Soldering paste with low voidage, preparation method of soldering paste and application of soldering paste in electronic component packaging

By employing a finely ball-milled and chemically plated solder paste formulation, combined with precise printing and reflow soldering parameters, the problems of high void ratio and insufficient strength in solder paste have been solved, achieving highly reliable and stable soldering results.

CN118893362AActive Publication Date: 2024-11-05SHENZHEN VITAL NEW MATERIAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411130897.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-05
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Existing solder pastes suffer from high void ratios, poor thermal conductivity, and poor mechanical strength, resulting in insufficient mechanical strength of solder joints, increased maintenance costs, and negatively impacting user satisfaction.

Method used

By employing a specific ratio of tin, silver, and copper metal powders combined with flux and additives, including polyethylene glycol, environmentally friendly rosin, silane coupling agents, silver nanoparticles, and carbon nanotubes, and through processes such as fine ball milling, chemical plating, and vacuum degassing, the metal powders are ensured to be uniformly mixed and the flux is fully dispersed, controlling the particle size within the range of 20-38μm. Combined with precise printing and reflow soldering parameters, the soldering process is optimized.

Benefits of technology

It significantly reduces the void rate of solder joints, improves the mechanical strength and electrical stability of solder joints, enhances thermal conductivity, meets environmental protection requirements, maintains the stability of solder paste performance, and improves welding reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118893362A_ABST
    Figure CN118893362A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of soldering paste, and discloses low-void-rate soldering paste and a preparation method and application thereof in electronic component packaging, and materials of the low-void-rate soldering paste comprise metal powder, a soldering flux component and an additive; and the metal powder comprises 96.5% of tin, 3.0% of silver and 0.5% of copper. According to the soldering paste with the low void rate, the preparation method of the soldering paste and the application of the soldering paste in electronic component packaging, due to the fact that fine metal powder treatment and specific scaling powder configuration are adopted, the void rate in a welding spot can be remarkably reduced in the welding process of an electronic assembly; the low voidage directly improves the mechanical strength and the electrical stability of the welding spot, so that higher connection reliability is provided, the nano-silver particles and the carbon nanotubes are added as additives, the mechanical strength of the welding spot is enhanced, the heat conductivity and the conductivity are optimized, and the service life of the welding spot is prolonged. Environment-friendly rosin and a silane coupling agent are used as an activating agent and an antioxidant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tin solder paste, in particular to a tin solder paste with low void ratio, a preparation method thereof and application in electronic component packaging. Background Art

[0002] Solder paste is a material widely used in the field of electronic manufacturing. It is mainly used in surface mount technology to achieve welding connections between electronic components and printed circuit boards (PCBs). It is a slurry composed of fine metal powder (usually based on tin, with alloy elements such as silver and copper added) and a series of chemical fluxes.

[0003] Existing solder pastes have a high void rate and poor thermal conductivity and mechanical strength. Solder pastes often have a high void rate due to trapped gas or separation of solder paste components. The voids will significantly affect the mechanical strength and electrical properties of the solder joints. In addition, traditional solder pastes have insufficient welding strength due to uneven mixing of metal powders or inappropriate flux ratios, which leads to early failure of solder joints during use, increases maintenance costs and affects user satisfaction. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A solder paste with low void rate, the material of which includes metal powder, flux component and additives;

[0007] Metal powder: tin 96.5%, silver 3.0%, copper 0.5%;

[0008] Particle size range: 20-38μm;

[0009] Flux components: 2.5% polyethylene glycol (PEG) as a binder, 0.5% environmentally friendly rosin as an activator, and 0.1% high-efficiency antioxidant (including silane coupling agent);

[0010] Additives: 1.0% of nano silver particles (for improving welding strength and reducing void ratio) and 0.1% of trace carbon nanotubes (for improving thermal conductivity and mechanical strength).

[0011] A method for preparing a solder paste with low void ratio, comprising:

[0012] S1. Metal powder pretreatment;

[0013] S2, flux and additive configuration;

[0014] S3, mixing metal powder and flux;

[0015] S4, degassing and viscosity adjustment;

[0016] S5. Packaging.

[0017] As a further solution of the present invention: in the step S1, weigh Sn96.5Ag3.0Cu0.5 alloy: tin (96.5%), silver (3%), copper (0.5%), use a high-precision electronic scale to weigh each element, and the error is controlled within ±0.1g, put all the metal powders into a ball mill in an argon atmosphere, set the ball milling speed to 400 rpm, and continue ball milling for 24 hours to ensure that the metal particles are fully refined and evenly mixed;

[0018] Using the chemical plating method, the metal powder is immersed in a solution containing a silane coupling agent, the temperature is controlled at room temperature (25°C), and the reaction is allowed to stand for 30 minutes. The powder is then taken out of the solution and placed in an oven at 60°C for 4 hours to cure the surface treatment layer.

[0019] As a further solution of the present invention: in the step S2, according to 2.5% PEG, 0.5% environmentally friendly rosin and 0.1% antioxidant, if the total mass is 1kg, 25g PEG, 5g rosin and 1g antioxidant are weighed respectively, and after uniform distribution, they are heated to 60°C and stirred continuously until completely dissolved;

[0020] 10 g of nanosilver particles and 1 g of carbon nanotubes were added and dispersed at a speed of 5000 rpm for 30 minutes using a high-speed disperser to ensure that the additives were fully dispersed in the flux without aggregation.

[0021] As a further solution of the present invention: in the step S3, the pretreated metal powder is slowly added to the flux mixture at 40° C., and mixed with a stirrer at a speed of 200 rpm for 60 minutes to ensure thorough fusion;

[0022] In step S4, the mixture is placed in a vacuum degassing machine, the pressure is set to -0.1 MPa, and the degassing effect is observed and recorded to ensure that no significant bubbles are generated. If necessary, the viscosity is adjusted according to the rheometer results, and the viscosity of the final product is controlled by appropriately increasing or decreasing the amount of PEG.

[0023] As a further solution of the present invention: in the step S5, in a dust-free environment, the solder paste is divided into small containers and stored in sealed containers to avoid air contact and contamination, the printing performance test is carried out according to the welding standard, and the completed solder joints are subjected to X-ray inspection and microstructure analysis to ensure that the solder joints have low void rate and good mechanical properties.

