Phosphorus-silicon-indium-cadmium compound, phosphorus-silicon-indium-cadmium nonlinear optical crystal and preparation method and application thereof
By developing the phosphosilicon indium cadmium compound Cd2In3Si2P7, the crystal structure is optimized using multiple preparation methods, and the problem of insufficient damage threshold of existing long-wave infrared nonlinear optical crystals is solved, and efficient nonlinear optical and mechanical properties are achieved, suitable for multiple Infrared laser application.
Patent Information
- Application Number
- CN202410930052.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-05
AI Technical Summary
When the existing long-wave infrared nonlinear optical crystal materials face the demand for ultra-short pulse, high refrigeration and high power mid-infrared laser output, the laser damage threshold is insufficient, making it difficult to meet the rapidly developing solid-state laser technology needs.
Develop a phosphorus silicon indium cadmium compound Cd2In3Si2P7, and prepare phosphorus silicon indium cadmium nonlinear optical crystals by mixing Cd, In, Si, P source materials in a specific molar ratio and calcining at high temperature. Various preparation methods are adopted, such as high-temperature solid phase method , flux method, chemical gas phase transport method, physical gas phase transport method and crucible drop method to optimize crystal structure and performance.
It realizes a phosphosilicon indium cadmium nonlinear optical crystal with high laser damage threshold, large nonlinear optical effect, wide infrared transmission band and excellent mechanical properties. It is suitable for nonlinear optical devices such as infrared laser frequency conversion devices, infrared electro-optical devices and infrared communications. Device.
Smart Images

Figure CN118894531A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional crystal materials, and in particular relates to a phosphosilicate indium cadmium compound, a phosphosilicate indium cadmium nonlinear optical crystal, and a preparation method and application thereof. Background Art
[0002] Mid-infrared lasers (2.5-25μm), especially long-wave infrared tunable lasers at 8-14μm, have very important applications in military and civilian fields, such as laser guidance, optoelectronic countermeasures, infrared remote sensing, medical diagnosis, environmental monitoring, etc. At present, the practical nonlinear optical crystal materials used to obtain long-wave infrared lasers using nonlinear optical methods are mainly AgGaS2, AgGaSe2, ZnGeP2, CdSe, etc. However, with the rapid development of solid-state laser technology and the increasing demand for ultra-short pulse high repetition rate and high power mid-infrared laser output, it is urgent to develop new long-wave infrared nonlinear optical crystals with better comprehensive performance, especially high laser damage threshold. Phosphomonium compounds have large nonlinear optical coefficients, high thermal conductivity and wide light transmittance range, and are ideal candidate material systems. Summary of the invention
[0003] The first object of the present invention is to provide a phosphorus silicon indium cadmium compound, whose chemical formula is Cd2In3Si2P7.
[0004] The second object of the present invention is to provide a phospho-silicon-indium-cadmium nonlinear optical crystal, whose chemical formula is Cd2In3Si2P7.
[0005] The third object of the present invention is to provide a method for preparing the phosphorus silicon indium cadmium nonlinear optical crystal.
[0006] The fourth object of the present invention is to provide a use of the phosphorus silicon indium cadmium nonlinear optical crystal material.
[0007] The technical solution of the present invention is as follows:
[0008] A phosphine-silicon-indium-cadmium compound with the chemical formula Cd2In3Si2P7.
[0009] According to an embodiment of the present invention, the preparation method of the phosphorus silicon indium cadmium compound comprises: mixing a Cd source material, an In source material, a Si source material and a P source material, grinding them, and calcining them at a high temperature to obtain the phosphorus silicon indium cadmium compound.
[0010] The present invention also provides a method for preparing the phosphorus silicon indium cadmium compound, which comprises: mixing a Cd source material, an In source material, a Si source material and a P source material, grinding them, and calcining them at high temperature to obtain the phosphorus silicon indium cadmium compound.
[0011] According to an embodiment of the present invention, in the Cd source material, the In source material, the Si source material and the P source material, the molar ratio of the elements Cd, In, Si and P is 2:3-4:2:7-8, for example, 2:3:2:7.
[0012] According to an embodiment of the present invention, the Cd source material is selected from Cd element or Cd3P2.
[0013] According to an embodiment of the present invention, the In source material is selected from In single substance or InP.
