Production process of high-strength precise titanium foil for low-cost 3C flexible screen
Patent Information
- Application Number
- CN202410962125.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-18
AI Technical Summary
The dimensional stability of titanium foil is poor in the rolling process, resulting in poor dimensional accuracy of titanium foil, and the concentration of internal stress leads to surface defects, affecting the strength of titanium foil.
Using a multi-channel rolling process combined with lubricant spraying technology, the high-temperature first lubricant improves the plastic deformation ability, the low-temperature second lubricant stabilizes the grain structure, reduces stress concentration and processing defects, and reduces residual stress and deformation through annealing treatment.
It improves the dimensional stability and processing accuracy of titanium foil, reduces internal stress and surface defects, and improves the strength and tensile performance of titanium foil.
Smart Images

Figure BDA0004950578460000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of foil production, and in particular to a production process of high-strength and precision titanium foil for low-cost 3C flexible screens. Background Art
[0002] Flexible screen is a new type of display technology. Compared with traditional rigid screen, it has better bendability, can realize various special-shaped designs, and is light, thin and portable. In the production process of flexible screen, flexible materials are usually selected as substrates, such as plastic substrates, glass substrates or metal substrates. Metal substrates have better application prospects in small flexible screens because their high temperature resistance is far better than that of plastic substrates and glass substrates.
[0003] Titanium foil has good high temperature resistance and flexibility, so it has become a common choice for flexible screen substrates. The rolling process has become the main production process of titanium foil due to its low production cost. However, the dimensional stability of titanium foil is poor during the rolling process, resulting in poor dimensional accuracy of titanium foil, and stress concentration inside the titanium foil, resulting in more defects on the surface of the titanium foil, affecting the strength of the titanium foil. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a low-cost production process of high-strength and precision titanium foil for 3C flexible screens.
[0005] The technical solution of the present invention is: a low-cost high-strength precision titanium foil production process for 3C flexible screens, comprising the following steps:
[0006] S1. Cutting
[0007] Using a plate or a coil as a raw material (Note: In actual production, a plate or a coil with a thickness greater than 0.4 m is generally selected for cutting, and the solution of the present invention is also mainly for a plate or a coil with a thickness greater than 0.4 m), and cleaning the raw material to obtain the cleaned raw material;
[0008] S2. Rolling
[0009] The cleaned raw material is sent to a rolling mill for multiple rolling until the raw material thickness reaches 0.05-0.1 mm to obtain a semi-finished titanium foil;
[0010] During the rolling process, when δ1≥1 / 2δ, the single-pass rolling deformation rate is 25-30%, and the first lubricant at 120-140°C is sprayed on the surface of the raw material before each rolling;
[0011] When 1 / 4δ≤δ1<1 / 2δ, the single rolling deformation rate is 10-15%, and the first lubricant of 90-100°C is sprayed on the surface of the raw material before each rolling, and the second lubricant of 10-20°C is sprayed on the surface of the raw material after each rolling and left to stand for 2-3 minutes;
[0012] When δ1<1 / 4δ, the single-pass rolling deformation rate is 5-8%, and after each rolling, the second lubricant at 5-10℃ is sprayed on the surface of the raw material and left to stand for 1-2 minutes;
[0013] Among them, δ is the initial thickness of the raw material, and δ1 is the current thickness of the raw material;
[0014] S3, Annealing
[0015] The semi-finished titanium foil is sent to a vacuum furnace for annealing. After the annealing is completed, the semi-finished titanium foil is stretched and straightened to obtain titanium foil.
[0016] Description: In the above process, when the deformation rate is large, the high-temperature first lubricant is sprayed to improve the plastic deformation ability of the raw material, reduce the difficulty of raw material processing, and improve the processing efficiency. Then, the first lubricant is used in combination with the second lubricant, so that the raw material does not need to be annealed multiple times, and the internal stress concentration of the raw material can be reduced. The two lubricants can form a protective film on the surface of the raw material, reduce the processing defects on the surface of the raw material, and when the deformation rate is small, the low-temperature second lubricant is sprayed to stabilize the grain structure, make the raw material size more stable, and improve the processing accuracy.
