 Step S1014 of "SD formation"), thereby completing Figure 1 A semiconductor device 10 is shown.

[0154] The semiconductor device 10 manufactured by the above-mentioned manufacturing method can make the direction and growth speed of crystal growth consistent in the oxide semiconductor layer 140. As a result, when the channel length L of the channel region CH in the semiconductor device 10 is within the range of 2 μm to 4 μm and the channel width of the channel region CH is within the range of 2 μm to 25 μm, a mobility of 30 [cm 2 / Vs] or more, 35[cm 2 / Vs] or more, preferably 40 [cm 2 / Vs] or above. The mobility in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10. Specifically, the mobility refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the value (Vg-Vth) obtained by subtracting the threshold voltage (Vth) of the semiconductor device 10 from the voltage (Vg) supplied to the gate electrode.

[0155] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by wet etching, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0156] μ=-10.033Ra+48.23

[0157] (Among which, the arithmetic mean roughness Ra≤0.80)

[0158] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by plasma treatment, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0159] μ=-5.9584Ra+43.978

[0160] (Among which, the arithmetic mean roughness Ra≤0.67)

[0161] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by wet etching or plasma treatment, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0162] μ=-5.770Ra+44.22

[0163] (Among which, the arithmetic mean roughness Ra≤0.73)

[0164] <Modification 1 of the first embodiment>

[0165] use Figure 14 to Figure 16 A first modification of the present embodiment will be described. The structure of the semiconductor device 10 according to the first modification is similar to Figure 1 Same, but its manufacturing method is different from Figure 3 to Figure 13 In the following description, the Figure 3 to Figure 13 The description of the manufacturing method common to the manufacturing methods shown will mainly describe the manufacturing method related to the differences between the two.

[0166] Fig.14 It is a timing chart showing a method for manufacturing a semiconductor device according to a modification of one embodiment of the present invention. Fig.15 and Fig.16 1 is a cross-sectional view showing a method for manufacturing a semiconductor device according to a modified example of one embodiment of the present invention. Fig.14 As shown, in Modification 1, the patterns of the metal oxide layer 130 and the oxide semiconductor layer 140 are formed at the same time (“OS / AlOx pattern formation” in step S1020 ).

[0167] like Fig.15As shown in FIG. 1 , after the metal oxide layer 130 and the oxide semiconductor layer 140 are formed, a resist mask 220 is formed on the oxide semiconductor layer 140. Then, as shown in FIG. Fig.16 As shown, the resist mask 220 is used to form a pattern of the metal oxide layer 130 and the oxide semiconductor layer 140. As the etching of the metal oxide layer 130 and the oxide semiconductor layer 140, wet etching or dry etching can be used. In the case of etching the metal oxide layer 130 and the oxide semiconductor layer 140 by wet etching, the same etchant as described above can be used. In the modification example 1, OS annealing is performed in a state where the pattern of the metal oxide layer 130 and the oxide semiconductor layer 140 is formed (step S1006). The subsequent steps S1008 to S1014 are due to the Figure 3 Likewise, detailed description is therefore omitted.

[0168] <Modification 2 of the first embodiment>

[0169] use Fig.17 and Fig.18 A second modification of the present embodiment will be described. The structure and manufacturing method of the semiconductor device 10 according to the second modification are similar to those of the semiconductor device 10 of FIG. Figure 1 and Figure 3 to Figure 13 In the following description, the Figure 1 and Figure 3 to Figure 13 The description of the manufacturing method common to the manufacturing methods shown will mainly describe the manufacturing method related to the differences between the two.

[0170] Fig.17 It is a cross-sectional view schematically showing a semiconductor device according to a modified example of one embodiment of the present invention. Fig.18 It is a timing chart showing a method for manufacturing a semiconductor device according to a modification of one embodiment of the present invention.

[0171] like Fig.17 As shown, the structure of the semiconductor device 10 according to the second modification is similar to Figure 1 The structure of the semiconductor device 10 shown is similar to that of the semiconductor device 10 shown in FIG. 1 , but the pattern of the oxide metal layer 130 is not formed. Figure 1 The structure of the semiconductor device 10 shown is different. That is, in Modification 2, the metal oxide layer 130 extends outward from the pattern of the oxide semiconductor layer 140 . The metal oxide layer 130 is in contact with the gate insulating layer 150 outside the pattern of the oxide semiconductor layer 140 .

[0172] like Fig.18 As shown, the manufacturing method of the semiconductor device 10 according to the modification example 2 is the same as Figure 3 The manufacturing method of the semiconductor device 10 is similar, but the patterning of the oxide metal layer 130 is omitted ( Figure 3The process of step S1007) is similar to Figure 3 The manufacturing method of the semiconductor device 10 shown in FIG. 1 is different from that of FIG. 1 . Figure 3 Likewise, detailed description is therefore omitted.

[0173] <Variation 3 of the First Embodiment>

[0174] use Figure 19 to Figure 23 The structure and manufacturing method of the semiconductor device 10 according to the modification example 3 of the present embodiment are described below. Figures 1 to 13 In the following description, the Figures 1 to 13 The description of the manufacturing method common to the manufacturing methods shown will mainly describe the manufacturing method related to the differences between the two.

[0175] Fig.19 It is a cross-sectional view schematically showing a semiconductor device according to an embodiment of the present invention. Fig. 20 It is a plan view schematically showing a semiconductor device according to an embodiment of the present invention.

[0176] like Fig.19 and Fig. 20 As shown, the structure of the semiconductor device 10 according to the modification example 3 is similar to Figure 1 and Figure 2 The structure of the semiconductor device 10 shown is similar to that of the semiconductor device 10 shown in FIG. 1 , but the pattern of the metal oxide layer 130 is different from the pattern of the oxide semiconductor layer 140. Figure 1 The structure of the semiconductor device 10 shown is different. Specifically, Fig.19 In a cross-sectional view, the pattern of the oxide semiconductor layer 140 extends outward compared to the pattern of the oxidized metal layer 130. That is, the oxide semiconductor layer 140 crosses the pattern of the oxidized metal layer 130. The oxide semiconductor layer 140 is in contact with the gate insulating layer 120 outside the pattern of the oxidized metal layer 130. The gate insulating layer 120 is sometimes referred to as a "first insulating layer".