[0014] According to an embodiment of the present invention, the Si source material is selected from Si single substance.
[0015] According to an embodiment of the present invention, the P source material is selected from P single substance.
[0016] According to an embodiment of the present invention, the high temperature calcination comprises: heating to 950°C-1100°C and then calcining. Preferably, the heating rate is 20°C / h-80°C / h. Preferably, the calcination time is 24 hours-120 hours.
[0017] According to an embodiment of the present invention, in the preparation method, after high-temperature calcination, the temperature is further reduced. Preferably, the temperature reduction refers to reducing the temperature to 700°C-500°C at a rate of 1°C / h-5°C / h, and then reducing the temperature to room temperature.
[0018] The invention also provides a phosphorus silicon indium cadmium nonlinear optical crystal, whose chemical formula is Cd2In3Si2P7.
[0019] According to the embodiment of the present invention, the nonlinear optical crystal Cd2In3Si2P7 belongs to the monorthic system, and its structural schematic diagram is as follows: Figure 1 As shown; the space group is P21, and the unit cell parameters are: α=γ=90°, β=103, z=2.
[0020] Preferably, the unit cell parameters of the phosphosilicon indium cadmium nonlinear optical crystal Cd2In3Si2P7 are: α=γ=90°, β=103.772, z=2.
[0021] The present invention provides a method for preparing the above-mentioned phosphorus silicon indium cadmium nonlinear optical crystal, the preparation method comprising:
[0022] The Cd source material, the In source material, the Si source material and the P source material are mixed, a transport agent and / or a co-solvent are added, the mixture is ground, and the mixture is calcined at a high temperature to obtain the phosphorus silicon indium cadmium nonlinear optical crystal.
[0023] According to an embodiment of the present invention, the molar ratio of the element Cd in the Cd source material, the element In in the In source material, the element Si in the Si source material, and the element P in the P source material is 2:3-4:2:7-8, for example, 2:3:2:7.
[0024] According to an embodiment of the present invention, the Cd source material is selected from Cd element or Cd3P2.
[0025] According to an embodiment of the present invention, the In source material is selected from In single substance or InP.
[0026] According to an embodiment of the present invention, the Si source material is selected from Si single substance.
[0027] According to an embodiment of the present invention, the P source material is selected from P single substance.
[0028] According to an embodiment of the present invention, the flux is selected from at least one of SrCl2, SrBr2, SrI2, BaCl2, BaBr2 and BaI2.
[0029] According to an embodiment of the present invention, the transport agent is selected from at least one of I2 elemental substance, NH4Cl, NH4Br, and NH4I.
[0030] According to an embodiment of the present invention, the molar ratio of the element Cd in the Cd source material, the element In in the In source material, the element Si in the Si source material, the element P in the P source material and the flux is 2:3-4:2:7-8:4-10, for example, 2:3:2:7:5.
[0031] According to an embodiment of the present invention, the concentration of the transport agent is 1 mg / cm 3 -20mg / cm 3 , for example 5 mg / cm 3 、10mg / cm 3 、15mg / cm 3 , 20mg / cm 3 .
[0032] According to an embodiment of the present invention, the method for preparing the phosphosilicate indium cadmium nonlinear optical crystal further comprises: mixing the prepared phosphosilicate indium cadmium nonlinear optical crystal with a second transport agent, grinding the crystal, and calcining the crystal at a high temperature to obtain the phosphosilicate indium cadmium nonlinear optical crystal. Preferably, the concentration of the second transport agent can be 1 mg / cm 3 -20mg / cm 3 Preferably, the second transport agent is the same as or different from the transport agent, and is independently selected from at least one of I2 elemental substance, NH4Cl, NH4Br, and NH4I.
[0033] According to the embodiment of the present invention, the mixing and grinding can be performed by methods known in the art, which are not specifically limited in the present invention.
[0034] According to an embodiment of the present invention, high temperature calcination is carried out at a vacuum degree of 10 -5 -10 -1 For example, the raw materials (such as Cd source material, In source material, Si source material, P source material, and optional transport agent and / or cosolvent) are mixed and ground and then loaded into a quartz tube, which is evacuated to 10 -5 -10 -1 Pa and then sealed and further calcined at high temperature.
