Carbon-coated lithium lanthanum zirconium gallium oxide-coated titanium phosphate solid electrolyte and preparation method thereof
By doping gallium into lithium lanthanum zirconium oxygen and carbon coated with titanium-based phosphate solid electrolyte, the low conductivity and interface stability of solid electrolyte materials of lithium-ion batteries are solved, and high energy density and high safety are achieved. Lithium-ion battery.
Patent Information
- Application Number
- CN202411195441.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-05
AI Technical Summary
The solid electrolyte materials of existing lithium-ion batteries have problems such as low ion conductivity, poor stability to metal lithium, and large grain boundary resistance, which is difficult to meet the needs of high energy density and high safety in the future.
Carbon-coated lithium lanthanum zirconium gallium oxygen coated titanium-based phosphate solid electrolyte. By doping gallium into lithium lanthanum zirconium oxygen and carbon coated, a stable cubic crystal structure is formed, ionic conductivity is improved, and through sol- The surface coating is carried out by gel method to improve the interface stability with the lithium negative electrode.
It significantly improves the room temperature ion conductivity of lithium-ion batteries, enhances the electrochemical stability of metal lithium, improves grain boundary transmission efficiency, reduces impurity generation, and improves the energy density and safety of the battery.
Smart Images

Figure CN118899522A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte and a preparation method thereof. Background Art
[0002] In recent years, with the growing demand for energy, lithium-ion batteries have been widely used in our daily lives. Due to their advantages such as high energy density, long cycle life, low self-discharge rate, and no memory effect, they have stood out from many energy storage technologies and become the most important part of the current electrochemical energy storage field. In recent years, the application scenarios of lithium-ion batteries have rapidly expanded, from portable electronic products to electric vehicles, home energy storage, industrial energy storage, etc., lithium-ion batteries have penetrated into all aspects of society, which also puts higher requirements on the safety and energy density of lithium-ion batteries.
[0003] Traditional lithium-ion batteries mainly rely on organic liquid electrolytes to conduct lithium ions. The flammable and volatile characteristics of the electrolyte lead to safety risks such as thermal runaway, fire, and explosion in the case of overheating, short circuit, overcharging, and mechanical damage. Safety accidents of new energy vehicles occur from time to time, and ensuring the safe operation of new energy vehicles is the primary task of the current industry development. In recent years, the operation safety of power batteries has been improved to a certain extent through the innovation of battery system structure. Looking to the future, it is an inevitable trend for power batteries to develop from battery structure innovation to material system innovation. In addition, energy density is a key indicator of power lithium batteries. It is expected that in 2025 and 2030, the single cell energy density of the battery cell will gradually achieve the goal of 400-500Wh / kg. However, liquid lithium-ion batteries are limited by the chemical system, and the upper limit of energy density is expected to be 300Wh / kg, which is difficult to meet future strategic needs. Therefore, developing high-safety and high-energy-density energy storage technology to make up for the shortcomings of liquid lithium-ion batteries is an important development direction for lithium-ion batteries in the future.
[0004] Using solid electrolytes to replace liquid electrolytes and developing all-solid-state lithium batteries can solve the energy density bottleneck and safety risks faced by current liquid ion batteries, and become the most promising follow-up technology for the next generation of lithium ion batteries. Currently, the most commonly used solid electrolyte materials are polymer solid electrolytes, oxide solid electrolytes, and sulfide solid electrolytes. Due to the low ion conductivity and narrow electrochemical window of polymer solid electrolytes, the poor stability and high cost of sulfide solid electrolytes, oxide solid electrolytes have become the mainstream.
[0005] Oxide solid electrolytes mainly include LiPON, NASICON, perovskite and garnet structures. Among them, NASICON (LATP, LAGP) and garnet (LLZO) have received widespread attention. Both have wide electrochemical windows and are relatively stable in air, standing out among many solid electrolytes. However, the interfacial stability between LATP and metallic lithium is a challenge. Ti in LATP is a promising target for solid electrolytes. 4+ Will be restored to Ti 3+ Moreover, the chemical and electrochemical incompatibility with lithium leads to a limited electrochemical stability window, increases grain boundary resistance, and generates cracks in adjacent ion channels. At room temperature, the ionic conductivity of LATP is relatively low (10 -4 S / cm). Garnet-type LLZO is stable to metallic lithium and has high ionic conductivity at room temperature, but it has large grain boundary resistance, which affects the overall ion transmission efficiency. In addition, it has two crystal forms. The tetragonal phase has low ionic conductivity at low temperatures (10 -6 S / cm), the cubic phase structure has a higher ionic conductivity at high temperature (10 -3 S / cm), so it needs to be doped to form a stable cubic phase structure to improve its conductivity.