[0024] As a further solution of the present invention: the particle size range of the metal powder is obtained by the following steps:

[0025] S11. Calculate the average particle size of the metal powder based on the speed and time setting of the ball mill, where the average particle size (D) is calculated by the formula D = 20 + 18 × (speed / 400) 0.5 ×(time / 24) 1 Sure;

[0026] S12, adjusting the rotation speed and time of the ball mill so that the calculated average particle size (D) is greater than or equal to 20 μm and less than or equal to 38 μm;

[0027] S13, verify the particle size distribution by sieving method to ensure that more than 90% of the metal powder particle size is within the range of 2038μm;

[0028] S14: If the particle size distribution does not meet the requirements, return to step S11 to readjust the speed and time of the ball mill.

[0029] As a further solution of the present invention: in the step S11, when the calculated average particle size (D) is less than 20 μm, the rotation speed of the ball mill is increased;

[0030] When the calculated average particle size (D) is greater than 38 μm, reduce the speed of the ball mill;

[0031] In the step S12, if the adjusted average particle size (D) is still not within the range of 2038 μm, the ball milling time is further adjusted, wherein the ball milling time (T) is determined by the formula T=24×(38D) / D20);

[0032] In step S13, if the particle size distribution does not meet the requirements after verification by the screening method, the speed and time of the ball mill are adjusted according to the screening results, wherein the speed (R) is calculated by the formula R = 400 × 38D max ) / (D min 20) Determine, where D max and D min are the maximum and minimum particle sizes, respectively;

[0033] In step S14, if the particle size distribution requirement cannot be met after multiple adjustments, it is necessary to check the working state of the ball mill or replace the metal raw material to ensure that the particle size range of the final metal powder meets the standard of 2038 μm.

[0034] The invention discloses an application of tin solder paste in electronic component packaging, wherein the tin solder paste is applied to Ball Grid Array (BGA) packaging technology.

[0035] As a further solution of the present invention: its application method is as follows:

[0036] (1) Preparation: Ensure that the surface of the circuit board (PCB) to be soldered and the bottom of the BGA component are clean and dust-free, and select a suitable solder paste printing template. The template design should be based on the size and arrangement of the solder joints of the BGA component;

[0037] (2) Printing solder paste: Use a printer or a manual scraper to evenly distribute the precisely configured low voiding solder paste to the predetermined solder joint locations on the PCB. By precisely controlling the printing pressure, speed, and angle, ensure that the solder paste transfer through the holes of the template is accurate.

[0038] (3) Placing BGA components: Use precision placement equipment (pick-and-place machine) to accurately place BGA components on the corresponding position of the PCB printed with solder paste;

[0039] (4) Reflow soldering: Send the PCB with BGA components into the reflow soldering furnace and set a reasonable temperature curve according to the specific composition and performance of the solder paste;

[0040] (41) Preheating stage: The temperature is gradually increased to drive out the solvent in the solder paste;

[0041] (42) Liquid welding stage: reaching the melting point of the solder paste, melting the metal powder to form a good welding connection;

[0042] (43) Cooling stage: Slowly cool down to avoid solder joint stress

[0043] (5) Inspection and quality control: After reflow soldering, the solder joints under the BGA components are inspected using X-ray inspection equipment to verify whether the internal void rate of the solder joints is low and the connectivity is good. For BGA components with key functions, electrical performance tests can also be performed to ensure that soldering does not affect component performance.

[0044] As a further solution of the present invention: Step (2) printing the solder paste based on precise control of printing parameters comprises:

[0045] Adjust the pressure P of the printing press to the set range [Pmin, Pmax];

[0046] Control the printing speed V to be within Vopt±ΔV;

[0047] Determine that the printing angle θ meets the requirement of θopt±Δθ;

[0048] Ensure that the solder paste transfer rate T meets the conditions in the [Tmin, Tmax] range.

[0049] As a further solution of the present invention: Step (3) placing the BGA component based on the control of position accuracy includes:

[0050] Set the positioning accuracy E of the placed device to Eopt±ΔE;

[0051] Confirm that the relative position deviation Δd between the BGA component and the PCB is less than the maximum allowable deviation Δd max ;

[0052] Adjust the vertical descent speed S of the placement head to Sopt±ΔS;

[0053] Monitor the horizontal offset Δx and Δy of BGA components during placement to ensure Δx 2 +Δy 2 <(Δd m ax) 2 .

[0054] As a further solution of the present invention: Step (4) reflow soldering based on the optimization of the temperature curve comprises:

[0055] The rising rate R1 of the temperature T1 in the preheating stage is controlled at R1opt±ΔR1;

[0056] The temperature T2 in the liquid soldering stage reaches Tmelt±ΔTmelt, where Tmelt is the melting point of the solder paste;

[0057] The decreasing rate R3 of the temperature T3 in the cooling stage is controlled at R3opt±ΔR3;

[0058] Monitor the actual temperature curve T(t) during reflow soldering to ensure that T(t) is consistent with the target temperature curve T t The deviation ΔT(t) of arget(t) satisfies |ΔT(t)|<ΔT m ax.

[0059] As a further solution of the present invention: Step (5) detection and quality control is based on the evaluation of solder joint void rate, including:

[0060] Using X-ray inspection equipment to obtain solder joint image I;

[0061] Apply image processing algorithm to calculate the void ratio H of solder joints;

[0062] Determine whether the void rate H of the solder joint satisfies H≤Hmax, where Hmax is the maximum allowable void rate value;

[0063] If H>Hmax, the solder joint is marked as a failed solder joint and the position information Pfail is recorded.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] Due to the use of fine metal powder processing and specific flux configuration, the tin solder paste of the present invention can significantly reduce the void rate in the solder joint during the soldering process of electronic components. This low void rate directly improves the mechanical strength and electrical stability of the solder joint, thereby providing higher connection reliability. The addition of nano silver particles and carbon nanotubes as additives not only enhances the mechanical strength of the solder joint, but also optimizes the thermal conductivity and electrical conductivity. By using environmentally friendly rosin and silane coupling agents as activators and antioxidants, the present invention not only meets the current stringent environmental protection requirements, but also can effectively prevent the oxidation of the solder paste during storage and use, and maintain the stability and consistency of its performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 It is a flow chart of the method for preparing solder paste of the present invention;

[0067] Figure 2 This is a flow chart of the application method of the solder paste of the present invention in electronic component packaging;

[0068] Figure 3 The present invention is a flow chart of a reflow soldering method for applying the solder paste of the present invention in electronic component packaging. DETAILED DESCRIPTION

[0069] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and understandable, the specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings.