[0035] According to an embodiment of the present invention, the high temperature calcination comprises: heating to 950°C-1100°C and then calcining. Preferably, the heating rate is 20°C / h-80°C / h. Preferably, the calcination time is 24 hours-120 hours.
[0036] According to an embodiment of the present invention, in the preparation method, after high-temperature calcination, the temperature is further reduced. Preferably, the temperature reduction refers to reducing the temperature to 700°C-500°C at a rate of 1°C / h-5°C / h, and then reducing the temperature to room temperature.
[0037] According to an embodiment of the present invention, in the preparation method, when a co-solvent or a transport agent is added, deionized water or anhydrous ethanol needs to be added for washing and filtering after cooling.
[0038] According to a preferred embodiment of the present invention, the preparation method of the phospho-silicon-indium-cadmium nonlinear optical crystal is a flux method, and the steps are as follows: Cd source material, In source material, Si source material, P source material and flux are mixed and ground, and the phospho-silicon-indium-cadmium nonlinear optical crystal is obtained after high-temperature calcination.
[0039] Preferably, the molar ratio of Cd in the Cd source material to the flux is 2:4-10.
[0040] Preferably, in the flux method, high temperature calcination means: heating to 950°C-1100°C at a rate of 20°C / h-80°C / h, calcining at a constant temperature for 24 hours-120 hours; and then cooling to 700°C-500°C at a rate of 1°C / h-5°C / h.
[0041] Preferably, in the flux method, after high-temperature calcination, the temperature is lowered, and then deionized water or anhydrous ethanol is added to dissolve the flux, and then filtered.
[0042] According to a preferred embodiment of the present invention, the preparation method of the phosphorus silicon indium cadmium nonlinear optical crystal is a chemical vapor transport method, and the steps are as follows:
[0043] The Cd source material, the In source material, the Si source material, the P source material and the I2 single substance are mixed and ground, and calcined at high temperature in a tubular growth furnace to obtain the phosphorus silicon indium cadmium nonlinear optical crystal.
[0044] According to an embodiment of the present invention, the concentration of the transport agent is 1 mg / cm 3 -20mg / cm 3 .
[0045] Preferably, in the chemical vapor transport method, the high temperature end or evaporation end in the tubular growth furnace is heated to 950°C-1100°C at a rate of 20°C / h-80°C / h, and the low temperature end or crystallization end in the tubular growth furnace is heated to 900°C-1000°C at a rate of 20°C / h-80°C / h, and constant temperature calcination is carried out for 24 hours to 120 hours.
[0046] Preferably, after calcination, the temperature is lowered to 700-500°C at a rate of 1°C / h-3°C / h at the high temperature end or the evaporation end, and to 600-400°C at a rate of 1°C / h-3°C / h at the low temperature end or the crystallization end, and then cooled to room temperature.
[0047] According to a preferred embodiment of the present invention, the preparation method of the phosphorus silicon indium cadmium nonlinear optical crystal is a physical vapor transport method, and the steps are as follows:
[0048] The Cd2In3Si2P7 crystal is mixed with a transport agent, ground, and calcined at high temperature to obtain the phosphorus silicon indium cadmium nonlinear optical crystal.
[0049] Preferably, in the physical vapor transport method, the high temperature end or evaporation end in the tubular growth furnace is heated to 950°C-1100°C at a rate of 20°C / h-80°C / h, and the low temperature end or crystallization end in the tubular growth furnace is heated to 900°C-1000°C at a rate of 20°C / h-80°C / h, and constant temperature calcination is carried out for 24 hours to 120 hours.
[0050] Preferably, after calcination, the temperature is lowered to 700-500°C at a rate of 1°C / h-3°C / h at the high temperature end or the evaporation end, and to 600-400°C at a rate of 1°C / h-3°C / h at the low temperature end or the crystallization end, and then cooled to room temperature.
[0051] According to a preferred embodiment of the present invention, the preparation method of the phosphorus silicon indium cadmium nonlinear optical crystal is a crucible descent method, and the specific steps are as follows: Cd source material, In source material, Si source material, P source material and flux are mixed and ground, and high-temperature calcined in a crucible descent furnace to obtain the phosphorus silicon indium cadmium nonlinear optical crystal.