[0006] Therefore, obtaining a solid electrolyte with high ionic conductivity, high stability to metallic lithium negative electrode and low grain boundary resistance and a preparation method thereof are technical problems that need to be solved at present. Summary of the invention
[0007] The object of the present invention is to provide a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte and a preparation method thereof, so as to solve the above technical problems.
[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0009] The present invention provides a method for preparing a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte, comprising the following steps:
[0010] (1) dissolving a first lithium source, a lanthanum source, a zirconium source and a gallium source in water and then adding a nitric acid solution to obtain a solution A, dissolving a carbon source in water to obtain a solution B; adding the solution B to the solution A to adjust the pH to obtain a colorless transparent sol;
[0011] (2) dissolving the second lithium source, phosphorus source, titanium source, aluminum source and the first dispersant in water for nano-processing to obtain a titanium phosphate solid electrolyte precursor slurry, and sequentially spray drying, solid phase sintering and crushing the obtained slurry to obtain a titanium phosphate solid electrolyte powder;
[0012] (3) dispersing titanium phosphate solid electrolyte powder and a second dispersant in water to obtain an electrolyte slurry, mixing a colorless transparent sol into the electrolyte slurry and sequentially performing shear dispersion, aging, a second spray drying and a second solid phase sintering to obtain a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte.
[0013] Further, the first lithium source and the second lithium source independently include one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate, lithium dihydrogen phosphate, lithium chloride and lithium sulfate; the lanthanum source includes one or more of lanthanum oxide, lanthanum nitrate, lanthanum carbonate and lanthanum hydroxide; the zirconium source includes one or more of zirconium oxide, zirconium nitrate, zirconyl nitrate and zirconium n-propoxide; the gallium source includes one or more of gallium oxide, gallium nitrate and gallium chloride;
[0014] The molar ratio of the first lithium source, lanthanum source, zirconium source and gallium source is 6-6.8:3-4:2-3:0.1-0.3.
[0015] Furthermore, the concentration of the nitric acid solution is 0.4-0.6 mol / L, and the amount of the nitric acid solution is 100-500 mL;
[0016] In the step (1), the pH is adjusted to 4-10.
[0017] Furthermore, the carbon source comprises one or more of glucose, citric acid, sucrose, asphalt, polyethylene glycol and polyvinyl alcohol, and the added amount of the carbon source is 5-10% of the total weight of the first lithium source, lanthanum source, zirconium source and gallium source; the concentration of the carbon source in solution B is 0.8-2.5 g / mL; in solution A, the concentration of the lanthanum source is 0.18-0.4 g / mL.
[0018] Further, the phosphorus source comprises one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the titanium source comprises one or more of anatase titanium dioxide, rutile titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; the aluminum source comprises one or more of aluminum oxide, aluminum hydroxide, pseudo-boehmite and aluminum nitrate; the first dispersant and the second dispersant independently comprise one or more of polyvinyl alcohol, polypropylene pyrrolidone, sodium carboxymethyl cellulose, polyvinyl pyrrolidone and polyethylene glycol;
[0019] The molar ratio of the lithium source, the aluminum source, the titanium source and the phosphorus source is 1.1-1.5:0.1-0.5:1.5-1.9:3, wherein the lithium source comprises a first lithium source and a second lithium source;
[0020] The amount of the first dispersant used is 2-10% of the total weight of the titanium source, the phosphorus source, the aluminum source and the second lithium source.
[0021] Furthermore, the nano-treatment is carried out under sand milling, the sand milling speed is 1000-1500rpm, and the sand milling time is 1-3h; the particle size of the titanium phosphate solid electrolyte precursor slurry is 0.2-0.8μm, and the solid content of the titanium phosphate solid electrolyte precursor slurry is 20-50%.
