Preparation method and application of high-conductivity high-strength light Cu / basalt fiber composite wire
By depositing metallic copper on the surface of basalt fibers, high-conductivity and high-strength Cu/basalt fiber composite conductors are prepared, solving the problem that the insulation of basalt fibers limits their application in the field of power transmission, and realizing low-cost, environmentally friendly large-scale production and widespread application.
Patent Information
- Application Number
- CN202411002733.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-05
AI Technical Summary
Basalt fiber is limited in the field of power transmission due to its insulation properties. Traditional alternatives are costly, complex in process, and difficult to apply on a large scale.
After sensitization with stannous chloride hydrochloric acid solution and activation with silver nitrate aqueous solution, metallic copper is deposited on the surface of basalt fibers using chemical plating technology to prepare highly conductive and high-strength Cu/basalt fiber composite wires.
It achieves high conductivity (3.13×10⁸S/m), high mechanical strength (1561MPa), low density (2.93g/cm³) and excellent high-frequency stability, making it suitable for multiple applications and reducing production costs and environmental impact.
Smart Images

Figure CN118899121A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of wire manufacturing, and specifically relates to a preparation method and application of a high-conductivity, high-strength and lightweight Cu / basalt fiber composite wire. Background Art
[0002] For a long time, traditional pure copper wire has been widely used in power transmission, telecommunications, aerospace, miniaturization and lightweight of electronic devices due to its high electrical conductivity. However, its relatively poor mechanical strength makes it unsuitable for high-pressure scenarios. Its relatively high density and rigidity bring difficulties and challenges to the installation and maintenance processes. Its relatively poor stability and easy oxidation corrosion shorten its service life and reduce its reliability. Its relatively high cost limits its application in more fields.
[0003] Basalt fiber is derived from natural basalt rock. It is a continuous fiber extracted after melting the rock at a temperature of 1450℃-1500℃. It has a low density and has good mechanical properties, elastic modulus, thermal stability (200℃-800℃), flame retardancy, corrosion resistance and low hygroscopicity. After being discarded, it can be converted into a soil matrix through a biodegradation process. Basalt fiber and its composite materials are widely used in national defense, fire protection, aerospace, construction, chemical industry, transportation and other fields. Specific uses include fiber reinforcement materials, friction materials, thermal insulation materials, shipbuilding materials, automotive industry parts, high-temperature filter cloth and fire protection materials. However, the main components of basalt fiber are silicon dioxide, iron oxide and calcium oxide, etc., which do not have good conductivity and are a typical electrical insulation material. This property limits the application of basalt fiber in the field of power transmission.
[0004] In order to overcome these challenging problems, the present invention introduces chemical plating technology. Under the premise of maintaining the original physical and chemical properties of basalt fiber such as light weight, flame retardancy, thermal stability, corrosion resistance and environmental friendliness, the present invention further makes up for the shortcomings of basalt fiber in conductivity through environmentally friendly, high-yield and low-cost means, giving it higher conductivity, making it lighter, safer, more durable, more versatile, more widely used, and easier to install and maintain than traditional pure copper wire, thus becoming an effective alternative to traditional pure copper wire in the field of power transmission.