[0052] Preferably, in the crucible descent method, the raw materials are placed in a crucible descent furnace, heated to 950°C-1100°C at a rate of 30-40°C / h, kept warm for 40 hours-50 hours until the raw materials are completely melted, and then vertically descended at a speed of 0.1mm / h-1mm / h for crystal growth. The growth cycle is 10-40 days.
[0053] Preferably, after the crystal growth is completed, the temperature is lowered to room temperature at a rate of 50° C.-10° C. / h to obtain a phosphorus silicon indium cadmium nonlinear optical crystal.
[0054] The present invention also provides the use of the above-mentioned phospho-silicate-indium-cadmium nonlinear optical crystal, which is preferably used in the field of nonlinear optics or in the mid-infrared band, for example, in nonlinear optical devices.
[0055] The present invention also provides a nonlinear optical device, which comprises the above-mentioned phospho-silicate-indium-cadmium nonlinear optical crystal.
[0056] According to an embodiment of the present invention, in the nonlinear optical device, at least one beam of incident electromagnetic radiation passes through at least one piece of the phospho-silicate-indium-cadmium nonlinear optical crystal to generate at least one beam of output radiation having a frequency different from the incident electromagnetic radiation.
[0057] According to an embodiment of the present invention, the nonlinear optical device includes but is not limited to at least one of an infrared laser frequency conversion device, an infrared electro-optical device, an infrared communication device, an infrared laser guidance device, and an infrared optoelectronic countermeasure system.
[0058] Beneficial Effects
[0059] The phosphosilicon indium cadmium nonlinear optical crystal Cd2In3Si2P7 of the present invention has the advantages of large nonlinear optical effect (the frequency doubling output intensity is about 2.2 times that of ZnGeP2 under the same conditions), wide infrared light transmission band (2.5-10 microns), easy growth, high hardness, good mechanical properties, not easy to break and deliquesce, easy processing and preservation, etc., and can be applied to various nonlinear optical fields or mid-infrared bands, for example, it can be used to prepare infrared laser frequency conversion devices, infrared electro-optical devices, infrared communication devices or infrared laser guidance devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 Schematic diagram of the crystal structure of phosphosilicon indium cadmium nonlinear optical crystal Cd2In3Si2P7.
[0061] Figure 2 This is a comparison chart of X-ray powder diffraction and simulated X-ray diffraction of the phospho-silicon-indium-cadmium compound obtained in Example 1 and the phospho-silicon-indium-cadmium nonlinear optical crystal Cd2In3Si2P7 obtained in Example 2.
[0062] Figure 3This is the infrared transmission spectrum of the phospho-silicon-indium-cadmium nonlinear optical crystal Cd2In3Si2P7 obtained in Example 5 after directional cutting and polishing.
[0063] Figure 4 This is a graph showing the harmonic generation intensity and sample particle size of the phosphosilicon indium cadmium nonlinear optical crystal Cd2In3Si2P7 obtained in Example 5 and the commercial ZnGeP2 crystal. DETAILED DESCRIPTION
[0064] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0065] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0066] Example 1
[0067] The compound Cd2In3Si2P7 is prepared by high temperature solid phase method, and its chemical reaction equation is: 2Cd
[0068] +3In+2Si+7P=Cd2In3Si2P7, the specific operation steps are as follows:
[0069] The raw materials Cd, In, Si, and P were evenly mixed and ground in a molar ratio of 2:3:2:7, and then placed in a quartz tube and evacuated to 10 -3 Pa and sealed, put into a muffle furnace; heat to 1080℃ at a rate of 50℃ / h, keep constant temperature for 48 hours, reduce to 100℃ at 5℃ / h, close the muffle furnace, cool to room temperature, take out the quartz tube, cut it open, and obtain Cd2In3Si2P7 compound, its X-ray powder diffraction is as follows Figure 2 shown.
[0070] Example 2
[0071] The flux method is used to grow Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal. The specific operation steps are as follows:
[0072] The raw materials Cd, In, Si, P, and SrCl2 were evenly mixed and ground in a molar ratio of 2:3:2:7:4, and then placed in a quartz tube and evacuated to 10 -3Pa and seal it, put it in a muffle furnace; heat it to 1080℃ at a rate of 50℃ / h, keep it constant for 48 hours, then reduce it to 100℃ at 5℃ / h, close the muffle furnace, and after cooling to room temperature, take out the quartz tube, cut it open, wash away the flux SrCl2 with deionized water, and dry it in an oven to obtain Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal. Its crystal structure is as follows Figure 1 Its X-ray powder diffraction is shown as Figure 2 shown.