[0022] Furthermore, in the step (2), the inlet temperature of the spray drying is 200-240°C, the outlet temperature is 90-130°C, and the spray particle size is 10-30 μm; the solid phase sintering temperature is 600-1000°C, and the solid phase sintering time is 8-14 hours; the crushing method is mechanical crushing or air flow crushing, and the particle size of the titanium phosphate solid electrolyte powder after crushing is 1-6 μm.
[0023] Furthermore, the dosage of the second dispersant is 1-6% of the weight of the titanium phosphate solid electrolyte powder, and the dosage ratio of the second dispersant to water is 20-60 g: 2000 mL;
[0024] The amount of the colorless transparent sol is 1-10% of the weight of the titanium phosphate solid electrolyte powder.
[0025] Furthermore, the shear dispersion time is 1 to 5 hours, the shear dispersion frequency is 10 to 30 Hz, and the aging time is 1 to 6 hours;
[0026] The inlet temperature of the second spray drying is 200-240°C, the outlet temperature is 90-130°C, and the particle size of the spray is 4-10 μm;
[0027] The second solid-phase sintering is performed in an inert gas, which includes argon or nitrogen; the temperature of the second solid-phase sintering is 500-900° C., and the time of the second solid-phase sintering is 6-13 hours.
[0028] The present invention provides a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte, wherein the chemical formula of lithium lanthanum zirconium gallium oxygen in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 7-3X La3Zr2Ga X O 12 , where 0.1≤X≤0.3;
[0029] The chemical formula of the titanium phosphate solid electrolyte in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 1+Y Al Y Ti 2-Y (PO4)3, where 0.1≤Y≤0.5;
[0030] The coating amount of the lithium lanthanum zirconium gallium oxygen coated titanium phosphate solid electrolyte is 1-10%.
[0031] Beneficial effects of the present invention:
[0032] (1) The present invention replaces Li by doping gallium in the lithium lanthanum zirconium oxygen solid electrolyte + Obtaining higher ionic conductivity and mobility, enabling it to form a stable cubic crystal structure at room temperature, and then adding a carbon source for carbon coating and sintering under inert gas can improve the problem that LLZO reacts with H2O and CO2 in the air, which will generate LiOH and Li2CO3 impurities on its surface and reduce the ionic conductivity.
[0033] (2) The present invention adopts the method of first preparing amorphous carbon-coated lithium lanthanum zirconium gallium oxide and then coating titanium phosphate solid electrolyte to improve the high-valent ion Ti when matching with the lithium negative electrode. 4+ It will be reduced by metallic lithium to form an interfacial intermediate phase with mixed ion and electron conductivity and its interface stability problem. Moreover, due to the high ion conductivity of lithium lanthanum zirconium gallium oxide at room temperature (up to 10 at 25°C), the -2 ~10 -3 S / cm), and its electrochemical stability to metallic lithium is better than that of titanium phosphate. By coating the two, the problem of low ionic conductivity of titanium phosphate at room temperature can be further improved (10 -4 S / cm). In addition, by using the sol-gel method for surface coating, pre-treating it to make it uniformly dispersed, and then calcining it at high temperature, a surface-coated powder with good chemical uniformity, finer particles and narrower particle size distribution can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the XRD pattern of the titanium phosphate solid electrolyte sample obtained in Example 1;
[0035] Figure 2 This is the XRD pattern of the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte sample obtained in Example 1. DETAILED DESCRIPTION
[0036] The present invention provides a method for preparing a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte, comprising the following steps:
[0037] (1) dissolving a first lithium source, a lanthanum source, a zirconium source and a gallium source in water and then adding a nitric acid solution to obtain a solution A, dissolving a carbon source in water to obtain a solution B; adding the solution B to the solution A to adjust the pH to obtain a colorless transparent sol;
[0038] (2) dissolving the second lithium source, phosphorus source, titanium source, aluminum source and the first dispersant in water for nano-processing to obtain a titanium phosphate solid electrolyte precursor slurry, and sequentially spray drying, solid phase sintering and crushing the obtained slurry to obtain a titanium phosphate solid electrolyte powder;
[0039] (3) dispersing titanium phosphate solid electrolyte powder and a second dispersant in water to obtain an electrolyte slurry, mixing a colorless transparent sol into the electrolyte slurry and sequentially performing shear dispersion, aging, a second spray drying and a second solid phase sintering to obtain a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte.