[0070] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0071] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0072] Example 1

[0073] See also Figure 1 , which is the first embodiment of the present invention, provides a method for preparing a solder paste with a low void rate, which is specifically as follows:

[0074] S101: The accuracy of the metal powder composition was ensured by accurately weighing the elements in the Sn96.5Ag3.0Cu0.5 alloy. A high-precision electronic scale was used to weigh 96.5% tin, 3% silver, and 0.5% copper. The error was controlled within ±0.1g. This step ensured that the composition ratio of the metal powder met the requirements. Then, all the metal powders were placed in a ball mill in an argon atmosphere, and the ball milling speed was set to 400 rpm. The ball milling was continued for 24 hours to ensure that the metal particles were fully refined and evenly mixed. , using chemical plating method, immerse the metal powder in a solution containing silane coupling agent, control the temperature at room temperature 25℃, let it stand for 30 minutes, then take out the powder from the solution, put it in an oven at 60℃ and dry it for 4 hours to solidify the surface treatment layer. Assuming that 1 kg of metal powder needs to be prepared, 965 grams of tin powder, 30 grams of silver powder and 5 grams of copper powder need to be weighed, and then the above steps are followed. Through the above steps, the surface activity of the metal powder can be effectively improved and the formation of voids in the subsequent welding process can be reduced;

[0075] S102: The performance of the solder paste is ensured by accurately configuring the flux components and additives. First, according to 2.5% PEG, 0.5% environmentally friendly rosin and 0.1% antioxidant, if the total mass is 1kg, 25g PEG, 5g rosin and 1g antioxidant are weighed respectively. After uniform configuration, heat to 60°C and continue stirring until completely dissolved. Then, add 10g nano silver particles and 1g carbon nanotubes, and use a high-speed disperser to disperse at a speed of 5000 rpm for 30 minutes to ensure that the additives are fully dispersed in the flux without aggregation. For 1 kg of flux components, it is necessary to accurately weigh various ingredients according to the above ratio and ensure that they can be evenly mixed. Through the above steps, the thermal conductivity and mechanical strength of the solder paste can be effectively improved, while reducing the void rate;

[0076] S103: The uniformity and stability of the solder paste are ensured by mixing the pretreated metal powder with the flux. The pretreated metal powder is slowly added to the flux mixture at 40°C and mixed at 200 rpm for 60 minutes using a blender to ensure thorough fusion. For 1 kg of metal powder, it is necessary to evenly disperse it into the prepared flux and ensure uniform mixing. Through the above steps, the separation between the metal powder and the flux can be effectively avoided, thereby reducing the formation of voids during the welding process.

[0077] S104: The applicability of the solder paste is ensured by degassing and adjusting the viscosity. The mixture is placed in a vacuum degassing machine, and the pressure is set to -0.1MPa for 30 minutes. The degassing effect is observed and recorded to ensure that no significant bubbles are generated. If necessary, the viscosity is adjusted according to the rheometer results. The viscosity of the final product is controlled by appropriately increasing or decreasing the amount of PEG. If many bubbles are found during the degassing process, it can be improved by extending the degassing time or increasing the vacuum degree. Through the above steps, bubbles in the solder paste can be effectively reduced, the void rate during the welding process can be reduced, and the solder paste can be ensured to have a suitable viscosity for easy printing and welding;

[0078] S105: The quality of solder paste is ensured through packaging and testing. In a dust-free environment, the solder paste is divided into small containers and sealed to avoid air contact and contamination. The printing performance test is carried out according to the welding standard. The completed solder joints are subjected to X-ray inspection and microstructure analysis to ensure that the solder joints have low voiding rate and good mechanical properties. The completed solder paste needs to be divided in a dust-free workshop, and each batch needs to be strictly tested to ensure that its performance meets the standards. Through the above steps, the quality of the solder paste can be effectively guaranteed, the voiding rate during the welding process can be reduced, and the mechanical strength and electrical properties of the solder joints can be improved;

[0079] S106: The performance of the solder paste is ensured by precisely controlling the particle size range of the metal powder. The average particle size of the metal powder is calculated based on the speed and time setting of the ball mill. The speed and time of the ball mill are adjusted so that the calculated average particle size is greater than or equal to 20 μm and less than or equal to 38 μm. The particle size distribution is verified by screening to ensure that more than 90% of the metal powder particle size is within the range of 20-38 μm. If the particle size distribution does not meet the requirements, the speed and time of the ball mill are adjusted according to the screening results. If the initially calculated average particle size is less than 20 μm, the speed of the ball mill needs to be increased. If the average particle size is greater than 38 μm, it is necessary to prepare various raw materials according to the formula and proportion described in claim 1 during actual operation when the device is used. The invention comprises metal powder, flux components and additives. The composition of the metal powder strictly follows the ratio of Sn96.5Ag3.0Cu0.5, and is pretreated by a ball mill to ensure that the metal powder particle size range is between 20-38μm. This particle size range is crucial for reducing the void rate of solder joints. During the pretreatment process, the metal powder is also subjected to chemical plating treatment to enhance its surface activity. Next, according to the steps of claims 2-8, the flux components and additives are configured, and then mixed with the pretreated metal powder, and mixed at a specific temperature and stirring speed to ensure that the various components can be evenly dispersed. After the mixing is completed, a degassing treatment is required to remove bubbles in the mixture, and the viscosity of the solder paste is adjusted as needed to make it suitable for subsequent printing processes.