[0017] Furthermore, during the rolling, the rolling speed is 2-4 m / s, and the rolling force is 50-80 kN.
[0018] Note: The above rolling parameters can ensure production efficiency and reduce processing defects on the raw material surface.
[0019] Furthermore, the cleaning step is: soaking the raw material in a pickling solution for 5 to 10 minutes, and then washing and drying the raw material in sequence; the pickling solution includes, by weight percentage, 30 to 40% nitric acid, 0.3 to 0.6% hydrofluoric acid, and the remainder is water.
[0020] Note: The above cleaning steps can effectively remove the oil and oxide layer on the surface of the raw materials, reduce processing defects, and ensure the accuracy of subsequent processing.
[0021] Furthermore, the first lubricant comprises, by weight: 15 to 25 parts of stearic acid, 35 to 40 parts of trimethylolpropane oleate, 10 to 15 parts of triisooctanoin, and 4 to 8 parts of dialkyl diphenylamine;
[0022] The components of the second lubricant include, by weight: 20-25 parts of cocamidopropyl betaine, 8-12 parts of triethanolamine, 5-10 parts of pentaerythritol phosphate, 6-9 parts of sorbitan monooleate, and 30-40 parts of water.
[0023] Description: The first lubricant can make the surface of the raw material smoother, make grain boundary sliding easier, improve the plastic deformation ability of the raw material, and facilitate the expansion of plastic deformation. The second lubricant can absorb the temperature generated by material deformation, stabilize the grain structure, and reduce the shrinkage of the raw material after rolling. When the first lubricant is used in combination with the second lubricant, it can reduce the internal stress concentration of the raw material, form a protective film on the surface of the raw material, and reduce the processing defects on the surface of the raw material.
[0024] Furthermore, when δ1≥1 / 2δ, the spraying amount of the first lubricant is 300-400 ml / m 2 ;
[0025] When 1 / 4δ≤δ1<1 / 2δ, the spraying amount of the first lubricant is 200~250ml / m 2 The spraying amount of the second lubricant is 150~200ml / m 2 ;
[0026] When δ1<1 / 4δ, the spraying amount of the second lubricant is 100~150ml / m 2 .
[0027] Note: By limiting the spraying amount of the first lubricant and the second lubricant, the performance of the titanium foil can be ensured while reducing the waste of the first lubricant and the second lubricant.
[0028] Furthermore, the annealing method is: at a vacuum degree of ≤1.0×10 -4 Under Pa conditions, the semi-finished titanium foil is kept at 550-580°C for 30-40 minutes, then cooled to 320-340°C along with the furnace, and then air-cooled to room temperature.
[0029] Description: Annealing treatment can reduce the residual stress in the titanium foil, refine the grains, improve the toughness of the titanium foil, and reduce the deformation and cracks on the surface of the titanium foil.
[0030] Furthermore, the cooling rate during the furnace cooling process is 6 to 9° C. / min.
[0031] Note: Limiting the cooling rate can prevent the titanium foil from deformation and cracking due to excessively fast cooling rate, thus ensuring the annealing effect.
[0032] Furthermore, the straightening tension of the tension leveling is 60-80 kN, and the tensile deformation rate is 0.05-0.1%.
[0033] Description: Tensile straightening can eliminate wrinkles and curls on titanium foil and make the thickness of titanium foil uniform.
[0034] The beneficial effects of the present invention are:
[0035] (1) In the process of the present invention, when the deformation rate is large, a high-temperature first lubricant is sprayed to improve the plastic deformation ability of the raw material. The two lubricants are used in combination to reduce the internal stress concentration of the raw material and the processing defects on the surface of the raw material. When the deformation rate is small, a low-temperature second lubricant is sprayed to make the raw material size more stable and improve the processing accuracy.