[0005] At present, the common alternative to the inherent defects of traditional pure copper wires at home and abroad is to deposit high-strength and lightweight non-metallic materials on the surface of metal matrix materials and implement winding, pressing, drawing and other processes to prepare composite wires with high conductivity. For example, patent CN110444320B reports that the aluminum matrix is infiltrated into the gaps between the carbon fiber filaments of the carbon fiber bundle through ultrasound, pulsed magnetic field, cooling, extrusion and other steps. The obtained carbon fiber reinforced aluminum-based composite wire has good conductivity, but its tensile strength is only 114MPa, which is lower than conventional alloy wires such as 6101, 6063, 6061, and even lower than 1350 pure aluminum wire (124MPa). The durability and reliability are not ideal, which shortens the service life in high-pressure scenarios. For example, patent CN117079890A reports that graphene coating is uniformly deposited on the upper and lower surfaces of high-purity copper foil by chemical vapor deposition, and then the conductivity of the graphene / copper composite wire obtained by curling, rough drawing, fine drawing, annealing and other steps reaches 104.5% IACS, but the copper content of its original metal substrate is required to be greater than 99.95%, which increases the production cost and faces huge challenges in economic feasibility. For example, patent CN113012860A reports that copper / graphene oxide composite film is prepared by pulse electrodeposition, and then the conductivity of the copper / nanocarbon composite wire obtained by welding, winding, packaging, drawing, high vacuum heat treatment and other steps can reach 150% IACS, but the implementation conditions of the above steps are strict, the equipment used is expensive, and the process is cumbersome, making it difficult to achieve large-scale industrial application. As reported in patent CN114446541A, a preparation device including main components such as a composite chamber, a wire-reeling mechanism, and a feed roller is built by oneself, and the metal / graphene composite wire obtained through parameter adjustment, growth, winding, hot pressing, cooling and other steps has a high conductivity. However, the above-mentioned self-made preparation device has a complex structure, is difficult to operate, and has a small production scale. In addition, the production and hot pressing steps all need to maintain high temperature conditions, and the process consumes a lot of energy, which is not conducive to ecological environmental protection and sustainable development. Summary of the invention
[0006] The purpose of the present invention is to solve the problem that basalt fiber is limited in the field of power transmission due to its insulation. The present invention provides a method for preparing a high-conductivity, high-strength and lightweight Cu / basalt fiber composite conductor and its application. The method first uses a stannous chloride hydrochloric acid solution to sensitize the original basalt fiber substrate, then uses a silver nitrate aqueous solution to activate the basalt fiber surface, and then uses chemical plating technology to deposit metal copper on the basalt fiber surface, thereby obtaining a Cu / basalt fiber composite conductor with high conductivity. The Cu / basalt fiber composite conductor prepared by the method has a maximum conductivity of 3.13×10 8 The electrical conductivity of S / m is much higher than that of traditional pure copper wire 5.89×10 7 S / m conductivity; its maximum density is 2.93g / cm 3, much lower than the traditional pure copper wire 8.96g / cm 3 The composite conductor has a density of up to 1561MPa and can maintain excellent stability in the frequency range of 1,000,000-5,000,000Hz. The composite conductor has broad application prospects in the fields of telecommunications, marine engineering, microelectronics, new energy, chemical engineering, automobile manufacturing, aerospace, miniaturization and lightweight of electronic devices.
[0007] A method for preparing a high-conductivity, high-strength, lightweight Cu / basalt fiber composite conductor is carried out according to the following steps:
[0008] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0009] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0010] c. Chemical copper plating: first, 8g of copper sulfate pentahydrate, 46g of ethylenediaminetetraacetic acid, 5ppm 2,2′-bipyridine, 5-15ml of formaldehyde and 800ml of water are prepared into a copper deposition solution, and then the pH value of the copper deposition solution is adjusted to 13 with sodium hydroxide, and then the basalt fiber activated in step b is immersed in the copper deposition solution, and the temperature is continuously kept at 20°C-60°C for 60 minutes, and the pH value of the copper deposition solution is maintained at 13 with sodium hydroxide, and metallic copper is deposited on the surface of the basalt fiber, and then the basalt fiber after copper deposition is fully washed with deionized water, and then dried at a temperature of 105°C for 60 minutes, so as to obtain a mechanical strength range of 1480MPa-1561MPa; a density range of 2.93-3.48g / cm 3 , the conductivity range is 2.44×10 8 S / m-3.03×10 8 S / m Cu / basalt fiber composite conductor.
[0011] The application of the Cu / basalt fiber composite wire obtained by the method in the field of preparing composite wires.