[0080] The material ratio experimental data table is as follows:

[0081]

[0082]

[0083] Example 2

[0084] See also Figure 2-3 , which is the second embodiment of the present invention, and this embodiment provides an application of a solder paste with a low void rate in electronic component packaging, as follows:

[0085] S101: First, an ideal soldering environment is created by ensuring that the PCB surface and the bottom of the BGA component to be soldered are clean and dust-free. To achieve this, compressed air blowing, ultrasonic cleaning or chemical solvent cleaning are used to remove surface dirt and oxides. In addition, it is also crucial to select a suitable solder paste printing template. The design of the template must accurately match the solder joint size and arrangement of the BGA component to ensure that the solder paste can be accurately placed in the required position. When designing the template, consider using laser cutting or electroforming technology to manufacture the template. Both methods can provide high-precision openings to ensure the correct distribution of solder paste. In addition, the template needs to be regularly maintained and cleaned to prevent uneven distribution of solder paste due to template clogging;

[0086] S102: By using a printer or manual scraper to evenly distribute the precisely configured low voiding solder paste to the predetermined solder joint position on the PCB, we ensure the precise placement of the solder paste. During the printing process, the printing pressure, speed and angle need to be precisely controlled to ensure that the solder paste transfer through the hole of the stencil is accurate. The printer is usually equipped with a visual system to monitor the printing process to ensure that the thickness and shape of the solder paste meet the requirements. In addition, the scraper hardness regulator can be used to adjust the hardness of the scraper to adapt to solder pastes of different viscosities. For manual printing, the operator needs to be specially trained to ensure the consistency and accuracy of each print. Through these measures, the void formation of solder paste during the printing process can be effectively reduced, thereby improving the quality and reliability of welding;

[0087] S103: By using precision placement equipment, pick and place machines, we can accurately place BGA components on the corresponding positions of the PCB printed with tin solder paste. We ensure the precise alignment between the BGA components and the PCB. Pick and place machines usually have high-precision positioning systems that can place BGA components within a tolerance range of millimeters or even smaller. Some advanced pick and place machines are equipped with optical alignment systems that can automatically correct the position deviation of BGA components before placement to ensure that each solder joint can accurately correspond to the solder ball on the BGA component. In addition, the pick and place machine also has an automatic correction function that can compensate for the expansion and deformation of the PCB during heating, further improving the accuracy of placement;

[0088] S104: By sending the PCB with BGA components into the reflow oven and setting a reasonable temperature curve according to the specific composition and performance of the solder paste, high-quality soldering results are achieved. The reflow soldering process is divided into three main stages: preheating stage, liquid soldering stage and cooling stage. In the preheating stage, the temperature is gradually increased to drive out the solvent in the solder paste. This process requires a gentle heating rate to avoid rapid evaporation of the solvent, which causes the solder paste to burst and form voids. The preheating rate can be set between 1-3℃ / second to ensure that the solvent is smoothly discharged from the solder paste. After entering the liquid soldering stage, the temperature reaches the soldering temperature. The melting point of the paste is used to melt the metal powder to form a good solder connection. At this stage, the temperature needs to be kept stable to ensure that the solder flows fully and forms a firm solder joint. For Sn63Pb37 solder paste, the melting point is 183°C, so the peak temperature of the reflow oven should be set between 210-230°C. Finally, there is the cooling stage. The temperature needs to be slowly reduced to avoid stress inside the solder joint. The cooling rate can be controlled at 3-5°C / second to ensure the stability of the internal structure of the solder joint. Through these precise temperature controls, the void rate in the solder joint can be effectively reduced and the mechanical strength of the solder joint can be improved.

[0089] S105: We ensure the quality of soldering by inspecting the solder joints under the BGA components with X-ray inspection equipment after reflow soldering. X-ray inspection is a non-destructive inspection method that can clearly show the situation inside the solder joints, including the presence or absence of voids and the connectivity of the solder joints. X-ray inspection equipment is used to evaluate the void rate of the solder joints. If the void rate is found to be too high, the soldering parameters or solder paste formula need to be adjusted. In addition, for BGA components with key functions, electrical performance tests can also be performed to ensure that welding does not affect component performance. The function of the BGA components is tested by applying voltage and current to ensure that all solder joints are in good electrical connection. Through these rigorous inspection procedures, the reliability and consistency of the final product can be ensured, thereby solving the problems existing in traditional solder paste, such as excessive void rate, poor thermal conductivity and mechanical strength.

[0090] Next, the specific steps of printing solder paste based on precise control of printing parameters in the application of solder paste in electronic component packaging are described:

[0091] S201: Adjusting the pressure of the printer: An application of solder paste in electronic component packaging. The present invention further defines that in step 2, the process of printing the solder paste requires precise control of the pressure P of the printer to ensure that the solder paste can be evenly and fully filled into the pad. Specifically, the pressure P needs to be adjusted to a set range [Pmin, Pmax], where Pmin and Pmax are the minimum and maximum pressure values, respectively. For a specific printing process, if Pmin is determined to be 0.5 kg / cm 2 And Pmax is 1.5kg / cm 2 , then in the actual operation process, it should be ensured that the pressure of the printer is always within this range to avoid the problem of insufficient solder paste filling due to too low pressure or solder paste overflow due to too high pressure;

[0092] S202: Control printing speed: In order to further improve the printing quality, it is also necessary to control the printing speed V to be within the range of Vopt±ΔV, where Vopt is the optimal printing speed and ΔV is the allowable speed fluctuation range. If Vopt is set to 10mm / s and the maximum allowable deviation ΔV is ±2mm / s, then in the actual printing process, the printing speed should be maintained between 8mm / s and 12mm / s, which can ensure that the solder paste will not be unevenly distributed due to too fast a speed, nor will it be unable to be printed before the solder paste solidifies due to too slow a speed;

[0093] S203: Determine the printing angle: In addition, the printing angle θ must also meet the requirements of θopt±Δθ, where θopt is the optimal printing angle and Δθ is the allowable angle deviation. If θopt is set to 45° and the maximum allowable deviation Δθ is ±5°, then in the actual printing process, the printing angle should be maintained between 40° and 50° to ensure that the solder paste can be correctly transferred to the pad during printing, avoiding uneven distribution or loss of solder paste due to improper angles;

[0094] S204: Ensure solder paste transfer rate: Finally, it is also necessary to ensure that the solder paste transfer rate T meets the conditions in the [Tmin, Tmax] range, where Tmin and Tmax are the minimum and maximum values ​​of the solder paste transfer rate, respectively. If Tmin is set to 80% and Tmax is set to 95%, then during the actual printing process, the solder paste transfer rate should be maintained between 80% and 95%, which helps ensure that the solder paste can be effectively transferred from the template to the pad while avoiding the problem of too much or too little solder paste.