[0036] (2) The first lubricant of the present invention can improve the plastic deformation ability of the raw material, and the second lubricant can stabilize the size of the raw material and reduce the shrinkage of the raw material after rolling. When the first lubricant and the second lubricant are used together, they can reduce the internal stress concentration of the raw material and form a protective film on the surface of the raw material, thereby reducing the processing defects on the surface of the raw material. DETAILED DESCRIPTION
[0037] In order to further illustrate the method adopted by the present invention and the effect achieved, the technical solution of the present invention will be clearly and completely described in combination with experiments below.
[0038] Embodiment 1: A low-cost high-strength precision titanium foil production process for 3C flexible screens, comprising the following steps:
[0039] S1. Cutting
[0040] A 1.0 mm plate is used as a raw material, and the raw material is cleaned to obtain a cleaned raw material; wherein the cleaning step is: placing the raw material in a pickling solution and soaking it for 8 minutes, and then washing and drying the raw material in sequence; the pickling solution includes, by weight percentage, 35% nitric acid, 0.5% hydrofluoric acid, and the balance is water;
[0041] S2. Rolling
[0042] As shown in Table 1 below, the cleaned raw material is sent to a rolling mill for 19 rolling passes until the raw material thickness reaches 0.1 mm to obtain a semi-finished titanium foil;
[0043] During the rolling process, when δ1≥1 / 2δ, the single-pass rolling deformation rate is 25-30%, and the first lubricant at 130°C is sprayed on the surface of the raw material before each rolling, and the spraying amount of the first lubricant is 350ml / m 2 ;
[0044] When 1 / 4δ≤δ1<1 / 2δ, the single rolling deformation rate is 10-15%, and the first lubricant at 95℃ is sprayed on the raw material surface before each rolling, and the second lubricant at 15℃ is sprayed on the raw material surface after each rolling and left to stand for 2.5 minutes. The spraying amount of the first lubricant is 220ml / m 2 The spraying amount of the second lubricant is 170ml / m 2 ;
[0045] When δ1<1 / 4δ, the single-pass rolling deformation rate is 5-8%. After each rolling, the second lubricant at 8°C is sprayed on the surface of the raw material and left to stand for 1.5 minutes. The spraying amount of the second lubricant is 120ml / m 2 ;
[0046] Among them, δ is the initial thickness of the raw material, δ1 is the current thickness of the raw material; the rolling speed during rolling is 3m / s, and the rolling force is 65kN;
[0047] Table 1 Rolling deformation rate data of each pass in this embodiment
[0048]
[0049] S3, Annealing
[0050] The semi-finished titanium foil is sent to a vacuum furnace for annealing. After the annealing is completed, the semi-finished titanium foil is straightened to obtain the titanium foil. The annealing method is: at a vacuum degree of 1.0×10 -4 Under the conditions of Pa, the semi-finished titanium foil was kept at 560°C for 35 minutes, then cooled to 330°C with the furnace, the cooling rate during the furnace cooling process was 7°C / min, and then air-cooled to room temperature; the straightening tension of the straightening was 70kN, and the tensile deformation rate was 0.08%;
[0051] The first lubricant comprises, by weight, 20 parts of stearic acid, 38 parts of trimethylolpropane oleate, 12 parts of triisooctanoin, and 6 parts of dialkyl diphenylamine;
[0052] The components of the second lubricant include, by weight: 23 parts of cocamidopropyl betaine, 10 parts of triethanolamine, 8 parts of pentaerythritol phosphate, 7 parts of sorbitan monooleate, and 35 parts of water.
[0053] Example 2: This example is basically the same as Example 1, except that, when δ1≥1 / 2δ, the temperature of the first lubricant is 120°C; when 1 / 4δ≤δ1<1 / 2δ, the temperature of the first lubricant is 90°C and the temperature of the second lubricant is 10°C; when δ1<1 / 4δ, the temperature of the second lubricant is 5°C.
[0054] Example 3: This example is basically the same as Example 1, except that, when δ1≥1 / 2δ, the temperature of the first lubricant is 140°C; when 1 / 4δ≤δ1<1 / 2δ, the temperature of the first lubricant is 100°C and the temperature of the second lubricant is 20°C; when δ1<1 / 4δ, the temperature of the second lubricant is 10°C.