[0177] The source / drain electrode 200 is in contact with the oxide semiconductor layer 140 in a region where the metal oxide layer 130 is not provided. Fig. 20 In a plan view, the pattern of the metal oxide layer 130 is located inside the pattern of the oxide semiconductor layer 140. Openings 171 and 173 are provided in regions that do not overlap with the pattern of the metal oxide layer 130.

[0178] Fig.21 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Fig. 22 and Fig.23 1 is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Fig.21 As shown, in the third variant, after the pattern of the oxidized metal layer 130 is formed (the "AlOx film formation" of step S1030 and the "AlOx pattern formation" of step S1031), the oxidized metal layer 130 is planarized (step S1032). Thereafter, the pattern of the oxide semiconductor layer 140 is formed (the "OS film formation" of step S1033 and the "OS pattern formation" of step S1034). Figure 3 The difference is that the OS annealing (“OS annealing” in step S1035 ) is performed after the gate insulating layer 150 is formed.

[0179] like Fig. 22 As shown, a metal oxide layer 130 is formed on the gate insulating layer 120 (step S1030), and a pattern of the metal oxide layer 130 is formed (step S1031). The patterning (etching) of the metal oxide layer 130 is performed by the same method as described above. Thereafter, the surface of the patterned metal oxide layer 130 is planarized (step S1032).

[0180] like Fig.23 As shown in FIG. 1 , an oxide semiconductor layer 140 is formed on the patterned metal oxide layer 130 (step S1033), and a pattern of the oxide semiconductor layer 140 is formed (step S1034). The patterning (etching) of the oxide semiconductor layer 140 is performed in the same manner as described above. Fig.23 OS annealing is performed in the state shown (step S1035). The following steps S1008 to S1014 are related to Figure 3 Likewise, detailed description is therefore omitted.

[0181] As described above, according to the semiconductor devices 10 according to Modifications 1 to 3 of the present embodiment, it is possible to obtain the same effects as those of the present embodiment.

[0182] <Second Embodiment>

[0183] use Figure 24 to Figure 35 A semiconductor device according to an embodiment of the present invention will be described.

[0184] [Configuration of Semiconductor Device 10]

[0185] The configuration of the semiconductor device 10 according to the present embodiment is the same as that of the first embodiment. Figure 1 and Figure 2The semiconductor device 10 according to the present embodiment will be described. The semiconductor device 10 according to the present embodiment is different from the semiconductor device 10 according to the first embodiment in the manufacturing method. Therefore, in the present embodiment, the description of the structure of the semiconductor device 10 is omitted, and the manufacturing method thereof will be described. In the following description, as the metal oxide layer 190 (also referred to as the metal oxide layer), the same material as the metal oxide layer 130 can be used.

[0186] [Method of Manufacturing Semiconductor Device 10]

[0187] use Figure 24 to Figure 35 A method for manufacturing a semiconductor device according to an embodiment of the present invention will be described. Fig.24 This is a timing chart showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. Figure 25 to Figure 35 1 is a cross-sectional view showing a method for manufacturing a semiconductor device according to an embodiment of the present invention. In the following description of the manufacturing method, a method for manufacturing the semiconductor device 10 using aluminum oxide as the metal oxide layers 130 and 190 will be described.

[0188] like Fig.24 and Fig.25 As shown, a gate electrode 105 is formed on the substrate 100 as a bottom gate, and gate insulating layers 110 and 120 are formed on the gate electrode 105 ( Fig.24 (“Bottom GI / GE formation” in step S2001). For example, silicon nitride is formed as the gate insulating layer 110. For example, silicon oxide is formed as the gate insulating layer 120. The gate insulating layers 110 and 120 are formed by a CVD (Chemical Vapor Deposition) method.

[0189] By using silicon nitride as the gate insulating layer 110, the gate insulating layer 110 can block, for example, impurities diffusing from the substrate 100 toward the oxide semiconductor layer 140. Silicon oxide used as the gate insulating layer 120 has a property of releasing oxygen by heat treatment.

[0190] like Fig.24 and Fig.26 As shown, a metal oxide layer 130 and an oxide semiconductor layer 140 are formed on the gate insulating layer 120 ( Fig.24 The metal oxide layer 130 is formed by sputtering or atomic layer deposition (ALD: Atomic Layer Deposition).

[0191] The thickness of the metal oxide layer 130 during film formation is, for example, 6 nm to 60 nm, 6 nm to 50 nm, 6 nm to 25 nm, or 6 nm to 15 nm. The thickness of the metal oxide layer 130 can also be appropriately set according to the planarization method to be described later. In this embodiment, aluminum oxide is used as the metal oxide layer 130. Aluminum oxide has a high barrier property against gases such as oxygen and hydrogen. The metal oxide layer 130 is formed by sputtering. In this embodiment, aluminum oxide used as the metal oxide layer 130 blocks hydrogen and oxygen released from the gate insulating layer 120, and inhibits the released hydrogen and oxygen from reaching the oxide semiconductor layer 140.

[0192] The surface of the metal oxide layer 130 has a surface unevenness of about 1 nm to 4 nm just after film formation. When the oxide semiconductor layer 140 formed on the metal oxide layer 130 is crystallized, if there is a surface unevenness, even if it is about 1 nm to 4 nm, the direction of crystal growth becomes random. However, it is difficult to form a film by sputtering in a manner that the surface unevenness of the metal oxide layer 130 is less than 1 nm. Therefore, it is preferred to flatten the surface of the metal oxide layer 130 so that the surface unevenness of the metal oxide layer 130 is less than 1 nm.

[0193] like Fig.24 and Fig. 27 As shown, the metal oxide layer 130 is planarized ( Figure 3 As the AlOx planarization process, wet etching process or plasma treatment is used.