[0040] In the present invention, the first lithium source and the second lithium source independently contain one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate, lithium dihydrogen phosphate, lithium chloride and lithium sulfate. The first lithium source is preferably one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate and lithium dihydrogen phosphate, and the second lithium source is preferably lithium chloride or lithium sulfate.
[0041] In the present invention, the lanthanum source is preferably one or more of lanthanum oxide, lanthanum nitrate, lanthanum carbonate and lanthanum hydroxide; the zirconium source is preferably one or more of zirconium oxide, zirconium nitrate, zirconium oxynitrate and zirconium n-propoxide; the gallium source is preferably one or more of gallium oxide, gallium nitrate and gallium chloride.
[0042] In the present invention, the molar ratio of the first lithium source, lanthanum source, zirconium source and gallium source is 6-6.8:3-4:2-3:0.1-0.3, preferably 6.2-6.6:3.3-3.8:2.3-2.6:0.2, and more preferably 6.4:3.5:2.5:0.2.
[0043] In the present invention, the concentration of the nitric acid solution is 0.4-0.6 mol / L, preferably 0.5 mol / L; the amount of the nitric acid solution is 100-500 mL, preferably 200-300 mL.
[0044] In the present invention, in step (1), the pH is adjusted to 4-10, preferably 6-8, and more preferably 7.
[0045] In the present invention, the carbon source is preferably one or more of glucose, citric acid, sucrose, asphalt, polyethylene glycol and polyvinyl alcohol; the added amount of the carbon source is 5-10% of the total weight of the first lithium source, lanthanum source, zirconium source and gallium source, preferably 6-9%, and more preferably 7-8%; the concentration of the carbon source in the solution B is 0.8-2.5 g / mL, preferably 1.0-2.0 g / mL, and more preferably 1.5 g / mL; in the solution A, the concentration of the lanthanum source is 0.18-0.4 g / mL, preferably 0.2-0.3 g / mL.
[0046] In the present invention, the phosphorus source is preferably one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the titanium source is preferably one or more of anatase titanium dioxide, rutile titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; the aluminum source is preferably one or more of aluminum oxide, aluminum hydroxide, pseudo-boehmite and aluminum nitrate.
[0047] In the present invention, the first dispersant and the second dispersant independently contain one or more of polyvinyl alcohol, polypropylene pyrrolidone, sodium carboxymethyl cellulose, polyvinyl pyrrolidone and polyethylene glycol. The first dispersant is preferably polyvinyl alcohol, polypropylene pyrrolidone or polyethylene glycol, and the second dispersant is preferably polyethylene glycol, polypropylene pyrrolidone or sodium carboxymethyl cellulose.
[0048] In the present invention, the molar ratio of the lithium source, aluminum source, titanium source and phosphorus source is 1.1-1.5:0.1-0.5:1.5-1.9:3, preferably 1.2-1.4:0.2-0.4:1.6-1.8:3, and more preferably 1.3-1.4:0.3:1.7:3, wherein the lithium source comprises a first lithium source and a second lithium source; the amount of the first dispersant used is 2-10% of the total weight of the titanium source, phosphorus source, aluminum source and the second lithium source, preferably 3-9%, and more preferably 4-6%.
[0049] In the present invention, the nano-treatment is carried out under sand milling, the sand milling speed is 1000-1500rpm, preferably 1200rpm; the sand milling time is 1-3h, preferably 2h; the particle size of the titanium phosphate solid electrolyte precursor slurry is 0.2-0.8μm, preferably 0.3-0.6μm; the solid content of the titanium phosphate solid electrolyte precursor slurry is 20-50%, preferably 30-40%, and more preferably 35%.
[0050] In the present invention, in the step (2), the inlet temperature of the spray drying is 200-240°C, preferably 220°C; the outlet temperature is 90-130°C, preferably 110°C; the particle size of the spray is 10-30μm, preferably 20μm; the temperature of the solid phase sintering is 600-1000°C, preferably 700-900°C, and more preferably 800°C; the solid phase sintering time is 8-14h, preferably 10-13h, and more preferably 12h; the crushing method is mechanical crushing or air flow crushing, and the particle size of the titanium phosphate solid electrolyte powder after crushing is 1-6μm, preferably 2-4μm.