[0012] Compared with the prior art, the preparation method and application of a high-conductivity, high-strength and lightweight Cu / basalt fiber composite conductor described in the present invention have the following characteristics and advantages:
[0013] 1. The present invention uses cheap and readily available raw materials to replace expensive activators such as PtCl2, and avoids conventional acid, alkali and heat treatment of the basalt fiber surface, which fully demonstrates the environmental friendliness of the above technical solution, simplifies the production process, significantly reduces production costs, and improves cost-effectiveness, making it suitable for large-scale production.
[0014] 2. The chemical plating technology described in the present invention effectively enhances the inherent properties of basalt fiber, such as light weight, flame retardancy, corrosion resistance, and environmental friendliness, and gives full play to its inherent advantages, and integrates the highlights of basalt fiber and metallic copper that focus on different aspects.
[0015] 3. The micron-level ultra-thin metal coating on the surface of the Cu / basalt fiber composite conductor prepared by the present invention achieves a 3.13×10 8 The electrical conductivity of S / m is 6 times that of traditional copper wire; and its lightness is particularly suitable for industries and fields with strict requirements on weight and space.
[0016] 4. The Cu / basalt fiber composite conductor prepared by the present invention inherits the excellent mechanical properties and thermal stability of the original basalt fiber substrate, and further improves its mechanical strength to 1561MPa, while supporting its high conductivity in a wider temperature range, thus being suitable for extreme environments such as high temperature and extremely low temperature.
[0017] 5. The chemical plating technology described in the present invention can accurately control the surface copper plating process, and flexibly customize the conductivity of the Cu / basalt fiber composite conductor by adjusting the copper deposition treatment temperature, so that it is widely applicable to a variety of application scenarios.
[0018] The method of the present invention does not require surface pretreatment of the original basalt fiber substrate, and the tin chloride / hydrochloric acid sensitizer helps to create a firm and uniform copper deposition site on the surface of the basalt fiber. The silver nitrate activation solution replaces the traditional, rare, and expensive palladium chloride activator to reduce the activation treatment cost. The chemical plating technology is implemented at different temperatures to flexibly customize the conductivity of the Cu / basalt fiber composite conductor. In addition, the technical solution adopted by the present invention also has significant advantages such as simple process, low cost, and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1Scanning electron microscope images of original basalt fiber and copper-plated basalt fiber used in the present invention: (A) original basalt fiber bundle, (B) original single basalt fiber, (C) cross section of original single basalt fiber, (D) low magnification of copper-plated basalt fiber bundle at 50°C, (E) high magnification of copper-plated basalt fiber bundle, (F) surface of copper-plated single basalt fiber, (G) cross section of copper-plated basalt fiber bundle, (H) cross section of copper-plated single basalt fiber, (I) copper-plated layer on single basalt fiber;
[0020] Figure 2 is a density diagram of the original and copper-plated basalt fibers of the present invention;
[0021] Figure 3 This is the conductivity diagram of the copper-plated basalt fiber of the present invention. DETAILED DESCRIPTION
[0022] The present invention is further described below in conjunction with specific embodiments, which are used to help those skilled in the art further understand the present invention, but are not limited to the scope of the embodiments of the present invention.
[0023] Example 1
[0024] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0025] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0026] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 5 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand for 60 minutes at 50°C. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.18 g / cm 3 , mechanical strength is 1452MPa, electrical conductivity is 2.2×10 8 S / m Cu / basalt fiber composite conductor.
[0027] Example 2
[0028] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0029] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0030] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 10 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand at 55°C for 60 minutes. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.48 g / cm 3 , mechanical strength is 1528MPa, electrical conductivity is 3.13×10 8 S / m Cu / basalt fiber composite conductor.
[0031] Example 3
[0032] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0033] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0034] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 15 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand for 60 minutes at 48°C. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.23 g / cm 3 , mechanical strength is 1448MPa, electrical conductivity is 2.15×10 8 S / m Cu / basalt fiber composite conductor.