[0194] In the case of performing a planarization treatment by wet etching, as a liquid, an alkaline liquid such as a developer for removing resist materials is used. As an alkaline liquid, a solution such as tetramethylammonium hydroxide (TMAH) or potassium hydroxide (KOH) is used. In addition, an acidic liquid such as phosphoric acid, nitric acid, hydrofluoric acid, hydrochloric acid, sulfuric acid, acetic acid, oxalic acid or a mixture thereof may be used. As an acidic liquid, a mixed acid such as phosphoric acid, nitric acid and acetic acid may be used. In addition, by wet etching, it is preferred to remove more than 5 nm from the surface of the metal oxide layer 130, and more preferably to remove more than 40 nm. When the thickness of the metal oxide layer 130 when formed is 6 nm to 25 nm or 6 nm to 15 nm, by performing a planarization treatment, the thickness of the metal oxide layer 130 becomes 1 nm to 20 nm or 1 nm to 10 nm. The arithmetic mean roughness of the metal oxide layer 130 measured by observing the surface of the metal oxide layer 130 with a square of 1000 nm and a height of 10 nm (fixed) using an AFM is set to Ra<1 nm, preferably Ra≤0.80, and more preferably Ra≤0.73 nm. When wet etching is performed as the planarization process, a cleaning process before forming the oxide semiconductor layer 140 can also be taken into consideration.

[0195] In the case of flattening by plasma treatment, the treatment is performed by reverse sputtering or etching. In the case of plasma treatment by reverse sputtering, an inert gas such as argon gas and nitrogen gas can be used. In addition, in the case of plasma treatment by reverse sputtering, oxygen gas can be used, or a mixed gas of oxygen gas and an inert gas can be used. In addition, in the case of plasma treatment by etching, a halogen gas such as a chlorine gas and a fluorine gas can be used. It is preferred to remove more than 5nm of the surface of the oxidized metal layer 130 by plasma treatment. In the case where the thickness of the oxidized metal layer 130 is 6nm to 60nm or 6nm to 50nm when the film is formed, by performing a flattening treatment, the thickness of the oxidized metal layer 130 becomes 1nm to 20nm, preferably 1nm to 10nm. The arithmetic mean roughness of the oxidized metal layer 130 measured by observing the surface of the oxidized metal layer 130 with a square of 1000nm and a height of 10nm (fixed) and using AFM is set to Ra<1nm, preferably Ra≤0.73, and more preferably Ra≤0.67nm. When plasma treatment is performed as the planarization treatment, particles adhering to the surface can also be removed.

[0196] The flatness of the metal oxide layer 130 can be evaluated using an atomic force microscope (AFM). As described in the first embodiment, the roughness curve is obtained by AFM analysis, and the arithmetic mean roughness (Ra), root mean square roughness (Rq), maximum height difference (Rmax), etc. are obtained as roughness curve parameters.

[0197] The thickness of the metal oxide layer after the planarization treatment is 1 nm to 20 nm, preferably 1 nm to 10 nm.

[0198] like Fig.24 and Fig.28 As shown, an oxide semiconductor layer 140 is formed on the planarized metal oxide layer 130 ( Figure 3 "OS film formation" in step S2004).

[0199] For example, the thickness of the oxide semiconductor layer 140 is 10 nm to 100 nm, 15 nm to 70 nm, or 20 nm to 40 nm. In this embodiment, an oxide containing indium (In) and gallium (Ga) is used as the oxide semiconductor layer 140. The oxide semiconductor layer 140 before OS annealing described below is amorphous.

[0200] When the oxide semiconductor layer 140 is crystallized by OS annealing described later, the oxide semiconductor layer 140 after film formation and before OS annealing is preferably in an amorphous state (a state in which the crystalline component of the oxide semiconductor is small). That is, the film formation conditions of the oxide semiconductor layer 140 are preferably conditions in which the oxide semiconductor layer 140 immediately after film formation is not crystallized as much as possible. For example, when the oxide semiconductor layer 140 is formed by sputtering, the oxide semiconductor layer 140 is formed under a state in which the temperature of the object to be formed (the substrate 100 and the structure formed thereon) is controlled.

[0201] When a film is formed on an object to be formed by sputtering, ions generated in the plasma and atoms recoiled from the sputtering target will collide with the object to be formed. Therefore, the temperature of the object to be formed will rise along with the film forming process. If the temperature of the object to be formed rises during the film forming process, the oxide semiconductor layer 140 contains microcrystals in the state just after the film is formed. Due to the microcrystals, the subsequent crystallization caused by OS annealing is hindered. In order to control the temperature of the object to be formed as described above, the film can also be formed while cooling the object to be formed. For example, the object to be formed can also be cooled from the surface opposite to the film forming surface in such a way that the temperature of the film forming surface of the object to be formed is below 100°C, below 70°C, below 50°C, or below 30°C. By forming the oxide semiconductor layer 140 while cooling the object to be formed as described above, it is possible to form an oxide semiconductor layer 140 with a small amount of crystalline components in the state just after the film is formed.

[0202] like Fig.24 and Fig.29 As shown, the pattern of the oxide semiconductor layer 140 is formed ( Fig.24 Although not shown in the figure, a resist mask is formed on the oxide semiconductor layer 140, and the oxide semiconductor layer 140 is etched using the resist mask. As the etching of the oxide semiconductor layer 140, wet etching or dry etching can be used. As wet etching, etching can be performed using an acidic etchant. For example, as the etchant, oxalic acid or hydrofluoric acid can be used.

[0203] After the patterning of the oxide semiconductor layer 140, the oxide semiconductor layer 140 is subjected to a heat treatment (OS annealing) ( Fig.24 In this embodiment, the oxide semiconductor layer 140 is crystallized by the OS annealing.

[0204] like Fig.24 and Fig.30 As shown, the pattern of the oxidized metal layer 130 is formed ( Fig.24 The oxide semiconductor layer 140 patterned in the above process is used as a mask to etch the metal oxide layer 130. As the etching of the metal oxide layer 130, wet etching or dry etching can be used. As the wet etching, for example, diluted hydrofluoric acid (DHF) is used. By etching the metal oxide layer 130 using the oxide semiconductor layer 140 as a mask as described above, the photolithography process can be omitted.

[0205] like Fig.24 and Fig.31 As shown, the gate insulating layer 150 ( Fig.24 GI formation in step S2008). For example, silicon oxide is formed as the gate insulating layer 150. The gate insulating layer 150 is formed by a CVD method. For example, in order to form an insulating layer with few defects as the gate insulating layer 150 as described above, the gate insulating layer 150 may be formed at a film forming temperature of 350° C. or higher. For example, the thickness of the gate insulating layer 150 is between 50 nm and 300 nm, between 60 nm and 200 nm, or between 70 nm and 150 nm. After forming the gate insulating layer 150, a process of injecting oxygen into a portion of the gate insulating layer 150 may be performed. A metal oxide layer 190 ( Fig.24 The metal oxide layer 190 is formed by sputtering. Oxygen is injected into the gate insulating layer 150 by forming the metal oxide layer 190.