[0095] Next, the specific steps for BGA component placement accuracy control in the application of solder paste in electronic component packaging are described:

[0096] S301: Setting the positioning accuracy of the placement device: By adjusting the mechanical system or software parameters of the placement device, the positioning accuracy E is set to the optimal value Eopt, and a certain error range ΔE is allowed. This step ensures that the placement device can be aligned to the predetermined position with high accuracy and reduces the position deviation caused by mechanical vibration or other factors;

[0097] S302: Confirm the relative position deviation between the BGA component and the PCB: Measure the relative position deviation Δd between the BGA component and the printed circuit board PCB through a visual inspection system or other sensors, and ensure that the deviation is less than the preset maximum allowable deviation Δd max , which helps to avoid poor welding problems caused by excessive position deviation;

[0098] S303: Adjust the vertical descending speed of the placement head: According to factors such as the weight and size of the BGA component and the surface characteristics of the PCB, adjust the vertical descending speed S of the placement head to the optimal value Sopt, and allow a certain range of fluctuation ΔS, so as to ensure that the BGA component is placed on the PCB stably and reduce the impact of the impact force on the component;

[0099] S304: monitoring the horizontal offset of the BGA component: during the placement process, continuously monitor the horizontal offsets Δx and Δy of the BGA component relative to the predetermined position to ensure that the sum of the squares of the offsets in these two directions is less than the square of the maximum allowable deviation Δd_max. If it is found that the offset exceeds the allowable range, the placement strategy needs to be adjusted in time to ensure that the BGA component is accurately placed at the designated position.

[0100] These steps together constitute a strict control over the BGA component placement accuracy, thereby improving the reliability and efficiency of the electronic component packaging process.

[0101] Next, the specific steps of optimizing the temperature curve for reflow soldering in the application of solder paste in electronic component packaging are described:

[0102] S401: Ensure uniform heating of the solder paste by precisely controlling the temperature rise rate in the preheating stage. Specifically, in the preheating stage, the temperature rise rate R1 of T1 is strictly controlled near an optimal value R1 opt, and the allowable deviation range is ±ΔR1, which can avoid solder paste oxidation or component damage caused by local overheating and ensure uniform temperature distribution in the entire welding area;

[0103] S402: Ensure that the solder paste can be fully melted and form a good solder joint by precisely controlling the temperature in the liquid soldering stage. In this stage, the temperature T2 needs to reach the melting point of the solder paste Tmelt±ΔTmelt, which is crucial for forming a stable and reliable solder joint, because if the temperature is too low, the solder paste may not be completely melted, and if the temperature is too high, it may cause excessive diffusion of the solder or the formation of a poor intermetallic compound layer;

[0104] S403: Ensure the quality of solder joints by controlling the temperature drop rate in the cooling stage. In the cooling stage, the drop rate R3 of temperature T3 is controlled within the range of R3opt±ΔR3. Rapid cooling helps to form a fine grain structure, thereby improving the mechanical strength and reliability of the solder joint, while slow cooling helps to reduce the stress inside the solder joint and prevent cracks.

[0105] S404: During the entire reflow soldering process, the actual temperature curve Tt is monitored in real time and compared with the preset target temperature curve T t arget(t) to ensure that the deviation ΔTt between the two is always less than the maximum allowable deviation ΔTmax. The monitoring mechanism can be realized by installing a temperature sensor in the reflow oven. Once it is detected that the deviation exceeds the allowable range, the system will automatically adjust the heating power or other parameters to correct the temperature curve, thereby ensuring the quality control of the welding process.

[0106] Next, the specific steps for solder joint void rate detection and quality control in the application of solder paste in electronic component packaging are described:

[0107] S501: Obtaining solder joint images I through X-ray inspection equipment. This process involves placing the packaged electronic components under the X-ray inspection equipment and using the ability of X-rays to penetrate materials to capture images of the internal structure of the solder joints. The X-ray inspection equipment is usually equipped with a high-resolution imaging system that can clearly display the details inside the solder joints, including possible void areas.

[0108] S502: Calculate the void ratio H of the solder joint by applying an image processing algorithm. After obtaining the X-ray image of the solder joint, the image needs to be analyzed to determine the proportion of voids inside the solder joint. This step includes image preprocessing such as denoising, contrast enhancement, etc., void area identification, and calculation of the proportion of the void area to the entire solder joint area. Modern image processing software or custom-developed algorithms can automatically complete these tasks, thereby quickly and accurately obtaining the void ratio H of the solder joint.

[0109] S503: Determine whether the solder joint void ratio H satisfies H≤H ma, where Hmax is the maximum allowable void rate. A maximum allowable void rate threshold Hmax is set according to industry standards or specific application requirements, and then the calculated actual void rate H is compared with Hmax. If H is greater than Hmax, it indicates that the solder joint has quality problems. Otherwise, the solder joint is considered qualified.

[0110] S504: If H>H max , then mark the solder joint as a failed solder joint and record the position information P fail Once the void rate of a solder joint exceeds the maximum allowable value, the solder joint needs to be marked for subsequent processing. At the same time, the location information P of the unqualified solder joint is recorded. fail This is crucial for tracking problem solder joints, analyzing causes and improving process flows. The data can be stored in a database for quality control and statistical analysis.

[0111] Next, the specific steps of the electrical performance test of BGA components in the application of solder paste in electronic component packaging are described:

[0112] S601: Start the electrical performance test process by applying a standard test signal S to the BGA Ball Grid Array component. This standard test signal S is usually an electrical signal with known characteristics, such as a sine wave or pulse signal of a specific frequency and amplitude, which is used to simulate the input signal under actual working conditions;

[0113] S602: Proceed to the next step by measuring the output response signal R of the BGA component, using precision measuring equipment, such as an oscilloscope or a network analyzer, to ensure that the details of the output signal can be accurately captured;

[0114] S603: Calculate the signal distortion D, that is, the difference between the input signal S and the output signal R, which can be done by comparing the waveform, phase, amplitude and other parameters of the two. If the signal distortion D exceeds the preset maximum allowable distortion Dmax, it is considered that the BGA component has quality problems;

[0115] S604: If the signal distortion D is greater than the maximum allowable distortion Dmax, the BGA component is determined to be unqualified, and the specific fault type Ffail is recorded;

[0116] In actual operation, a signal generator can be used to generate a standard test signal S and apply it to a pin of the BGA component. Then an oscilloscope can be used to monitor the signal changes on the pin and the corresponding output pin at the same time to obtain the output response signal R. By comparing the waveforms of the input signal S and the output signal R, the signal distortion D can be calculated. If the distortion is found to exceed the preset threshold Dmax, it is necessary to further check whether the BGA component has problems such as poor welding, and record the specific fault type for subsequent analysis and improvement.