[0051] In the present invention, the dosage of the second dispersant is 1-6% of the weight of the titanium phosphate solid electrolyte powder, preferably 2-5%, and more preferably 3-4%; the dosage ratio of the second dispersant to water is 20-60g:2000mL, preferably 30-50g:2000mL, and more preferably 40g:2000mL.
[0052] In the present invention, the amount of the colorless transparent sol is 1 to 10% of the weight of the titanium phosphate solid electrolyte powder, preferably 3 to 8%, and more preferably 5 to 7%.
[0053] In the present invention, the shear dispersion time is 1 to 5 hours, preferably 2 to 4 hours, and more preferably 3 hours; the shear dispersion frequency is 10 to 30 Hz, preferably 20 Hz; the aging time is 1 to 6 hours, preferably 2 to 5 hours, and more preferably 3 to 4 hours.
[0054] In the present invention, the inlet temperature of the second spray drying is 200-240°C, preferably 220°C; the outlet temperature is 90-130°C, preferably 110°C; the spray particle size is 4-10 μm, preferably 5-9 μm, and more preferably 6-8 μm.
[0055] In the present invention, the second solid-phase sintering is carried out in an inert gas, which includes argon or nitrogen, preferably nitrogen; the temperature of the second solid-phase sintering is 500-900°C, preferably 600-800°C, and more preferably 700°C; the time of the second solid-phase sintering is 6-13h, preferably 7-12h, and more preferably 8-10h.
[0056] The present invention provides a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte, wherein the chemical formula of lithium lanthanum zirconium gallium oxygen in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 7-3X La3Zr2Ga X O 12 , where 0.1≤X≤0.3;
[0057] The chemical formula of the titanium phosphate solid electrolyte in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 1+Y Al Y Ti 2-Y (PO4)3, where 0.1≤Y≤0.5.
[0058] In the present invention, X is preferably 0.1, 0.2, or 0.3.
[0059] In the present invention, Y is preferably 0.1, 0.2, 0.3, 0.4, or 0.5.
[0060] In the present invention, the coating amount of the lithium lanthanum zirconium gallium oxide coated titanium phosphate solid electrolyte is 1 to 10%, preferably 2 to 8%, and more preferably 3 to 5%.
[0061] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0062] Example 1
[0063] (1) 500.0 g of battery-grade La(NO3)3·6H2O, 178.0 g of ZrO(NO3)2, 14.8 g of Ga(NO3)3, and 190.4 g of LiNO3 were dissolved in 1300 mL of deionized water, and then 250 mL of 0.5 mol / L nitric acid solution was added to form solution A. 54.0 g of citric acid was dissolved in 50 mL of deionized water, and then solution B was slowly added to solution A. The mixed solution was transferred into a glass reactor and stirred at a speed of 30 r / min for 3 h in the glass reactor to form a mixed solution. Ammonia water was then added to adjust the pH to about 6.8, and stirring was continued for 1 h to obtain a carbon-coated amorphous lithium lanthanum zirconium gallium oxygen colorless and transparent sol.
[0064] (2) 200.6 g of PVP powder was dissolved in 6500 mL of deionized water, and after mixing evenly, 1000.0 g of titanium dioxide, 2528.9 g of ammonium dihydrogen phosphate, 112.2 g of aluminum oxide and 368.0 g of lithium carbonate were added in sequence. After being placed in a shearing machine for shearing dispersion at a frequency of 20 Hz for 30 min, it was transferred to a sand mill for wet grinding at 1500 rpm for 2 h. The grinding particle size was controlled at D50 = 0.3-0.5 μm. The ground slurry was centrifugally spray-dried, and the inlet and outlet temperatures were controlled to be 220 ° C and 110 ° C, respectively. At the same time, the spray-dried particle size was controlled to be D50 = 25 ± 5 μm to obtain lithium aluminum titanium phosphate precursor powder. The lithium aluminum titanium phosphate precursor powder was solid-phase sintered at a sintering temperature of 850 ° C for 12 h. The sintered material was first jaw-rolled and then air-milled to a grinding particle size of D50 = 1-2 μm.