[0055] Example 4: This example is basically the same as Example 1, except that when δ1≥1 / 2δ, the spraying amount of the first lubricant is 300ml / m 2; When 1 / 4δ≤δ1<1 / 2δ, the spraying amount of the first lubricant is 200ml / m 2 The spraying amount of the second lubricant is 150ml / m 2 ; When δ1<1 / 4δ, the spraying amount of the second lubricant is 100ml / m 2 .
[0056] Example 5: This example is basically the same as Example 1, except that when δ1≥1 / 2δ, the spraying amount of the first lubricant is 400ml / m 2 ; When 1 / 4δ≤δ1<1 / 2δ, the spraying amount of the first lubricant is 250ml / m 2 The spraying amount of the second lubricant is 200ml / m 2 ; When δ1<1 / 4δ, the spraying amount of the second lubricant is 150ml / m 2 .
[0057] Example 6: This example is basically the same as Example 1, except that the components of the first lubricant include, by weight: 15 parts of stearic acid, 35 parts of trimethylolpropane oleate, 10 parts of triethylhexanoin, and 4 parts of dialkyl diphenylamine.
[0058] Example 7: This example is basically the same as Example 1, except that the first lubricant comprises, by weight, 25 parts of stearic acid, 40 parts of trimethylolpropane oleate, 15 parts of triethylhexanoin, and 8 parts of dialkyl diphenylamine.
[0059] Example 8: This example is basically the same as Example 1, except that the components of the second lubricant include, by weight: 20 parts of cocamidopropyl betaine, 8 parts of triethanolamine, 5 parts of pentaerythritol phosphate, 6 parts of sorbitan monooleate, and 30 parts of water.
[0060] Example 9: This example is basically the same as Example 1, except that the components of the second lubricant include, by weight: 25 parts of cocamidopropyl betaine, 12 parts of triethanolamine, 10 parts of pentaerythritol phosphate, 9 parts of sorbitan monooleate, and 40 parts of water.
[0061] Example 10: This example is basically the same as Example 1, except that the semi-finished titanium foil is kept at 550° C. for 35 minutes.
[0062] Example 11: This example is basically the same as Example 1, except that the semi-finished titanium foil is kept at 580°C for 35 minutes.
[0063] Example 12: This example is basically the same as Example 1, except that the semi-finished titanium foil is cooled to 320°C in the furnace, and the cooling rate during the furnace cooling process is 6°C / min.
[0064] Example 13: This example is basically the same as Example 1, except that the semi-finished titanium foil is cooled to 340°C in the furnace, and the cooling rate during the furnace cooling process is 9°C / min.
[0065] Example 14: This example is basically the same as Example 1, except that the thickness of the raw material is 0.8 mm.
[0066] Example 15: This example is basically the same as Example 1, except that the thickness of the raw material is 1.2 mm.
[0067] Comparative Example 1: This embodiment is basically the same as Example 1, except that when δ1≥1 / 2δ, the single-pass rolling deformation rate is 20-25%; when 1 / 4δ≤δ1<1 / 2δ, the single-pass rolling deformation rate is 5-10%; when δ1<1 / 4δ, the single-pass rolling deformation rate is 2-5%.
[0068] Comparative Example 2: This embodiment is basically the same as Example 1, except that, when δ1≥1 / 2δ, the single-pass rolling deformation rate is 30-35%; when 1 / 4δ≤δ1<1 / 2δ, the single-pass rolling deformation rate is 15-20%; when δ1<1 / 4δ, the single-pass rolling deformation rate is 8-12%.
[0069] Comparative Example 3: This embodiment is basically the same as Embodiment 1, except that the single-pass rolling deformation rate is 10-15% throughout the entire process.
[0070] Comparative Example 4: This embodiment is basically the same as Embodiment 1, except that the temperature of the first lubricant is always 95°C, and the temperature of the second lubricant is always 15°C.
[0071] Comparative Example 5: This embodiment is basically the same as Embodiment 1, except that the spraying amount of the first lubricant is always 220 ml / m 2 The spraying amount of the second lubricant is always 170ml / m 2 .