[0117] Next, the specific steps of applying solder paste in electronic component packaging are described:

[0118] S701: Use appropriate inspection tools or equipment to measure the roughness of the PCB surface and the flatness of the bottom of the BGA component to obtain initial evaluation data, which will be used to determine the most appropriate cleaning method. A surface profiler can be used to measure the roughness of the PCB surface, and a microscope can be used to check the flatness of the bottom of the BGA component.

[0119] S702: Compare the obtained data with the preset first threshold and second threshold to determine which cleaning method to use. If the surface roughness of the PCB is less than the first threshold and the flatness of the bottom of the BGA component is greater than the second threshold, it indicates that the surface is relatively clean. In this case, a gentle cleaning method can be used, such as gently wiping with a soft brush or blowing with compressed air. On the contrary, if the surface roughness of the PCB is greater than or equal to the first threshold or the flatness of the bottom of the BGA component is less than or equal to the second threshold, it indicates that a more thorough cleaning process is required. In this case, a strong cleaning method should be used, such as solvent cleaning or ultrasonic cleaning.

[0120] S703: After the cleaning process is completed, the same inspection tool or equipment is used again to measure the surface roughness of the PCB and the flatness of the bottom of the BGA component to verify whether the cleaning effect meets the expected standard. If the data after cleaning meets the set standard, the next step of welding can be continued. If not, it is necessary to clean again until it meets the requirements. This process ensures that the surface conditions before welding can support high-quality welding operations.

[0121] Next, we will describe the application of solder paste in electronic component packaging, especially the specific steps of selecting a suitable solder paste printing template:

[0122] S801: First, the template is designed according to the solder joint size and arrangement of the BGABall Grid Array component, which involves detailed measurement of the solder joints on the BGA component to determine the diameter of the solder joints. The solder joint diameter is one of the key factors in determining the template aperture size, so it needs to be accurately measured;

[0123] S802: Next, calculate the distance between solder joints. The solder joint spacing refers to the distance between the centers of two adjacent solder joints. This parameter is crucial for determining the template aperture because it directly affects whether the solder paste can be accurately placed at the predetermined position without overflow or insufficient solder paste.

[0124] S803: Then, the size of the template aperture is determined based on the proportional relationship between the solder spot spacing and the solder spot diameter. Specifically, if the ratio of the solder spot spacing to the solder spot diameter is less than the preset third threshold, the template aperture size is set to the solder spot diameter minus the fourth threshold. Conversely, if the ratio of the solder spot spacing to the solder spot diameter is greater than or equal to the third threshold, the template aperture size is set to the solder spot diameter minus the fifth threshold. Here, the third, fourth and fifth thresholds are all pre-set values ​​based on actual experience, which are used to ensure that the solder paste can be correctly and evenly distributed to each solder spot.

[0125] The following are examples to illustrate the technical implementation of the above steps:

[0126] S801: Assume that we have a BGA component with a solder joint diameter of 0.5 mm. In order to obtain accurate measurement results, we can use a high-precision microscope or a special measuring tool to measure and record the diameter of each solder joint;

[0127] S802: Continuing with the above example, assuming that the measured solder joint spacing is 0.8 mm, in order to calculate the solder joint spacing, the same measuring tool can be used to measure the distance between the centers of two adjacent solder joints;

[0128] S803: Assume that the third threshold is set to 1.6, which is the ratio of the solder joint spacing to the solder joint diameter, the fourth threshold is 0.1 mm, and the fifth threshold is 0.05 mm. According to calculation, the ratio of the solder joint spacing to the solder joint diameter is 1.60.8 / 0.5=1.6, which is exactly equal to the third threshold. Therefore, the template aperture size should be set to the solder joint diameter minus the fifth threshold, that is, 0.45 mm 0.5-0.05=0.45. The template aperture designed in this way can ensure that the solder paste is neither too much nor too little during the printing process, thereby improving the welding quality and reliability.

[0129] Next, the specific steps of applying solder paste in electronic component packaging are described:

[0130] S901: Through the use of a precisely configured low voiding rate solder paste, in one embodiment of the present invention, a solder paste is used in electronic component packaging, and the step of printing the solder paste includes using a printer or a manual scraper to evenly distribute the precisely configured low voiding rate solder paste to predetermined solder joint positions on a PCB printed circuit board. The process needs to be precisely controlled to ensure that the solder paste can accurately fill the pores of the template and form a uniform solder paste layer on the PCB surface. In order to achieve this purpose, key parameters in the printing process need to be adjusted, including printing pressure, speed and angle;

[0131] S902: Ensure the accuracy of solder paste transfer by adjusting the printing pressure, speed and angle. During the printing process, the printing pressure needs to be adjusted first. If the printing pressure is detected to be less than the preset sixth threshold, the printing pressure needs to be increased to ensure that the solder paste can fully fill the template pores and transfer to the PCB. Next, the printing speed needs to be adjusted. If the printing speed is greater than the preset seventh threshold, the printing speed needs to be reduced to avoid uneven distribution caused by excessive flow of solder paste. Finally, the printing angle needs to be adjusted. If the printing angle deviation is greater than the preset eighth threshold, the printing angle needs to be corrected to ensure that the solder paste can be accurately transferred to the predetermined position. These adjustments can be completed automatically by the control system of the printer, or they can be adjusted manually by the operator.

[0132] S903: Check the solder paste transfer again to confirm that the solder paste is evenly distributed. After completing the above parameter adjustment, check the solder paste transfer again to confirm whether the solder paste is evenly distributed on the predetermined solder joint positions of the PCB. This step can be completed through visual inspection or using automated inspection equipment. If the solder paste is found to be unevenly distributed, it may be necessary to further adjust the printing parameters until the requirements are met. Once it is confirmed that the solder paste is evenly distributed, the subsequent packaging process steps can be continued.