[0065] (3) 40.0 g of polyethylene glycol was dissolved in 2000 mL of deionized water, and then 1000 g of the titanium phosphate solid electrolyte powder in step (2) was added. After shearing and dispersing evenly, 42.0 g of the colorless and transparent sol in step (1) was added to the dispersed solution, and the shearing was continued at a frequency of 25 Hz for 2 h. The slurry was then aged for 4 h, and then two-fluid spray drying was performed, with an inlet temperature of 220° C. and an outlet temperature of 110° C. The particle size D50 was controlled to be 6-8 μm. The spray material was solid-phase sintered in an argon atmosphere at a sintering temperature of 800° C. for 10 h. After cooling, it was sieved to obtain carbon-coated lithium lanthanum zirconium gallium oxygen-coated lithium titanium aluminum phosphate powder. In addition, the coating amount of lithium lanthanum zirconium gallium oxygen was 3%.
[0066] Example 2
[0067] The difference from Example 1 is that 500.0g of battery-grade La(NO3)3·6H2O, 261.5g of Zr(NO3)4, 19.8g of Ga(NO3)3, and 178.0g of CH3COOLi are dissolved in 1800mL of deionized water, and then 300mL of 0.5mol / L nitric acid solution is added to form solution A, 54.0 citric acid is dissolved in 50mL of deionized water, and then solution B is slowly added to solution A, and the mixed solution is transferred to a glass reactor, and stirred in the glass reactor at a speed of 30r / min for 2h to form a mixed solution, and then ammonia water is added to adjust the pH to about 7.5, and stirring is continued for 1h to obtain a carbon-coated amorphous lithium lanthanum zirconium gallium oxygen colorless and transparent sol. The preparation of titanium phosphate is omitted here, and the rest is the same as Example 1.
[0068] Example 3
[0069] The difference from Example 2 is that in step S1, 500.0g of battery-grade La(OH)3, 406.0g of ZrO(NO3)2, 22.5g of Ga(NO3)3, and 443.8g of LiNO3 are dissolved in 2600mL of deionized water, and then 250mL of 0.5mol / L nitric acid solution is added to form solution A, 109.0g of citric acid is dissolved in 50mL of deionized water, and then solution B is slowly added to solution A, and the mixed solution is transferred to a glass reactor, and stirred in the glass reactor at a speed of 30r / min for 3h to form a mixed solution, and then ammonia water is added to adjust the pH to about 7.0, and stirring is continued for 2h to obtain a carbon-coated amorphous lithium lanthanum zirconium gallium oxygen colorless and transparent sol. The rest is the same as Example 2.
[0070] Example 4
[0071] The difference from Example 1 is that in step (2), the grinding particle size is controlled at D50=0.2-0.3 μm, the sintering temperature is 900°C and maintained for 10 hours, the air flow crushing particle size is controlled at D50=2-3 μm, and the rest is the same as Example 1.
[0072] Example 5
[0073] The difference from Example 1 is that in step (2), the grinding particle size is controlled at D50=0.6-0.8μm, the sintering temperature is 800℃ and kept for 12h, the air flow crushing particle size is controlled at D50=1-2μm, and the rest is the same as Example 1.
[0074] Example 6
[0075] The difference from Example 1 is that the temperature of solid phase sintering in step (3) is 850° C. and the temperature is kept for 10 hours. The rest is the same as Example 1.
[0076] Example 7
[0077] The difference from Example 1 is that in step (3), 15 g of colorless and transparent sol of carbon-coated lithium lanthanum zirconium gallium oxide is taken, and the coating amount is 1%. The rest is the same as Example 1.
[0078] Comparative Example 1
[0079] The difference from Example 1 is that the titanium phosphate material is not coated, that is, step (3) is not performed.
[0080] Comparative Example 2
[0081] The difference from Example 1 is that in step (1), the lithium lanthanum zirconium gallium oxide material is not carbon-coated, the air sintering temperature is 750° C., and the temperature is kept for 8 hours. The rest is the same as Example 1.
[0082] Comparative Example 3
[0083] The difference from Example 1 is that in step (1), 48.0 g of glucose is added to coat lithium lanthanum zirconium gallium oxide, and the rest is the same as Example 1.
[0084] Comparative Example 4
[0085] The difference from Example 1 is that the temperature of the solid phase sintering in step (3) is 600° C. and maintained for 12 h. The rest is the same as Example 1.
[0086] Comparative Example 5
[0087] The difference from Example 1 is that in step (3), 75 g of colorless and transparent sol of carbon-coated lithium lanthanum zirconium gallium oxide is taken, and the coating amount is 5%. The rest is the same as Example 1.