[0206] For example, the thickness of the metal oxide layer 190 is 5 nm to 100 nm, 5 nm to 50 nm, 5 nm to 30 nm, or 7 nm to 15 nm. In this embodiment, aluminum oxide is used as the metal oxide layer 190. Aluminum oxide has a high barrier property against gases such as oxygen and hydrogen. In this embodiment, aluminum oxide used as the metal oxide layer 190 suppresses the diffusion of oxygen injected into the gate insulating layer 150 when the metal oxide layer 190 is formed.

[0207] For example, when the metal oxide layer 190 is formed by sputtering, the process gas used for sputtering may remain in the film of the metal oxide layer 190. For example, when Ar is used as the process gas for sputtering, Ar may remain in the film of the metal oxide layer 190. The remaining Ar can be detected by SIMS (Secondary Ion Mass Spectrometry) analysis performed on the metal oxide layer 190.

[0208] In a state where the gate insulating layer 150 is formed on the oxide semiconductor layer 140 and the metal oxide layer 190 is formed on the gate insulating layer 150, a heat treatment (oxidation annealing) for supplying oxygen to the oxide semiconductor layer 140 is performed ( Fig.24 In the process from forming the oxide semiconductor layer 140 to forming the gate insulating layer 150 on the oxide semiconductor layer 140, a large number of oxygen vacancies are generated on the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. The oxygen released from the gate insulating layers 120 and 150 by the above-mentioned oxidation annealing is supplied to the oxide semiconductor layer 140 to repair the oxygen vacancies.

[0209] Oxygen released from the gate insulating layer 120 by the oxidation annealing is blocked by the oxidized metal layer 130. Therefore, it is difficult to supply oxygen to the lower surface 142 of the oxide semiconductor layer 140. Oxygen released from the gate insulating layer 120 diffuses from the region where the oxidized metal layer 130 is not formed to the gate insulating layer 150 provided on the gate insulating layer 120, and reaches the oxide semiconductor layer 140 via the gate insulating layer 150. As a result, oxygen released from the gate insulating layer 120 is not easily supplied to the lower surface 142 of the oxide semiconductor layer 140, but is mainly supplied to the side surface 143 and the upper surface 141 of the oxide semiconductor layer 140. In addition, oxygen released from the gate insulating layer 150 by the oxidation annealing is supplied to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140. Hydrogen may be released from the gate insulating layers 110 and 120 by the above-mentioned oxidation annealing, but the hydrogen is blocked by the oxidized metal layer 130.

[0210] As described above, the oxidation annealing step can suppress oxygen supply to the lower surface 142 of the oxide semiconductor layer 140 having a small amount of oxygen vacancies, while supplying oxygen to the upper surface 141 and the side surface 143 of the oxide semiconductor layer 140 having a large amount of oxygen vacancies.

[0211] Similarly, in the above-mentioned oxidation annealing, oxygen injected into the gate insulating layer 150 is blocked by the oxidized metal layer 190. Therefore, the oxygen is suppressed from being released into the atmosphere. Therefore, through the oxidation annealing, the oxygen is efficiently supplied to the oxide semiconductor layer 140 to repair oxygen vacancies.

[0212] like Fig.24 and Fig.32 As shown, after the oxidation annealing, the oxide metal layer 190 is etched (removed) ( Fig.24 As the etching of the oxidized metal layer 190, wet etching or dry etching may be used. As the wet etching, for example, diluted hydrofluoric acid (DHF) may be used.

[0213] like Fig.24 and Fig.33 As shown, the film-forming gate electrode 160 ( Fig.24 The gate electrode 160 is formed by sputtering or atomic layer deposition and patterned by a photolithography process.

[0214] In the state where the gate electrode 160 is patterned, the resistance of the source region S and the drain region D of the oxide semiconductor layer 140 is reduced ( Fig.24Specifically, impurities are injected into the oxide semiconductor layer 140 from the gate electrode 160 side through the gate insulating layer 150 by ion implantation. For example, argon (Ar), phosphorus (P), and boron (B) are injected into the oxide semiconductor layer 140 by ion implantation. Oxygen vacancies are formed in the oxide semiconductor layer 140 by ion implantation, thereby reducing the resistance of the oxide semiconductor layer 140. Since the gate electrode 160 is provided above the oxide semiconductor layer 140 that functions as the channel region CH of the semiconductor device 10, impurities are not injected into the oxide semiconductor layer 140 in the channel region CH.

[0215] like Fig.24 and Fig.34 As shown, insulating layers 170 and 180 are formed on the gate insulating layer 150 and the gate electrode 160 as interlayer films ( Fig.24 The insulating layers 170 and 180 are formed by CVD. For example, silicon nitride is formed as the insulating layer 170, and silicon oxide is formed as the insulating layer 180. The materials used as the insulating layers 170 and 180 are not limited to the above. The thickness of the insulating layer 170 is not less than 50 nm and not more than 500 nm. The thickness of the insulating layer 180 is not less than 50 nm and not more than 500 nm.

[0216] like Fig.24 and Fig.35 As shown, openings 171 and 173 are formed in the gate insulating layer 150 and the insulating layers 170 and 180 ( Fig.24 The oxide semiconductor layer 140 in the source region S is exposed through the opening 171. The oxide semiconductor layer 140 in the drain region D is exposed through the opening 173. The source / drain electrodes 200 ( Fig.24 Step S2016 of "SD formation"), thereby completing Figure 1 A semiconductor device 10 is shown.

[0217] In the semiconductor device 10 manufactured by the above-mentioned manufacturing method, the direction and growth speed of crystal growth can be made uniform in the oxide semiconductor layer 140. As a result, when the channel length L of the channel region CH in the semiconductor device 10 is in the range of 2 μm to 4 μm and the channel width of the channel region CH is in the range of 2 μm to 25 μm, a mobility of 50 [cm 2 / Vs] or more, 55[cm 2 / Vs] or more or 60[cm 2 / Vs] or above. The mobility in this embodiment refers to the field effect mobility in the saturation region of the semiconductor device 10. Specifically, the mobility refers to the maximum value of the field effect mobility in the region where the potential difference (Vd) between the source electrode and the drain electrode is greater than the voltage (Vg) supplied to the gate electrode minus the threshold voltage (Vth) of the semiconductor device 10.