[0133] Next, the specific steps for placing BGA components in the application of solder paste in electronic component packaging are described:

[0134] S1001: The ball grid array (BGA) component is accurately placed on the specified position of the printed circuit board (PCB) where the solder paste has been printed by a precision placement device usually called a pick-and-place machine. Highly precise operations are required to ensure the alignment accuracy between the BGA component and the PCB. During the placement process, a visual inspection system is used to measure the relative position deviation between the BGA component and the PCB.

[0135] S1002: If the alignment error data obtained through measurement is found to exceed the ninth threshold value set in advance, that is, the alignment accuracy is insufficient, the position of the BGA component needs to be adjusted using the fine-tuning function of the pick-and-place machine until the error is reduced to an acceptable range. This adjustment process requires multiple iterations, and the alignment error needs to be re-measured after each adjustment until the error meets the requirements;

[0136] S1003: Once the alignment error between the BGA component and the PCB is adjusted to be less than or equal to the ninth threshold value, the required alignment accuracy is achieved. At this time, the BGA component can be kept in the current position. After the position adjustment is completed, the alignment error is measured again to finally confirm the accuracy of the placement, ensuring that the BGA component can be correctly aligned with the solder joints on the PCB, thereby ensuring the quality and reliability of the subsequent soldering process.

[0137] Next, the specific steps of the preheating stage in the reflow soldering step of a solder paste in the application of electronic component packaging are described:

[0138] S1101: Monitor the temperature change during the preheating process by measuring the temperature rise rate. This process can be achieved by installing temperature sensors in the reflow oven. These sensors can monitor and record the temperature change during the preheating stage in real time. The data of the temperature sensors are transmitted to the control system, and the control system calculates the actual temperature rise rate according to the set program;

[0139] S1102: Calculate the solvent volatilization rate by analyzing the solder paste composition and environmental conditions. It is necessary to determine the solvent volatilization rate of different types of solder pastes at specific temperatures through experiments in advance and store these data in a database. When actual soldering is performed, the control system will call the corresponding data and calculate the actual solvent volatilization rate in combination with the current temperature conditions.

[0140] S1103: Compare the proportional relationship between the temperature rise rate and the solvent volatilization rate. The control system compares the calculated temperature rise rate with the solvent volatilization rate. If it is found that the ratio of the temperature rise rate to the solvent volatilization rate is less than the tenth threshold, that is, a preset safety ratio, it is considered that the solvent volatilization may be insufficient. At this time, the control system will automatically extend the preheating time to ensure that the solvent can be completely volatilized. On the contrary, if the ratio of the temperature rise rate to the solvent volatilization rate is greater than or equal to the tenth threshold, it is considered that the solvent volatilization is sufficient. The control system will appropriately shorten the preheating time to improve production efficiency.

[0141] Through the above steps, the time of the preheating stage can be effectively controlled to ensure that the solvent in the solder paste can be fully volatilized, thereby improving the soldering quality and production efficiency.

[0142] In actual operation, when this device is used, the application of a solder paste in the packaging of electronic components first starts with preparation, that is, ensuring that the surface of the circuit board PCB to be soldered and the bottom of the BGA component are clean and dust-free, and selecting a suitable solder paste printing template. The design of the template needs to be carried out according to the size and arrangement of the solder joints of the BGA component to ensure that the solder paste can accurately cover the predetermined solder joint positions during the subsequent printing process. Subsequently, a printer or a manual scraper is used to evenly distribute the solder paste with a low void rate on the PCB. This process requires precise control of the printing pressure, speed and angle to ensure that the solder paste can be accurately transferred to the solder joints of the PCB. Next, a precision placement device such as a pick-and-place machine is used to accurately place the BGA component on the corresponding position of the PCB printed with the solder paste. This step is crucial to ensure the precise alignment between the BGA component and the PCB. After that, the PCB with the BGA component is placed on the It is sent into the reflow oven for welding. The reflow soldering process is divided into three main stages: preheating stage, liquid soldering stage and cooling stage. The preheating stage is to remove the solvent in the solder paste. The liquid soldering stage is to reach the melting point of the tin solder paste, so that the metal powder melts to form a good welding connection. Finally, in the cooling stage, the solder joint will slowly cool down to avoid internal stress. After completing the reflow soldering, inspection and quality control are required. This step uses X-ray inspection equipment to check the solder joints under the BGA components to verify whether the internal void rate of the solder joints is low and the connection is good. For some BGA components with key functions, additional electrical performance tests will be performed to ensure that the welding process does not affect the overall performance of the components. The whole process reflects the highly coordinated workflow between the components from the selection of solder paste to printing, placement, welding and final quality control, ensuring the high quality and reliability of electronic component packaging.

[0143]

[0144]

[0145]

[0146] Conclusion: The uniform refinement and good surface treatment of the metal powder (Sn96.5Ag3.0Cu0.5 alloy) were ensured through the process of precise weighing, ball milling and chemical plating. The ball milling process effectively reduced the size of the metal particles and achieved the specified particle size distribution (20-38μm), which is crucial to improving the reliability and solder joint quality during the welding process.

[0147] The correct proportion and uniform dispersion of flux and additives, especially nanosilver particles and carbon nanotubes, play a significant role in improving soldering strength and reducing voiding. Stirring at 60°C ensures complete dissolution of PEG, rosin and antioxidant, while the high-speed disperser ensures uniform distribution without aggregation.

[0148] At 40°C, slowly add the metal powder to the flux mixture and use appropriate stirring speed and time to ensure thorough fusion of the mixture, which is particularly important for ensuring the integrity and performance stability of the final product.

[0149] The above is a preferred embodiment of the present application. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present application.

Claims

1. A solder paste with low void rate, Features: Its materials include metal powder, flux components and additives; Metal powder: tin 96.5%, silver 3.0%, copper 0.5%; Particle size range: 20-38μm; Flux components: 2.5% polyethylene glycol (PEG) as a binder, 0.5% environmentally friendly rosin as an activator, and 0.1% high-efficiency antioxidant (including silane coupling agent); Additives: 1.0% of nano silver particles (for improving welding strength and reducing void ratio) and 0.1% of trace carbon nanotubes (for improving thermal conductivity and mechanical strength).

