3-4mm large-particle octahedral diamond and synthesis method thereof
By using the water mist method to prepare alloy powder and vacuum sintering in diamond synthesis, combined with specific assembly structures and high-temperature and high-pressure synthesis technology, the problems of low yield and poor quality of diamond synthesis in the existing technology are solved, and high yield and high hardness are achieved The synthesis of 3-4mm large-grain octahedral diamonds has improved economic benefits.
Patent Information
- Application Number
- CN202411093525.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-05
AI Technical Summary
In the prior art, the single production of diamond synthesis is low and the quality is poor, especially the synthesis method of carat-grade large-grain diamonds has limitations and is not economical, so further improvement is needed.
The alloy powder is prepared by water mist method, mixed graphite and alloy powder for vacuum sintering, and high-temperature and high-pressure synthesis is carried out in a six-sided top press. Through specific assembly structures and temperature pressure curves, the crystal surface accumulation of diamond is optimized to form 3- 4mm large particle octahedral diamond.
实现了高产量、高品质的3-4mm大颗粒八面体钻石的合成,硬度最大,经济效益高,优于传统方法。
Smart Images

Figure HDA0004987227320000011 
Figure HDA0004987227320000012 
Figure HDA0004987227320000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of superhard material synthesis, in particular to a 3-4 mm large-grain octahedral diamond and a synthesis method thereof. Background Art
[0002] The synthesis of artificial diamonds is usually carried out by a six-sided top press under high temperature and high pressure. The pressure and temperature conditions for graphite conversion to diamond are reduced through the action of a multi-alloy catalyst. In this process, the metal catalyst not only participates in the formation of diamond nuclei under high temperature and high pressure. At present, large-grain diamonds, especially carat-level diamonds, synthesized by domestic and foreign companies and organizations engaged in diamond synthesis usually adopt the seed method and temperature difference method. However, this method has limitations, the single output is relatively low, and the economy is not high, and further improvement is needed. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art seed method, that is, low single yield and poor quality, and to provide a 3-4 mm large-grain octahedral diamond with strong impurity removal ability, maximum packing density and maximum hardness and a synthesis method thereof.
[0004] One of the purposes of the present invention is to provide a method for synthesizing 3-4 mm large-grain octahedral diamonds, comprising the following steps:
[0005] S1. Alloy powder raw materials are configured according to the mass ratio and alloy powder is prepared by water mist method;
[0006] S2. Prepare mother powder;
[0007] S3. The graphite, alloy powder and mother powder are fully mixed and granulated and then pressed into graphite columns;
[0008] S4. vacuum sintering the graphite column;
[0009] S5. Assemble according to a specific structure;
[0010] S6. Perform high temperature and high pressure synthesis in a six-sided top press according to the temperature and pressure curve.
[0011] Preferably, in step S1, the alloy powder raw material is formulated in the following mass proportions: 50%-51.5% iron metal, 0.1%-0.5% copper metal, 25.5%-28.5% cobalt metal, 10.0%-10.6% nickel metal, and 5.2%-6.6% silicon, calcium and barium.
[0012] Preferably, in step S2, d10 diamond powder is added to acetone solution, dispersant SCN and anhydrous ethanol are used as dispersants in a ratio of 1:3, and natural flake graphite with 10 ppm ash is added for dilution to obtain a mother powder.
[0013] Preferably, in step S3, the graphite column is prepared by mixing graphite with 0 ash purity and alloy powder in a mass ratio of 48:52, and then adding 1% by mass of mother powder.
[0014] Preferably, in step S4, the prefabricated graphite column is vacuum sintered at 1150° C., kept at this temperature for 6 hours, and cooled to 300° C. with nitrogen, after which the reduction furnace is opened and the graphite column is taken out for natural cooling.
[0015] Preferably, in step S5, the external components of the specific structure are formed by composite pressing of phyllite and dolomite, and the internal components include a 2 mm thick high-purity magnesium oxide tube, a 0.2 mm thick heating steel belt, a conductive molybdenum circle with thicknesses of 0.5 mm and 0.7 mm at both ends respectively, two 13 mm thick barium zirconate rings, and a 26 mm diameter conductive steel ring.
[0016] The second object of the present invention is to provide a 3-4 mm large-grain octahedral diamond synthesized according to the above method.
[0017] The present invention has the following advantages: alloy powder is prepared by adding rare earth and other trace elements into the catalyst, thereby creating more sufficient impurity-removing conditions for diamond growth; the unique assembly structure can regulate and adjust the internal temperature field distribution of the synthesis chamber, and cooperate with the high-temperature and high-pressure synthesis curve to make the (1, 1, 1) crystal plane of the diamond crystal preferentially stacked, and the hardness is the highest among all the diamond faces, and the final macroscopic performance is a large octahedral diamond single crystal, which is superior to the traditional sheet catalyst method, has a high single synthesis output, good diamond single crystal quality, and high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic diagram of the assembly structure of the present invention;
[0019] Figure 2 is a schematic diagram of high temperature and high pressure synthesis of the present invention;
[0020] Figure 3 It is a product schematic diagram of the present invention.