[0072] Comparative Example 6: This embodiment is substantially the same as Embodiment 1, except that the first lubricant is used instead of the second lubricant.
[0073] Comparative Example 7: This embodiment is substantially the same as Embodiment 1, except that a second lubricant is used instead of the first lubricant.
[0074] Comparative Example 8: This embodiment is substantially the same as Embodiment 1, except that commercially available rolling lubricant is used to replace the first lubricant and the second lubricant.
[0075] Comparative Example 9: This embodiment is basically the same as Example 1, except that the semi-finished titanium foil is kept at 560° C. for 35 minutes and then directly taken out of the furnace and air-cooled.
[0076] Experimental Example: In order to explore the influence of the process parameters of each embodiment on the performance of the titanium foil, the performance test of the titanium foil prepared in each embodiment was carried out, and the specific exploration is as follows:
[0077] 1. Investigate the influence of rolling deformation rate range on the performance of titanium foil
[0078] Using Example 1 and Comparative Examples 1 to 4 as experimental comparisons, the properties of titanium foil under different rolling deformation rate ranges are shown in Table 2 below:
[0079] Table 2 Titanium foil properties under different rolling deformation rate ranges
[0080] Group Tensile strength / Mpa Thickness tolerance / mm Example 1 512 ±0.004 Comparative Example 2 514 ±0.004 Comparative Example 3 483 ±0.008 Comparative Example 4 445 ±0.030
[0081] It can be seen from the data in Table 2 that, compared with Comparative Examples 2 and 3, as the range of single-pass rolling deformation rate decreases, the tensile strength of the titanium foil gradually increases and the thickness tolerance gradually decreases in Example 1. The tensile strength of Example 1 is the highest and the thickness tolerance is the smallest, which indicates that the titanium foil of Example 1 has the highest strength and the best dimensional accuracy. As the range of single-pass rolling deformation rate continues to decrease, the performance of the titanium foil begins to have no obvious change. However, the decrease in the range of single-pass rolling deformation rate will lead to an increase in the number of rolling times. Therefore, from a cost perspective, the rolling deformation rate range selected in Example 1 is optimal.
[0082] Compared with Example 4, in Example 1, after the deformation rate range of a single rolling process does not change, the tensile strength of the titanium foil decreases and the dimensional tolerance increases. This may be because the processing method in which the deformation rate range of the rolling process changes can reduce internal defects of the titanium foil and result in less shrinkage after rolling.
[0083] 2. Investigate the effects of the temperature and spraying amount of the first lubricant and the second lubricant on the performance of titanium foil
[0084] Using Examples 1 to 5 and Comparative Examples 4 and 5 as experimental comparisons, the titanium foil performances of the first lubricant and the second lubricant at different temperatures and different spraying amounts are shown in Table 3 below:
[0085] Table 3 Titanium foil properties at different temperatures and spraying amounts of the first lubricant and the second lubricant
[0086] Group Tensile strength / Mpa Thickness tolerance / mm Example 1 512 ±0.004 Example 2 503 ±0.006 Example 3 495 ±0.006 Example 4 505 ±0.005 Example 5 490 ±0.006 Comparative Example 4 472 ±0.009 Comparative Example 5 476 ±0.008
[0087] It can be seen from the data in Table 3 that the temperature and spraying amount of the first lubricant and the second lubricant will affect the performance of the titanium foil. Too high or too low temperature and too high or too low spraying amount of the first lubricant and the second lubricant will lead to a decrease in the strength of the titanium foil and a deterioration in the dimensional accuracy. The titanium foil of Example 1 has the highest strength and the best dimensional accuracy. Therefore, the temperature and spraying amount of the first lubricant and the second lubricant selected in Example 1 are optimal.
[0088] In Example 1, compared with Comparative Examples 4 and 5, keeping the temperature and spraying amount of the first lubricant and the second lubricant constant will lead to a decrease in the strength of the titanium foil and a deterioration in the dimensional accuracy. This may be because keeping the temperature and spraying amount of the first lubricant and the second lubricant constant will cause the plastic deformation capacity of the titanium foil to not match the deformation amount, resulting in defects in the titanium foil processing process.