[0088] The powders obtained in Examples 1 to 6 and Comparative Examples 1 to 5 were tested using a solid electrolyte test system SEMS1100 in combination with a Donghua electrochemical workstation DH7001, using a 20-30 MPa pressurization mode and maintaining the pressure for 180 min. The test structure is shown in Table 1.
[0089] Table 1 Test performance of carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte obtained in Examples 1 to 6 and Comparative Examples 1 to 4
[0090]
[0091]
[0092] As can be seen from Table 1, Examples 1 to 3 illustrate that after doping lithium lanthanum zirconium gallium oxygen, due to the introduction of new elements or new phases at the interface to change the interface structure, the ion migration barrier is reduced and the interface ion mobility is increased, thereby improving the ionic conductivity of lithium lanthanum zirconium oxygen, and then the ionic conductivity of titanium phosphate is further improved by coating. The doping amount has a great influence on its conductivity. Too much or too little doping will reduce the ionic conductivity of lithium lanthanum zirconium oxygen, thereby affecting the conductivity of titanium phosphate. Examples 1, 4, and 5 illustrate that the grinding particle size of titanium phosphate has a certain influence on the overall ionic conductivity. The lower the grinding particle size, the more serious the agglomeration phenomenon, and the ionic conductivity will decrease to a certain extent. The grinding particle size increases, the lithium ion migration rate slows down, and the impedance is too large, thereby affecting the ionic conductivity of titanium phosphate. Examples 1, 6 and Comparative Example 4 illustrate that the solid-phase sintering temperature is too low, resulting in low crystallinity of lithium lanthanum zirconium gallium oxygen, poor coating effect, and the sintering temperature is too high, the secondary particles increase, and the ionic conductivity decreases. Example 1 and Comparative Example 1 show that the ionic conductivity of titanium phosphate is low (<10 -3 Example 1 and Comparative Examples 2 and 3 show that when no carbon coating is performed or the coating amount is small, the ionic conductivity is low. Lithium lanthanum zirconium gallium oxide is unstable when sintered in the air and will react with CO2 and H2O in the air to generate Li2CO3 with low ionic conductivity, which will reduce the ionic conductivity of lithium lanthanum zirconium gallium oxide (<10 -4 S / cm), thereby affecting the overall ionic conductivity of the phosphate. Examples 1, 7 and Comparative Example 5 show that the lower the lithium lanthanum zirconium gallium oxygen coating content, the less obvious the improvement in ionic conductivity. If the coating content is too high, the ionic conductivity will decrease to a certain extent.
[0093] Figure 1 This is the XRD diagram of the titanium phosphate solid electrolyte sample in Example 1. The prepared titanium phosphate solid electrolyte corresponds to the standard PDF card, no other impurity peaks appear, and the crystallinity is high, indicating that a relatively pure NASICON-type titanium phosphate solid electrolyte can be prepared at this temperature.
[0094] Figure 2This is the XRD pattern of the carbon-coated lithium lanthanum zirconium gallium oxide-coated titanium phosphate solid electrolyte sample after coating in Example 1. The tested XRD corresponds to the standard PDF card of lithium lanthanum zirconium gallium oxide, indicating that the coating effect is good. In addition, doping with gallium does not change the crystal structure, and a stable cubic phase of lithium lanthanum zirconium gallium oxide is generated.
[0095] It can be seen from the above embodiments that the present invention provides a carbon-coated lithium lanthanum zirconium gallium oxide-coated titanium phosphate solid electrolyte and a preparation method thereof. When the titanium phosphate solid electrolyte is matched with a metallic lithium negative electrode, the high-priced Ti 4+ It will be reduced by metallic lithium to form an interfacial intermediate phase with mixed ion and electron conductivity, which will affect the interface stability. Since lithium lanthanum zirconium gallium oxide has high compatibility with lithium negative electrode, the use of lithium lanthanum zirconium gallium oxide coating can avoid direct contact between titanium phosphate solid electrolyte and lithium metal, thereby improving the interface stability and reducing the interface contact resistance. In addition, the ionic conductivity of titanium phosphate is slightly lower at room temperature (10 -4 S / cm), while the ionic conductivity of lithium lanthanum zirconium gallium oxide at room temperature (10 -3 S / cm), coating lithium lanthanum zirconium gallium oxide on the surface of titanium phosphate can further improve ionic conductivity, and applying it to solid-state batteries is beneficial to improving battery rate performance and cycle performance. The present invention first prepares carbon-coated amorphous lithium lanthanum zirconium gallium oxide, and then coats it on the surface of titanium phosphate by sol-gel method, which can effectively solve the problem of low ionic conductivity of titanium phosphate at room temperature, and can also solve the problem of large resistance caused by titanium phosphate interface problems, further broadening the practical application of titanium phosphate in solid electrolytes.