[0021] In the figure, 1. talc; 2. dolomite; 3. artificial graphite tube; 4. pure magnesium oxide tube; 5. conductive molybdenum circle; 6. barium zirconate ring; 7. conductive steel ring. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the specific embodiments of the present invention will be clearly and completely described below.
[0023] A 3-4 mm large octahedral diamond is synthesized according to the following method:
[0024] S1. Configuration of catalyst alloy powder: Cobalt, nickel and copper elements are added to the iron-based catalyst. The catalyst alloy powder is composed of the following raw materials in the following mass ratio: 50%-51.5% iron metal, 0.1%-0.5% copper metal, 25.5%-28.5% cobalt metal, 10.0%-10.6% nickel metal, 5.2%-6.6% silicon calcium barium. The prepared catalyst powder is smelted and made into 250 mesh alloy powder by water mist method;
[0025] S2. Preparation of mother powder: Add d10 diamond powder to acetone solution, dispersant SCN and anhydrous ethanol 1:3 as dispersant, and dilute with 10ppm ash natural flake graphite to obtain mother powder;
[0026] S3. Mixed graphite column: Graphite with a purity of 0 ash and alloy powder according to a mass ratio of 48:52, 1% of the mother powder was added and mixed thoroughly, and granulated with a three-stage granulator to prepare high-density particles with a diameter of about 4.5 mm. The particles were pressed with a 315-ton press to produce a synthetic core column with a diameter of 52 mm;
[0027] S4. Sintering and reduction of synthetic core column: The prefabricated graphite column is subjected to vacuum sintering at 1150°C, kept at this temperature for 6 hours, reduced, and cooled to 300°C using nitrogen protection cooling; then the reduction furnace is opened and the graphite core column is taken out for natural cooling, and then vacuum packaging is performed;
[0028] S5. According to Figure 1 The specific structure shown is assembled: the external component of the specific structure is formed by composite pressing of pyrophyllite 1 and dolomite 2, and the internal component includes a 2mm thick high-purity magnesium oxide tube 4, a 0.2mm thick heating steel belt, a conductive molybdenum circle 5 with a thickness of 0.5mm and 0.7mm at both ends, two 13mm thick barium zirconate rings 6, and a conductive steel ring with a diameter of 26mm;
[0029] S6. High temperature and high pressure synthesis: By precisely configuring the temperature and pressure inside the synthesis chamber of the six-sided top press, a unique synthesis process with pressure and temperature ratio is designed, such as Figure 2 As shown, the (1,1,1) crystal plane of the diamond crystal is preferentially stacked during the growth process. The growth time is 24 hours, and an octahedral industrial large single crystal diamond with a particle size of 3-4 mm is synthesized, as shown in FIG. Figure 3 shown.
[0030] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for synthesizing 3-4 mm large octahedral diamonds. It is characterized in that The following steps are included: S1. Alloy powder raw materials are configured according to the mass ratio and alloy powder is prepared by water mist method; S2. Prepare mother powder; S3. The graphite, alloy powder and mother powder are fully mixed and granulated and then pressed into graphite columns; S4. vacuum sintering the graphite column; S5. Assemble according to a specific structure; S6. Perform high temperature and high pressure synthesis in a six-sided top press according to the temperature and pressure curve.
2. A method for synthesizing 3-4 mm large-grain octahedral diamonds according to claim 1, It is characterized in that In step S1, the alloy powder raw material is prepared in the following proportions by mass: 50%-51.5% iron metal, 0.1%-0.5% copper metal, 25.5%-28.5% cobalt metal, 10.0%-10.6% nickel metal, and 5.2%-6.6% silicon, calcium and barium.
3. A method for synthesizing 3-4 mm large-grain octahedral diamonds according to claim 1, It is characterized in that In step S2, d10 diamond powder is added to acetone solution, dispersant SCN and anhydrous ethanol are used as dispersants in a ratio of 1:3, and natural flake graphite with 10 ppm ash is added for dilution to obtain a mother powder.
4. A method for synthesizing 3-4 mm large-grain octahedral diamonds according to claim 1, It is characterized in that In step S3, the graphite column is prepared by mixing graphite with a purity of 0 ash and alloy powder in a mass ratio of 48:52, and then adding 1% by mass of mother powder.
5. A method for synthesizing 3-4 mm large-grain octahedral diamonds according to claim 1, It is characterized in that In step S4, the prefabricated graphite column is vacuum sintered at 1150°C, kept at this temperature for 6 hours, and cooled to 300°C with nitrogen. After that, the reduction furnace is opened and the graphite column is taken out for natural cooling.
6. A process for synthesizing 3-4 mm large octahedral diamond according to claim 1, It is characterized in that In step S5, the external components of the specific structure are made of talc and dolomite composite pressed, and the internal components include a 2mm thick high-purity magnesium oxide tube, a 0.2mm thick heating steel belt, a conductive molybdenum circle with a thickness of 0.5mm and 0.7mm at both ends respectively, two barium zirconate rings with a thickness of 13mm, and a conductive steel ring with a diameter of 26mm.
7. A 3-4 mm large-grain octahedral diamond prepared by the synthesis method according to any one of claims 1-6.
Citation Information
Cited By
Artificial diamond single crystal generation process
CN120268316A
Large-particle colorless diamond and synthesis method thereof
CN122586030A