[0089] 3. Investigate the effect of the ratio of the first lubricant to the second lubricant on the performance of titanium foil
[0090] Using Example 1, Examples 6 to 9 and Comparative Examples 6 to 8 as experimental comparisons, the titanium foil properties under different composition ratios of the first lubricant and the second lubricant are shown in Table 4 below:
[0091] Table 4 Titanium foil properties under different composition ratios of the first lubricant and the second lubricant
[0092] Group Tensile strength / Mpa Thickness tolerance / mm Example 1 512 ±0.004 Example 6 503 ±0.006 Example 7 496 ±0.006 Example 8 504 ±0.005 Example 9 498 ±0.007 Comparative Example 6 479 ±0.009 Comparative Example 7 473 ±0.011 Comparative Example 8 432 ±0.018
[0093] It can be seen from the data in Table 4 that the composition ratio of the first lubricant and the second lubricant will affect the performance of the titanium foil. The titanium foil of Example 1 has the highest strength and the best dimensional accuracy. Therefore, the composition ratio of the first lubricant and the second lubricant selected in Example 1 is optimal.
[0094] Compared with Comparative Examples 6 and 7, Example 1 shows that the use of only the first lubricant or the second lubricant will lead to a decrease in the strength of the titanium foil and a deterioration in the dimensional accuracy. This may be because the use of only one lubricant cannot improve the plastic deformation ability of the titanium foil and cannot stabilize the size of the titanium foil. Compared with Comparative Example 8, after using commercially available rolling lubricants to replace the first lubricant and the second lubricant in Example 1, the strength of the titanium foil is significantly reduced and the dimensional accuracy is significantly deteriorated. This may be because commercially available rolling lubricants cannot improve the plastic deformation ability of the titanium foil. Therefore, the first lubricant and the second lubricant in Example 1 are optimal.
[0095] 4. Investigate the influence of annealing parameters on the performance of titanium foil
[0096] Using Example 1, Examples 10 to 13 and Comparative Example 9 as experimental comparisons, the properties of the titanium foil under different annealing parameters are shown in Table 5 below:
[0097] Table 5 Titanium foil properties under different annealing parameters
[0098] Group Tensile strength / Mpa Thickness tolerance / mm Example 1 512 ±0.004 Example 10 497 ±0.007 Embodiment 11 492 ±0.006 Example 12 501 ±0.005 Example 13 499 ±0.006 Comparative Example 9 468 ±0.009
[0099] It can be seen from the data in Table 5 that the annealing parameters will affect the performance of the titanium foil. If the holding temperature is too high or too low, or the cooling rate is too fast or too slow, the strength of the titanium foil will decrease and the dimensional accuracy will deteriorate. Therefore, the annealing parameters selected in Example 1 are optimal.
[0100] Compared with Comparative Example 9, Example 1 shows that the strength of the titanium foil decreases and the dimensional accuracy deteriorates after direct air cooling. This may be because the cooling speed is too fast, resulting in more cracks inside the titanium foil. Therefore, the annealing method selected in Example 1 is the best.
[0101] 5. Explore the influence of raw material thickness on titanium foil performance
[0102] Using Example 1 and Examples 14-15 as experimental comparisons, the titanium foil properties under different raw material thicknesses are shown in Table 6 below:
[0103] Table 6 Titanium foil properties at different raw material thicknesses
[0104] Group Tensile strength / Mpa Thickness tolerance / mm Example 1 512 ±0.004 Embodiment 14 506 ±0.005 Embodiment 15 515 ±0.004
[0105] It can be seen from the data in Table 6 that selecting thicker raw materials will lead to a decrease in the strength of the titanium foil and a deterioration in dimensional accuracy. Selecting thinner raw materials will result in a similar performance difference in the titanium foil finally prepared, but the cost of using thinner raw materials is higher. Therefore, the raw material thickness selected in Example 1 is optimal.