[0218] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by wet etching, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0219] μ=-10.033Ra+48.23

[0220] (Among which, the arithmetic mean roughness Ra≤0.80)

[0221] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by plasma treatment, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0222] μ=-5.9584Ra+43.978

[0223] (Among which, the arithmetic mean roughness Ra≤0.67)

[0224] In the above-mentioned manufacturing method, in the semiconductor device 10 in which the oxidized metal layer 130 is planarized by wet etching or plasma treatment, the arithmetic mean roughness Ra (nm) and the field effect mobility μ (cm 2 The relationship between s and V is expressed by the following formula.

[0225] μ=-5.770Ra+44.22

[0226] (Among which, the arithmetic mean roughness Ra≤0.73)

[0227] <Third Embodiment>

[0228] use Figure 36 to Figure 40 A display device using a semiconductor device according to an embodiment of the present invention will be described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first and second embodiments is applied to a liquid crystal display device will be described.

[0229] [Overview of Display Device 20]

[0230] Fig.36 FIG. 1 is a top view showing an overview of a display device according to an embodiment of the present invention. Fig.36 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC 330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. A plurality of pixel circuits 301 are arranged in a matrix in a liquid crystal region 22 surrounded by the sealing portion 310. The liquid crystal region 22 is a region that overlaps with a liquid crystal element 311 described later in a plan view.

[0231] The sealing region 24 provided with the sealing portion 310 is the region around the liquid crystal region 22. The FPC 330 is provided in the terminal region 26. The terminal region 26 is the region where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 24. The outside of the sealing region 24 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.

[0232] [Circuit Configuration of Display Device 20]

[0233] Fig.37 FIG. 1 is a block diagram showing a circuit configuration of a display device according to an embodiment of the present invention. Fig.37 As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 22 in the first direction D1 (column direction) with respect to the pixel circuit 301, and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 22 in the second direction D2 (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 24. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 24, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.

[0234] The source wiring 304 extends from the source driving circuit 302 along the first direction D1 and is connected to the plurality of pixel circuits 301 arranged in the first direction D1. The gate wiring 305 extends from the gate driving circuit 303 along the second direction D2 and is connected to the plurality of pixel circuits 301 arranged in the second direction D2.

[0235] The terminal region 26 is provided with a terminal portion 306. The terminal portion 306 and the source driver circuit 302 are connected via a connection wiring 307. Similarly, the terminal portion 306 and the gate driver circuit 303 are connected via a connection wiring 307. By connecting the FPC 330 to the terminal portion 306, an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0236] The semiconductor device 10 described in the first embodiment and the second embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .

[0237] [Pixel Circuit 301 of Display Device 20]

[0238] Fig.38 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.38 As shown, the pixel circuit 301 includes elements such as the semiconductor device 10, the holding capacitor 350, and the liquid crystal element 311. The semiconductor device 10 has a gate electrode 160, a source electrode 201, and a drain electrode 203. The gate electrode 160 is connected to the gate wiring 305. The source electrode 201 is connected to the source wiring 304. The drain electrode 203 is connected to the holding capacitor 350 and the liquid crystal element 311. In this embodiment, for the sake of convenience of description, the electrode represented by the figure mark "201" is called the source electrode, and the electrode represented by the figure mark "203" is called the drain electrode, but it is also possible that the electrode represented by the figure mark "201" functions as a drain electrode and the electrode represented by the figure mark "203" functions as a source electrode.

[0239] [Cross-sectional Structure of Display Device 20]

[0240] Fig.39 FIG. 1 is a cross-sectional view of a display device according to an embodiment of the present invention. Fig.39 As shown in FIG. 1 , the display device 20 is a display device using the semiconductor device 10. In this embodiment, the semiconductor device 10 is used in the pixel circuit 301, but the semiconductor device 10 can also be used in peripheral circuits including the source driver circuit 302 and the gate driver circuit 303. In the following description, the semiconductor device 10 is used in the pixel circuit 301. Figure 1 The semiconductor device 10 shown is the same and therefore its description is omitted.

[0241] An insulating layer 360 is provided on the source electrode 201 and the drain electrode 203. A common electrode 370 provided in common to a plurality of pixels is provided on the insulating layer 360. An insulating layer 380 is provided on the common electrode 370. An opening 381 is provided on the insulating layers 360 and 380. A pixel electrode 390 is provided on the insulating layer 380 and inside the opening 381. The pixel electrode 390 is connected to the drain electrode 203.

[0242] Fig.40 FIG. 1 is a top view of a pixel electrode and a common electrode of a display device according to an embodiment of the present invention. Fig.40 As shown, the common electrode 370 has an overlapping region that overlaps with the pixel electrode 390 in a plan view and a non-overlapping region that does not overlap with the pixel electrode 390. When a voltage is supplied between the pixel electrode 390 and the common electrode 370, a transverse electric field is formed from the pixel electrode 390 in the overlapping region toward the common electrode 370 in the non-overlapping region. The liquid crystal molecules included in the liquid crystal element 311 are moved by the transverse electric field, thereby determining the grayscale of the pixel.

[0243] <Fourth Embodiment>

[0244] use Fig.41 and Fig.42 A display device using a semiconductor device according to an embodiment of the present invention will be described. In this embodiment, a circuit configuration in which the semiconductor device 10 described in the first and second embodiments is applied to an organic EL display device will be described. The overview and circuit configuration of the display device 20 are related to Fig.36 and Fig.37 The contents shown are the same, so the description is omitted.