[0073] The test shows that the space group of Cd2In3Si2P7 crystal is P21, and the unit cell parameters are: α=γ=90°, β=103.772, z=2.
[0074] Example 3
[0075] The Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal is grown by chemical vapor transport method. The specific operation steps are as follows:
[0076] The raw materials Cd, In, Si, and P were uniformly mixed and ground with I2 in a molar ratio of 2:3:2:7 (the concentration of I2 was 5 mg / cm 3 ), put it into a quartz tube, and evacuate it to 10 -3 Pa and sealed, and placed in a tube furnace; the high temperature end or the evaporation end is heated to 1100°C at a rate of 50°C / h, and the low temperature end or the crystallization end is heated to 1000°C at a rate of 50°C / h; the temperature is kept constant for 96 hours, the high temperature end or the evaporation end is reduced to 1000°C at 2°C / h, and the low temperature end or the crystallization end is reduced to 900°C at 20°C / h, the muffle furnace is closed, and after cooling to room temperature, the quartz tube is taken out and cut to obtain a Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal.
[0077] Example 4
[0078] The physical vapor transport method is used to grow Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal. The specific operation steps are as follows:
[0079] The Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal prepared in Example 2 was uniformly mixed and ground with I2 (where the concentration of I2 was 5 mg / cm 3 ), put it into a quartz tube, and evacuate it to 10 -3Pa and sealed, and placed in a tube furnace; the high temperature end or the evaporation end is heated to 1100°C at a rate of 50°C / h, and the low temperature end or the crystallization end is heated to 1000°C at a rate of 50°C / h; the temperature is kept constant for 96 hours, the high temperature end or the evaporation end is reduced to 1000°C at 2°C / h, and the low temperature end or the crystallization end is reduced to 900°C at 20°C / h, the muffle furnace is closed, and after cooling to room temperature, the quartz tube is taken out and cut to obtain a Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal.
[0080] Example 5
[0081] The crucible descent method was used to grow Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystals. The specific operation steps are as follows:
[0082] The Cd source material, In source material, Si source material, and P source material were uniformly mixed in a molar ratio of Cd: In: Si: P = 2: 3: 2: 7, ground, placed in a quartz tube, and evacuated to 10 -5 -10 -1 Pa and sealed, put into a crucible descending furnace, heat to 1080°C at a rate of 30°C / h, and keep the temperature constant for 50 hours to completely melt the raw materials, then vertically descend at a rate of 0.1°C / h to grow crystals. After the crystal growth is completed, cool to room temperature at a rate of 30°C / h to obtain the Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal.
[0083] The test shows that the crystal structure, space group and unit cell parameters of the Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal obtained in Examples 3-5 are basically the same as those of the Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal in Example 2.
[0084] Example 6
[0085] The infrared transmission spectrum of the Cd2In3Si2P7 phosphorus silicon indium cadmium nonlinear optical crystal obtained in Example 5 after directional cutting and polishing is shown in the figure below. Figure 3 As shown, Cd2In3Si2P7 crystal has good infrared transmittance in the 2.5-10 micron band.
[0086] The Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal obtained in Example 2-4 also has basically the same infrared transmittance as the Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal in Example 5.
[0087] Example 7
[0088] The nonlinear optical crystal Cd2In3Si2P7 (denoted as CISP) and the commercial ZnGeP2 crystal (denoted as ZGP) obtained in Example 5 were sieved into five particle size ranges, and they were placed in five sample boxes for frequency doubling effect testing. The frequency doubling intensity and sample particle size curve under 2.05μm laser testing is shown in Figure 4 .from Figure 4 It can be seen that the double frequency intensity of Cd2In3Si2P7 is 2.2 times that of ZnGeP2.
[0089] The Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal obtained in Example 2-4 also has substantially the same frequency doubling intensity as that of the Cd2In3Si2P7 phospho-silicon-indium-cadmium nonlinear optical crystal in Example 5.
[0090] The above is a description of the exemplary embodiments of the present invention. However, the protection scope of the present application is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A phosphorus silicon indium cadmium compound, characterized in that: Its chemical formula is Cd2In3Si2P7.