Claims
1. A low-cost high-strength precision titanium foil production process for 3C flexible screens, characterized in that: The following steps are involved: S1. Cutting Using a plate or a coil as a raw material, and cleaning the raw material to obtain a cleaned raw material; S2. Rolling The cleaned raw material is sent to a rolling mill for multiple rolling until the raw material thickness reaches 0.05-0.1 mm to obtain a semi-finished titanium foil; During the rolling process, when δ1≥1 / 2δ, the single-pass rolling deformation rate is 25-30%, and the first lubricant at 120-140°C is sprayed on the surface of the raw material before each rolling; When 1 / 4δ≤δ1<1 / 2δ, the single rolling deformation rate is 10-15%, and the first lubricant of 90-100°C is sprayed on the surface of the raw material before each rolling, and the second lubricant of 10-20°C is sprayed on the surface of the raw material after each rolling and left to stand for 2-3 minutes; When δ1<1 / 4δ, the single-pass rolling deformation rate is 5-8%, and after each rolling, the second lubricant at 5-10℃ is sprayed on the surface of the raw material and left to stand for 1-2 minutes; Among them, δ is the initial thickness of the raw material, and δ1 is the current thickness of the raw material; S3, Annealing The semi-finished titanium foil is sent to a vacuum furnace for annealing. After the annealing is completed, the semi-finished titanium foil is stretched and straightened to obtain titanium foil.
2. According to claim 1, a low-cost high-strength precision titanium foil production process for 3C flexible screens is characterized in that: During the rolling, the rolling speed is 2-4 m / s, and the rolling force is 50-80 kN.
3. According to claim 1, a low-cost high-strength precision titanium foil production process for 3C flexible screens is characterized in that: The cleaning step is: soaking the raw material in a pickling solution for 5 to 10 minutes, then washing and drying the raw material in sequence; the pickling solution comprises, by weight percentage, 30 to 40% nitric acid, 0.3 to 0.6% hydrofluoric acid, and the remainder water.
4. The low-cost high-strength precision titanium foil production process for 3C flexible screens according to claim 1 is characterized in that: The first lubricant comprises, by weight: 15 to 25 parts of stearic acid, 35 to 40 parts of trimethylolpropane oleate, 10 to 15 parts of triisooctanoin, and 4 to 8 parts of dialkyl diphenylamine; The components of the second lubricant include, by weight: 20-25 parts of cocamidopropyl betaine, 8-12 parts of triethanolamine, 5-10 parts of pentaerythritol phosphate, 6-9 parts of sorbitan monooleate, and 30-40 parts of water.
5. The low-cost high-strength precision titanium foil production process for 3C flexible screens according to claim 4 is characterized in that: When δ1≥1 / 2δ, the spraying amount of the first lubricant is 300~400ml / m 2 ; When 1 / 4δ≤δ1<1 / 2δ, the spraying amount of the first lubricant is 200~250ml / m 2 The spraying amount of the second lubricant is 150~200ml / m 2 ; When δ1<1 / 4δ, the spraying amount of the second lubricant is 100~150ml / m 2 .
6. The low-cost high-strength precision titanium foil production process for 3C flexible screens according to claim 1 is characterized in that: The annealing method is: in a vacuum degree of ≤1.0×10 -4 Under Pa conditions, the semi-finished titanium foil is kept at 550-580°C for 30-40 minutes, then cooled to 320-340°C along with the furnace, and then air-cooled to room temperature.
7. The low-cost high-strength precision titanium foil production process for 3C flexible screens according to claim 6 is characterized in that: The cooling rate during the furnace cooling process is 6-9°C / min.
8. The low-cost high-strength precision titanium foil production process for 3C flexible screens according to claim 1 is characterized in that: The straightening tension of the tension leveling is 60-80 kN, and the tensile deformation rate is 0.05-0.1%.
Citation Information
Patent Citations
Production method of titanium alloy cold-rolled strip for folding screen
CN115889460A
Production of titanium foil excellent in formability and having high brightness
JP1992110454A
Method for manufacturing titanium material, and lubricant
JP2003236604A
Titanium sheet with excellent formability and lubricity, and its manufacturing method
JP2004244671A
Titanium or titanium alloy sheet with an excellent balance of press formability and strength.
JP4452753B1