[0245] [Pixel Circuit 301 of Display Device 20]

[0246] Fig.41 FIG. 1 is a circuit diagram showing a pixel circuit of a display device according to an embodiment of the present invention. Fig.41As shown, the pixel circuit 301 includes components such as a driving transistor 11, a selection transistor 12, a holding capacitor 210 and a light-emitting element DO. The driving transistor 11 and the selection transistor 12 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 12 is connected to the signal line 211, and the gate electrode of the selection transistor 12 is connected to the gate line 212. The source electrode of the driving transistor 11 is connected to the anode power line 213, and the drain electrode of the driving transistor 11 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 11 is connected to the drain electrode of the selection transistor 12. The holding capacitor 210 is connected to the gate electrode and the drain electrode of the driving transistor 11. A grayscale signal that determines the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row to which the above-mentioned grayscale signal is to be written is supplied to the gate line 212.

[0247] [Cross-sectional Structure of Display Device 20]

[0248] Fig.42 It is a cross-sectional view of a display device according to one embodiment of the present invention. Fig.42 The display device 20 shown in FIG. Fig.39 The display device 20 shown is similar, but Fig.42 The structure above the insulating layer 360 in the display device 20 and Fig.39 The structure above the insulating layer 360 in the display device 20 is different. Fig.42 The display device 20 is configured as follows: Fig.39 The description of the same structure as the display device 20 is omitted, and the differences between the two are described.

[0249] like Fig.42 As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 (light-emitting element DO) above the insulating layer 360. The pixel electrode 390 is arranged on the insulating layer 360 and inside the opening 381. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. That is, the insulating layer 362 divides the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are arranged separately with respect to each pixel. On the other hand, the common electrode 394 is arranged in common with respect to a plurality of pixels. Different materials are used for the light-emitting layer 392 according to the display color of the pixel.

[0250] In the third and fourth embodiments, the semiconductor device described in the first and second embodiments is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device can also be applied to display devices other than the above display devices (for example, a self-luminous display device or an electronic paper display device other than an organic EL display device). In addition, unless otherwise specified, the semiconductor device can be applied to display devices ranging from small and medium-sized to large display devices.

[0251] Example

[0252] In this embodiment, refer to Figures 43 to 51 The effect of the planarization treatment performed on the surface of the metal oxide layer mainly composed of aluminum will be described. Figure 43 to Figure 46 , Figures 48 to 50 It is a graph showing the electrical characteristics of a semiconductor device. Fig.47 and Fig.51 is a box plot showing the field effect mobility of a semiconductor device.

[0253] [Relationship between the Flatness of Aluminum Oxide and the Electrical Characteristics of Semiconductor Devices]

[0254] In this embodiment, according to Fig.24 The semiconductor device 10 is formed by following the timing chart of the manufacturing method shown in FIG. 1. In the present embodiment, aluminum oxide is used as the metal oxide mainly composed of aluminum.

[0255] [Plasticization of aluminum oxide]

[0256] The conditions for the planarization treatment of aluminum oxide are as follows.

[0257] Substrate: Glass substrate

[0258] ·Aluminum oxide film thickness: 10nm, 11nm, 15nm, 50nm

[0259] Planarization condition 1 (developer (TMAH)): 1nm, 5nm, 40nm

[0260] Planarization condition 2 (Ar gas): less than 1nm, 1nm, 5nm

[0261] The thickness of aluminum oxide during film formation was set to 10 nm by performing a planarization treatment. When the thickness during film formation was 50 nm, 40 nm was removed by performing a planarization treatment, thereby setting it to 10 nm. When the thickness during film formation was 15 nm, 5 nm was removed by performing a planarization treatment, thereby setting it to 10 nm. When the thickness during film formation was 10 nm, less than 1 nm was removed by performing a planarization treatment, thereby setting it to approximately 10 nm.

[0262] [Initial characteristics]

[0263] Figure 43 to Figure 46 , Figures 48 to 50 The measurement conditions of the electrical characteristics shown are as follows.

[0264] ·Size of channel region CH: W / L=4.5μm / 3.0μm

[0265] Source-drain voltage: 0.1V, 10V

[0266] ·Gate voltage: -15V~+15V

[0267] ·Measurement environment: room temperature, dark room

[0268] ·Measurement sites: 26

[0269] First, the results of planarizing aluminum oxide using planarizing condition 1 (developer (TMAH)) will be described.

[0270] Fig.43 It is a graph showing the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device that has not been planarized. Fig.44 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by 1 nm through a planarization process. Fig.45 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by 5 nm through a planarization process. Fig.46 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by 40 nm through a planarization process. Figure 43 to Figure 46 All are the results of measuring the electrical characteristics at 26 locations within the substrate surface.

[0271] like Figure 43 to Figure 46 As indicated by the arrow in the figure, the vertical axis for the drain current (Id) is shown on the left side of the figure, and the vertical axis for the mobility calculated based on the drain current is shown on the right side of the figure.

[0272] Fig.43 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.51V. Fig.44 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.52V. Fig.45 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.53V. Fig.46 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.51V. Figure 43 to Figure 46As shown, the electrical characteristics of the semiconductor device show a so-called normally-off characteristic in which the drain current Id starts to flow when the gate voltage Vg is higher than 0V.

[0273] Fig.47 It indicates Figure 43 to Figure 46 The figure is a box plot of the distribution of mobility within the substrate surface (26 locations) of each semiconductor device shown. Fig.47 In the figure, the horizontal axis is the reference (Ref.) (untreated), the case where 1 nm, 5 nm, and 40 nm are removed, and the vertical axis is the field effect mobility (cm 2 / Vs).

[0274] like Fig.47 As shown, the average value of the mobility in the untreated case is 38.0 cm 2 / Vs, the average mobility when 1 nm of the aluminum oxide layer was removed was 38.6 cm 2 / Vs. The average mobility when 5 nm of the aluminum oxide layer was removed was 40.5 cm 2 / Vs, the average mobility when 5 nm of the aluminum oxide layer was removed was 41.0 cm 2 / Vs. Fig.47 As shown in FIG. 1 , it can be seen that the average value of the field effect mobility of the semiconductor device tends to increase according to the amount of aluminum oxide layer removed by wet etching. By removing more than 5 nm of the aluminum oxide layer, the average value of the mobility exceeds 40 cm 2 / Vs.

[0275] Next, the results of planarizing aluminum oxide under planarizing condition 2 (Ar gas) will be described.