[0035] Example 4
[0036] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0037] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0038] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 10 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand for 60 minutes at 20°C. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a bulk density of 2.93 g / cm 3 , mechanical strength is 1551MPa, electrical conductivity is 2.43×10 8 S / m Cu / basalt fiber composite conductor.
[0039] Example 5
[0040] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0041] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0042] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 10 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand at 30°C for 60 minutes. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.01 g / cm 3 , mechanical strength is 1561MPa, electrical conductivity is 2.49×10 8 S / m Cu / basalt fiber composite conductor.
[0043] Example 6
[0044] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0045] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0046] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 10 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand for 60 minutes at 40°C. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.23 g / cm 3 , mechanical strength is 1520MPa, electrical conductivity is 2.59×10 8 S / m Cu / basalt fiber composite conductor.
[0047] Example 7
[0048] a. Sensitization: At a temperature of 25°C, the original basalt fiber substrate was immersed in a sensitizer solution prepared by 10g of stannous chloride, 25ml of 37% hydrochloric acid and 800ml of water, and allowed to stand for 60 minutes, and then the sensitized basalt fiber was fully washed with deionized water;
[0049] b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2g of silver nitrate and 800ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water;
[0050] c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 36 g of ethylenediaminetetraacetic acid, 10 ppm of 2,2′-bipyridine, 10 ml of formaldehyde and 800 ml of water were used to prepare a copper deposition solution, and then the pH value of the copper deposition solution was adjusted to 13 with sodium hydroxide. Then, the basalt fiber activated in step b was immersed in the copper deposition solution, and was allowed to stand at 60°C for 60 minutes. At the same time, the pH value of the copper deposition solution was maintained at 13 with sodium hydroxide, and metallic copper was deposited on the surface of the basalt fiber. Then, the basalt fiber after copper deposition was fully washed with deionized water, and then dried at 105°C for 60 minutes to obtain a basalt fiber with a density of 3.28 g / cm 3 , mechanical strength is 1480MPa, electrical conductivity is 2.57×10 8 S / m Cu / basalt fiber composite conductor.
[0051] Example 8
[0052] The microstructure and important properties of the Cu / basalt fiber composite conductor obtained by the present invention are as follows:
[0053] Surface morphology of Cu / basalt fiber composite conductor prepared by chemical plating technology:
[0054] The chemical deposition copper plating on the surface of basalt fiber follows a three-step process of sensitization-activation-chemical plating; the surface morphology of basalt fiber before and after chemical plating technology is as follows Figure 1 ,As can be seen from the figure, the metal coating covers the surface of the treated basalt fiber comprehensively and evenly, showing significant firmness and consistency;
[0055] Density of Cu / basalt fiber composite conductor prepared by chemical plating technology:
[0056] The density of the original basalt fiber matrix is 2.68g / cm 3 , reflecting its inherent lightness; the density of the prepared material at room temperature is 2.93 g / cm 3 The density after treatment at 30°C is 3.01 g / cm3 The density after treatment at 40°C is 3.23 g / cm 3 The density after treatment at 50°C is 3.48 g / cm 3 The density after treatment at 60°C is 3.28 g / cm 3 (like Figure 2 ); The data show that the density of the treated Cu / basalt fiber composite conductor is closely related to the copper deposition treatment temperature, and is much lower than the bulk density of traditional pure copper wire (8.94 g / cm 3 , that is, chemical plating technology can enhance various performances of the original basalt fiber substrate without significantly increasing its density;
[0057] Mechanical properties of Cu / basalt fiber composite conductors prepared by chemical plating technology:
[0058] Chemical deposition copper plating at a temperature of 20℃-60℃ can gradually improve the mechanical properties of basalt fiber. The mechanical strength of the original basalt fiber substrate is 1279MPa, reflecting its inherent excellent mechanical properties. After copper deposition at room temperature, the mechanical strength increases to 1551MPa. As the treatment temperature increases to 30℃, the mechanical strength increases to 1561MPa. When the treatment temperature reaches 40℃, the mechanical strength slightly decreases to 1520MPa. At a temperature of 50℃, the mechanical strength continues to increase to 1528MPa. At a temperature of 60℃, the mechanical strength decreases slightly again to 1480MPa. The data show that chemical plating technology significantly enhances the mechanical properties of basalt fiber, and the copper deposition effect is best at a temperature of 30℃, at which time the mechanical strength of the Cu / basalt fiber composite conductor reaches the highest.