2. The phosphorus silicon indium cadmium compound according to claim 1, characterized in that The preparation method of the phosphorus silicon indium cadmium compound comprises: mixing a Cd source material, an In source material, a Si source material and a P source material, grinding them, and calcining them at a high temperature to obtain the phosphorus silicon indium cadmium compound.
3. The method for preparing the phosphorus silicon indium cadmium compound according to claim 1 or 2, characterized in that: The preparation method comprises: mixing a Cd source material, an In source material, a Si source material and a P source material, grinding them, and calcining them at a high temperature to obtain the phosphorus silicon indium cadmium compound. Preferably, in the Cd source material, In source material, Si source material and P source material, the molar ratio of the elements Cd, In, Si and P is 2:3-4:2:7-8. Preferably, the Cd source material is selected from Cd element or Cd3P2. Preferably, the In source material is selected from In single substance or InP. Preferably, the Si source material is selected from Si element. Preferably, the P source material is selected from P element. Preferably, the high temperature calcination comprises: heating to 950°C-1100°C and then calcining.
4. A phospho-silicon-indium-cadmium nonlinear optical crystal, characterized in that: Its chemical formula is Cd2In3Si2P7; the phosphorus silicon indium cadmium nonlinear optical crystal belongs to the monorhombic crystal system.
5. The phospho-silicate-indium-cadmium nonlinear optical crystal according to claim 4, characterized in that: The space group of the phospho-silicate-indium-cadmium nonlinear optical crystal is P21, and the unit cell parameters are: α=γ=90°, β=103, z=2. Preferably, the unit cell parameters of the phospho-silicate-indium-cadmium nonlinear optical crystal are: α=γ=90°, β=103.772, z=2.
6. The method for preparing the phospho-silicon-indium-cadmium nonlinear optical crystal according to claim 4 or 5, characterized in that: The preparation method comprises: The Cd source material, the In source material, the Si source material and the P source material are mixed, a transport agent and / or a co-solvent are added, the mixture is ground, and the mixture is calcined at a high temperature to obtain the phosphorus silicon indium cadmium nonlinear optical crystal.
7. The preparation method according to claim 6, characterized in that: The molar ratio of the element Cd in the Cd source material, the element In in the In source material, the element Si in the Si source material, and the element P in the P source material is 2:3-4:2:7-8. Preferably, the Cd source material is selected from Cd element or Cd3P2. Preferably, the In source material is selected from In single substance or InP. Preferably, the Si source material is selected from Si element. Preferably, the P source material is selected from P element. Preferably, the flux is selected from at least one of SrCl2, SrBr2, SrI2, BaCl2, BaBr2 and BaI2. Preferably, the transport agent is selected from at least one of I2 element, NH4Cl, NH4Br, and NH4I. Preferably, the molar ratio of the element Cd in the Cd source material, the element In in the In source material, the element Si in the Si source material, the element P in the P source material, and the flux is 2:3-4:2:7-8:4-10. Preferably, the concentration of the transport agent is 1 mg / cm 3 -20 mg / cm 3 .
8. The preparation method according to claim 6 or 7, characterized in that: The method for preparing the phospho-silicate-indium-cadmium nonlinear optical crystal further includes: mixing the prepared phospho-silicate-indium-cadmium nonlinear optical crystal with a second transport agent, grinding the crystal, and calcining the crystal at a high temperature to obtain the phospho-silicate-indium-cadmium nonlinear optical crystal. Preferably, the concentration of the second transport agent is 1 mg / cm 3 -20 mg / cm 3 Preferably, the second transport agent is selected from at least one of I2 elemental substance, NH4Cl, NH4Br, and NH4I. Preferably, the high temperature calcination is carried out at a vacuum degree of 10 -5 -10 -1 Pause and proceed. Preferably, the high temperature calcination comprises: heating to 950°C-1100°C and then calcining.
9. Use of the phospho-silicate-indium-cadmium nonlinear optical crystal according to claim 4 or 5 in the field of nonlinear optics.
10. A nonlinear optical device, characterized in that: The nonlinear optical device comprises the phosphosilicon indium cadmium nonlinear optical crystal according to claim 4 or 5.
Citation Information
Cited By
Phosphorus-doped cadmium selenide target material and preparation method thereof
CN117623777A