[0276] Fig.48 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by less than 1 nm through a planarization process. Fig.49 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by 1 nm through a planarization process. Fig.50 The graph shows the electrical characteristics (Id-Vg characteristics) and mobility of a semiconductor device in which the surface of the aluminum oxide layer is removed by 5 nm through a planarization process. Figures 48 to 50 All are the results of measuring the electrical characteristics at 26 locations within the substrate surface.

[0277] like Figures 48 to 50 As indicated by the arrow in the figure, the vertical axis for the drain current (Id) is shown on the left side of the figure, and the vertical axis for the mobility calculated based on the drain current is shown on the right side of the figure.

[0278] Fig.48 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.55V. Fig.49 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.53V. Fig.50 The average threshold voltage in the substrate surface of the electrical characteristics shown is 0.55V. Figures 48 to 50 As shown, the electrical characteristics of the semiconductor device show a so-called normally-off characteristic in which the drain current Id starts to flow when the gate voltage Vg is higher than 0V.

[0279] Fig.51 It indicates Fig.43 , Figures 48 to 50 The figure is a box plot of the distribution of mobility within the substrate surface (26 locations) of each semiconductor device shown. Fig.51 The horizontal axis is the reference (untreated), the case where less than 1 nm, 1 nm, and 5 nm are removed, and the vertical axis is the field effect mobility (cm 2 / Vs).

[0280] like Fig.51 As shown, the average value of the mobility in the untreated case is 38.0 cm 2 / Vs, the average mobility when the surface of the aluminum oxide layer was removed by less than 1 nm was 39.1 cm 2 / Vs. The average mobility when 1 nm of the surface of the aluminum oxide layer was removed was 39.7 cm 2 / Vs, the average mobility when 5 nm of the aluminum oxide layer was removed was 42.4 cm 2 / Vs. It can be seen that the average value of the field effect mobility of the semiconductor device tends to increase according to the amount of aluminum oxide layer removed by plasma treatment. By removing more than 5nm of the aluminum oxide layer, the average value of the mobility exceeds 40cm 2 / Vs.

[0281] As described above, under the planarization conditions 1 and 2, by removing 5 nm or more of aluminum oxide, the average mobility of the semiconductor device 10 becomes 40 cm 2 / Vs or above.

[0282] Next, refer to Figure 52A to Figure 55 The following describes the results of verifying the correlation between the arithmetic mean roughness Ra and the field effect mobility μ after the surface of aluminum oxide is planarized.

[0283] First, an aluminum oxide layer is formed on a substrate, and the arithmetic mean roughness Ra and the root mean square roughness Rq after the aluminum oxide layer is planarized will be described.

[0284] [Plasticization of aluminum oxide]

[0285] The conditions for the planarization treatment of aluminum oxide are as follows.

[0286] Substrate: Glass substrate

[0287] ·Aluminum oxide film thickness: 10nm, 11nm, 15nm, 50nm

[0288] Planarization condition 1 (developer (TMAH)): 1nm, 5nm, 40nm

[0289] Planarization condition 2 (Ar gas): less than 1nm, 1nm, 5nm

[0290] The thickness of aluminum oxide during film formation was set to 10 nm by performing a planarization treatment. When the thickness during film formation was 50 nm, 40 nm was removed by performing a planarization treatment, thereby setting it to 10 nm. When the thickness during film formation was 15 nm, 5 nm was removed by performing a planarization treatment, thereby setting it to 10 nm. When the thickness during film formation was 10 nm, less than 1 nm was removed by performing a planarization treatment, thereby setting it to approximately 10 nm.

[0291] Fig.52A is an AFM image of the surface of the metal oxide layer after the flattening treatment according to condition 1. Fig.52B This is an AFM image of the metal oxide layer after the planarization process was performed according to condition 2. Fig.52A and Fig.52B The AFM image of the surface of the metal oxide layer shown has an observation area of ​​1000 nm square and a height of 10 nm (constant).

[0292] according to Fig.52A and Fig.52B The roughness curve was obtained by using the AFM image shown in FIG. Based on the roughness curve, the arithmetic mean roughness (Ra) and the root mean square roughness (Rq) were obtained as roughness curve parameters.

[0293] [Table 1]

[0294]

[0295] As shown in Table 1, it was confirmed that under both Condition 1 and Condition 2, the arithmetic mean roughness (Ra) and the root mean square roughness (Rq) decreased according to the amount of surface removal of the aluminum oxide layer.

[0296] Next, refer to Figure 53 to Figure 55 The following describes the results of verifying the correlation between the arithmetic mean roughness Ra of the surface of the aluminum oxide layer and the field effect mobility μ of the semiconductor device.

[0297] Fig.53 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (condition 1) and the field effect mobility of the semiconductor device. Fig.54 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (condition 2) and the field effect mobility of the semiconductor device. Fig.55 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (conditions 1 and 2) and the field effect mobility of the semiconductor device.

[0298] Fig.53 The arithmetic mean roughness Ra shown corresponds to the case where the surface of the aluminum oxide layer is removed by 1 nm, 5 nm, and 40 nm according to Condition 1 shown in Table 1 and the case of reference (untreated). In addition, the field effect mobility μ corresponds to the case where the surface of the aluminum oxide layer is removed by 1 nm, 5 nm, and 40 nm according to Condition 1 shown in Table 1. Fig.47 The results shown are those in which 1 nm, 5 nm, and 40 nm of the aluminum oxide layer were removed from the surface and in the case of a reference (untreated) layer.

[0299] Fig.54 The arithmetic mean roughness Ra shown corresponds to the case where the surface of the aluminum oxide layer is removed by less than 1 nm, 1 nm, and 5 nm according to Condition 2 shown in Table 1 and the reference (untreated). In addition, the field effect mobility μ corresponds to the case where the surface of the aluminum oxide layer is removed by less than 1 nm, 1 nm, and 5 nm according to Condition 2 shown in Table 1. Fig.51 The results shown are for the cases where less than 1 nm, 1 nm, 5 nm of the aluminum oxide layer were removed from the surface and for the reference (untreated) case.

[0300] Fig.55 This is a diagram showing the dependency between the arithmetic mean roughness (Ra) of the aluminum oxide layer obtained by the planarization process (conditions 1 and 2) and the field effect mobility of the semiconductor device. Fig.55 Yes Fig.53 The results shown and Fig.54 The results shown are summarized in the figure.