[0059] Conductivity of Cu / basalt fiber composite conductor prepared by chemical plating technology:
[0060] The conductivity of basalt fiber treated by chemical plating technology at a temperature of 20-60°C is: 2.44×10 8 S / m, after treatment at 30°C, is 2.49×10 8 S / m, after treatment at 40°C, is 2.86×10 8 S / m, after treatment at 50°C, is 3.13×10 8 S / m, after treatment at 60°C, is 2.57×10 8 S / m (such as Figure 3 ); The data show that the conductivity of the treated Cu / basalt fiber composite wire is closely related to the copper deposition treatment temperature and is much higher than the conductivity of the traditional pure copper wire (5.98×10 7 S / m, and reaches the best state at the treatment temperature of 50℃;
[0061] High frequency stability of Cu / basalt fiber composite conductor prepared by chemical plating technology:
[0062] The conductivity of basalt fiber treated by chemical plating technology at a temperature of 20-60°C at different working frequencies is: 1.72×10 8 S / m, after being treated at 50°C and placed in a 10Hz low frequency environment, is 3.89×10 8 S / m, after being treated at 20°C and placed in a 1,000,000Hz high frequency environment, is 1.05×10 8 S / m, after being treated at 60°C and placed in a 1,000,000Hz high frequency environment, is 8.21×10 7 S / m, after being treated at 20°C and placed in a 5,000,000Hz high frequency environment, is 2.88×10 7 S / m, after being treated at 60°C and placed in a 5,000,000Hz high frequency environment, is 1.80×10 7 S / m; The data show that the high-frequency stability of the prepared Cu / basalt fiber composite conductor is closely related to the copper deposition treatment temperature, and both exhibit excellent high-frequency stability.
Claims
1. A method for preparing a high-conductivity, high-strength and lightweight Cu / basalt fiber composite conductor, characterized in that Follow these steps: a. Sensitization: At 25°C, soak the original basalt fiber substrate in a sensitizer solution prepared by 10g stannous chloride, 25ml 37% hydrochloric acid and 800ml water, and let it stand for 60 minutes. Then, wash the sensitized basalt fiber thoroughly with deionized water. b. Activation: At a temperature of 25°C, the basalt fiber sensitized in step a was immersed in an activator solution prepared by 2 g of silver nitrate and 800 ml of water, and allowed to stand for 60 minutes, and then the activated basalt fiber was fully washed with deionized water; c. Chemical copper plating: first, 8 g of copper sulfate pentahydrate, 46 g of ethylenediaminetetraacetic acid, 5 ppm of 2,2′-bipyridine, 5-15 ml of formaldehyde and 800 ml of water are prepared into a copper deposition solution, and then the pH value of the copper deposition solution is adjusted to 13 with sodium hydroxide, and then the basalt fiber activated in step b is immersed in the copper deposition solution, and the temperature is continuously kept at 20°C-60°C for 60 minutes, and the pH value of the copper deposition solution is maintained at 13 with sodium hydroxide, and metallic copper is deposited on the surface of the basalt fiber, and then the basalt fiber after copper deposition is fully washed with deionized water, and then dried at a temperature of 105°C for 60 minutes, so as to obtain a mechanical strength range of 1480MPa-1561MPa; a density range of 2.93-3.48 g / cm 3 , the conductivity range is 2.44×10 8 S / m-3.03×10 8 S / m Cu / basalt fiber composite conductor.
2. Application of the Cu / basalt fiber composite conductor obtained by the method as claimed in claim 1 in the field of preparing composite conductors.
Citation Information
Cited By
Preparation method for improving conductivity of carbon black