2. A method for preparing a solder paste with low void ratio, comprising the solder paste with low void ratio as claimed in claim 1, Features: include, S1. Metal powder pretreatment; S2, flux and additive configuration; S3, mixing metal powder and flux; S4, degassing and viscosity adjustment; S5. Packaging.

3. A method for preparing a solder paste with low void ratio according to claim 2, Features: In the step S1, weigh Sn96.5Ag3.0Cu0.5 alloy: tin (96.5%), silver (3%), copper (0.5%), use a high-precision electronic scale to weigh each element, and control the error within ±0.1g. Put all the metal powders into a ball mill in an argon atmosphere, set the ball milling speed to 400 rpm, and continue ball milling for 24 hours to ensure that the metal particles are fully refined and evenly mixed; Using the chemical plating method, the metal powder is immersed in a solution containing a silane coupling agent, the temperature is controlled at room temperature (25°C), and the reaction is allowed to stand for 30 minutes. The powder is then taken out of the solution and placed in an oven at 60°C for 4 hours to cure the surface treatment layer.

4. A method for preparing a solder paste with low void ratio according to claim 2, Features: In step S2, according to 2.5% PEG, 0.5% environmentally friendly rosin and 0.1% antioxidant, if the total mass is 1kg, 25g PEG, 5g rosin and 1g antioxidant are weighed respectively, and after uniform distribution, they are heated to 60°C and stirred continuously until completely dissolved; 10 g of nanosilver particles and 1 g of carbon nanotubes were added and dispersed at a speed of 5000 rpm for 30 minutes using a high-speed disperser to ensure that the additives were fully dispersed in the flux without aggregation.

5. The method for preparing a solder paste with low void ratio according to claim 2, Features: In step S3, the pretreated metal powder is slowly added to the flux mixture at 40° C. and mixed at 200 rpm for 60 minutes using a mixer to ensure thorough fusion; In step S4, the mixture is placed in a vacuum degassing machine, the pressure is set to -0.1 MPa, and the degassing effect is observed and recorded to ensure that no significant bubbles are generated. If necessary, the viscosity is adjusted according to the rheometer results, and the viscosity of the final product is controlled by appropriately increasing or decreasing the amount of PEG.

6. The method for preparing a solder paste with low void ratio according to claim 2, Features: In step S5, the solder paste is divided into small containers in a dust-free environment and sealed to avoid air contact and contamination. The printing performance test is carried out according to the welding standard, and the completed solder joints are subjected to X-ray inspection and microstructure analysis to ensure that the solder joints have low void rate and good mechanical properties.

7. The method for preparing a solder paste with low void ratio according to claim 2, Features: The particle size range of the metal powder is obtained by the following steps: S11. Calculate the average particle size of the metal powder based on the speed and time setting of the ball mill, where the average particle size (D) is calculated by the formula D = 20 + 18 × (speed / 400) 0.5 ×(time / 24) 1 Sure; S12, adjusting the rotation speed and time of the ball mill so that the calculated average particle size (D) is greater than or equal to 20 μm and less than or equal to 38 μm; S13, verify the particle size distribution by sieving method to ensure that more than 90% of the metal powder particle size is within the range of 2038μm; S14: If the particle size distribution does not meet the requirements, return to step S11 to readjust the speed and time of the ball mill.

8. The method for preparing a solder paste with low void ratio according to claim 7, Features: In the step S11, when the calculated average particle size (D) is less than 20 μm, the rotation speed of the ball mill is increased; When the calculated average particle size (D) is greater than 38 μm, reduce the speed of the ball mill; In the step S12, if the adjusted average particle size (D) is still not within the range of 2038 μm, the ball milling time is further adjusted, wherein the ball milling time (T) is determined by the formula T=24×(38D) / D20); In step S13, if the particle size distribution does not meet the requirements after verification by the screening method, the speed and time of the ball mill are adjusted according to the screening results, wherein the speed (R) is calculated by the formula R = 400 × 38D max ) / (D min 20) Determine, where D max and D min are the maximum and minimum particle sizes, respectively; In step S14, if the particle size distribution requirement cannot be met after multiple adjustments, it is necessary to check the working state of the ball mill or replace the metal raw material to ensure that the particle size range of the final metal powder meets the standard of 2038 μm.

9. Use of a solder paste in electronic component packaging, comprising the solder paste with low void ratio according to claim 1, Features: The solder paste is applied to Ball Grid Array (BGA) packaging technology.

10. Application of the solder paste according to claim 9 in electronic component packaging, Features: include, (1) Preparation: Ensure that the surface of the circuit board (PCB) to be soldered and the bottom of the BGA component are clean and dust-free, and select a suitable solder paste printing template. The template design should be based on the size and arrangement of the solder joints of the BGA component; (2) Printing solder paste: Use a printer or a manual scraper to evenly distribute the precisely configured low voiding solder paste to the predetermined solder joint locations on the PCB. By precisely controlling the printing pressure, speed, and angle, ensure that the solder paste transfer through the holes of the template is accurate. (3) Placing BGA components: Use precision placement equipment (pick-and-place machine) to accurately place BGA components on the corresponding position of the PCB printed with solder paste; (4) Reflow soldering: Send the PCB with BGA components into the reflow soldering furnace and set a reasonable temperature curve according to the specific composition and performance of the solder paste; (41) Preheating stage: The temperature is gradually increased to drive out the solvent in the solder paste; (42) Liquid welding stage: reaching the melting point of the solder paste, melting the metal powder to form a good welding connection; (43) Cooling stage: Slowly cool down to avoid solder joint stress; (5) Inspection and quality control: After reflow soldering, the solder joints under the BGA components are inspected using X-ray inspection equipment to verify whether the internal void rate of the solder joints is low and the connectivity is good. For BGA components with key functions, electrical performance tests can also be performed to ensure that soldering does not affect component performance.

Citation Information

Patent Citations

  • Lead-free and cleaning-free solder paste capable of realizing few-cavity welding layers and preparation method of lead-free cleaning-free solder paste

    CN102528315A

  • Reflow welding process of DIP through-hole part

    CN104308314A

  • Soldering paste for improving welding cavity of large-area bonding pad of electronic device

    CN115971719A

  • Low-cavity halogen-free solder paste and preparation method thereof

    CN117548901A

  • Active metal brazing paste and preparation method thereof

    CN117798543A