[0301] confirm Fig.53 The approximate line shown is y = -10.033x + 48.23. Fig.53 Confirm that in order to set the field effect mobility μ to 40 cm 2 / Vs or more, preferably Ra≤0.80. Fig.54The approximate line shown is y = -5.9584 + 43.978. Fig.54 Confirm that in order to set the field effect mobility μ to 40 cm 2 / Vs, preferably Ra≤0.67. Fig.55 The approximate line shown is y = -5.7697x + 44.223. Fig.55 Confirm that in order to set the field effect mobility μ to 40 cm 2 / Vs or more, preferably Ra≤0.73. Here, y represents field effect mobility, and x represents arithmetic mean roughness Ra.

[0302] [Influence of Planarization of Surface of Metal Oxide Layer on Electrical Characteristics of Semiconductor Device]

[0303] like Figure 53 to Figure 55 As shown, it is confirmed that the arithmetic mean roughness (Ra) of the surface of the aluminum oxide layer will be reduced and the field effect mobility μ will be improved by flattening according to any method in Condition 1 and Condition 2. In addition, it is confirmed that the smaller the arithmetic mean roughness (Ra) of the surface of the aluminum oxide layer, the higher the field effect mobility μ. That is, by flattening the surface of the aluminum oxide layer, the flatness of the surface of the aluminum oxide layer is improved, and by forming an oxide semiconductor layer thereon and performing a heat treatment, the direction of crystal growth can be suppressed from becoming random, and the direction of crystal growth and the growth rate can be made consistent. It is therefore believed that when a voltage is applied to the gate electrode of the semiconductor device, the main factor that hinders the movement of electrons in the oxide semiconductor layer is reduced, thereby improving the field effect mobility.

[0304] The various embodiments described above as embodiments of the present invention can be implemented in appropriate combination as long as they do not contradict each other. In addition, solutions obtained by adding, deleting or changing the design of components or adding, omitting or changing the conditions of processes based on the semiconductor devices and display devices of the various embodiments by those skilled in the art are also included in the scope of the present invention as long as they have the gist of the present invention.

[0305] Even if there are other effects different from the effects brought about by the schemes of the above-mentioned embodiments, if they are clearly known from the description of this specification or can be easily predicted by those skilled in the art, they are of course understood to be the effects brought about by the present invention.

[0306] Description of Reference Numerals

[0307] 10: semiconductor device, 11: driving transistor, 12: selecting transistor, 20: display device, 22: liquid crystal region, 24: sealing region, 26: terminal region, 100: substrate, 105, 160: gate electrode, 110, 120, 150: gate insulating layer, 130, 190: metal oxide layer, 140: oxide semiconductor layer, 141: upper surface, 142: lower surface, 143: side surface, 170, 180: insulating layer, 171, 173: opening, 200: source / drain electrode, 201: source electrode, 203: drain electrode, 210: holding capacitor, 211: signal line, 212: gate line, 213: anode Power supply line, 214: cathode power supply line, 220: resist mask, 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connection wiring, 310: sealing portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate (FPC), 340: IC chip, 350: holding capacitor, 360, 362: insulating layer, 363, 381: opening, 370: common electrode, 380: insulating layer, 390: pixel electrode, 392: light-emitting layer, 394: common electrode

Claims

1. A method for manufacturing a semiconductor device, wherein: An oxidized metal layer mainly composed of aluminum is formed on the insulating surface. The surface of the metal oxide layer is planarized. forming an oxide semiconductor layer on the surface subjected to the planarization treatment, forming a gate insulating layer on the oxide semiconductor layer, A gate electrode is formed on the gate insulating layer to face the oxide semiconductor layer.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The planarization treatment allows the surface of the metal oxide layer to have an arithmetic mean roughness Ra of 0.80 nm or less.

3. The method for manufacturing a semiconductor device according to claim 1, wherein: The planarization treatment removes the metal oxide layer by 5 nm or more from the surface of the metal oxide layer.

4. The method for manufacturing a semiconductor device according to claim 1, wherein: The planarization treatment is performed by wet etching using tetramethylammonium hydroxide, potassium hydroxide, or a mixed acid containing phosphoric acid, nitric acid, and acetic acid.

5. The method for manufacturing a semiconductor device according to claim 1, wherein: The planarization treatment is performed by plasma treatment using an inert gas or a halogen-based gas.

6. The method for manufacturing a semiconductor device according to claim 1, wherein: The thickness of the metal oxide layer after the planarization treatment is set to be not less than 1 nm and not more than 20 nm.

7. The method for manufacturing a semiconductor device according to claim 1, comprising: After forming the gate insulating layer, forming a metal oxide layer mainly composed of aluminum on the gate insulating layer, performing heat treatment in a state where the metal oxide layer is formed on the gate insulating layer, The oxidized metal layer is removed after the heat treatment.

8. A semiconductor device comprising: An aluminum-based metal oxide layer disposed on the insulating surface; an oxide semiconductor layer disposed on the metal oxide layer; a gate electrode opposed to the oxide semiconductor layer; and a gate insulating layer between the oxide semiconductor layer and the gate electrode, The arithmetic mean roughness Ra (nm) and field effect mobility μ (cm 2 The relationship between / V·s) is expressed as follows: μ=-10.033Ra+48.23 (in, Arithmetic mean roughness Ra≤0.80nm).

9. The semiconductor device according to claim 8, wherein: The thickness of the metal oxide layer is greater than or equal to 1 nm and less than or equal to 20 nm.

10. The semiconductor device according to claim 8, wherein The metal oxide layer has a barrier property against oxygen and hydrogen.

11. The semiconductor device according to claim 8, wherein The oxide semiconductor layer contains two or more metals including indium, and a ratio of indium in the two or more metals is 50% or more.

12. The semiconductor device according to claim 8, wherein The oxide semiconductor layer is an oxide semiconductor layer having crystallinity.

13. The semiconductor device according to claim 8, wherein The field effect mobility is 40cm 2 / V·s or above.

Citation Information

Patent Citations

  • Semiconductor device

    JP2016184771A

  • Semiconductor device and display device having semiconductor device

    JP2018006730A

  • Semiconductor device manufacturing method

    JP2021108405A

  • Manufacturing method for semiconductor device

    JP2021141338A

  • Semiconductor device

    JP2021153196A