[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte, characterized in that: The following steps are involved: (1) dissolving a first lithium source, a lanthanum source, a zirconium source and a gallium source in water and then adding a nitric acid solution to obtain a solution A, dissolving a carbon source in water to obtain a solution B; adding the solution B to the solution A to adjust the pH to obtain a colorless transparent sol; (2) dissolving the second lithium source, phosphorus source, titanium source, aluminum source and the first dispersant in water for nano-processing to obtain a titanium phosphate solid electrolyte precursor slurry, and sequentially spray drying, solid phase sintering and crushing the obtained slurry to obtain a titanium phosphate solid electrolyte powder; (3) dispersing titanium phosphate solid electrolyte powder and a second dispersant in water to obtain an electrolyte slurry, mixing a colorless transparent sol into the electrolyte slurry and sequentially performing shear dispersion, aging, a second spray drying and a second solid phase sintering to obtain a carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte.
2. The preparation method according to claim 1, characterized in that: The first lithium source and the second lithium source independently include one or more of lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, lithium oxalate, lithium dihydrogen phosphate, lithium chloride and lithium sulfate; the lanthanum source includes one or more of lanthanum oxide, lanthanum nitrate, lanthanum carbonate and lanthanum hydroxide; the zirconium source includes one or more of zirconium oxide, zirconium nitrate, zirconyl nitrate and zirconium n-propoxide; the gallium source includes one or more of gallium oxide, gallium nitrate and gallium chloride; The molar ratio of the first lithium source, lanthanum source, zirconium source and gallium source is 6-6.8:3-4:2-3:0.1-0.
3.
3. The preparation method according to claim 1 or 2, characterized in that: The concentration of the nitric acid solution is 0.4-0.6 mol / L, and the amount of the nitric acid solution is 100-500 mL; In the step (1), the pH is adjusted to 4-10.
4. The preparation method according to claim 1 or 2, characterized in that: The carbon source comprises one or more of glucose, citric acid, sucrose, asphalt, polyethylene glycol and polyvinyl alcohol, and the added amount of the carbon source is 5-10% of the total weight of the first lithium source, lanthanum source, zirconium source and gallium source; the concentration of the carbon source in the solution B is 0.8-2.5 g / mL; in the solution A, the concentration of the lanthanum source is 0.18-0.4 g / mL.
5. The preparation method according to claim 4, characterized in that: The phosphorus source comprises one or more of phosphoric acid, ammonium monohydrogen phosphate, ammonium dihydrogen phosphate and diammonium hydrogen phosphate; the titanium source comprises one or more of anatase titanium dioxide, rutile titanium dioxide, tetrabutyl titanate, titanium tetrachloride and titanium isopropoxide; the aluminum source comprises one or more of aluminum oxide, aluminum hydroxide, pseudo-boehmite and aluminum nitrate; the first dispersant and the second dispersant independently comprise one or more of polyvinyl alcohol, polypropylene pyrrolidone, sodium carboxymethyl cellulose, polyvinyl pyrrolidone and polyethylene glycol; The molar ratio of the lithium source, the aluminum source, the titanium source and the phosphorus source is 1.1-1.5:0.1-0.5:1.5-1.9:3, wherein the lithium source comprises a first lithium source and a second lithium source; The amount of the first dispersant used is 2-10% of the total weight of the titanium source, the phosphorus source, the aluminum source and the second lithium source.
6. The preparation method according to claim 1, 2 or 4, characterized in that: The nano-treatment is carried out under sand milling, the sand milling speed is 1000-1500rpm, and the sand milling time is 1-3h; the particle size of the titanium phosphate solid electrolyte precursor slurry is 0.2-0.8μm, and the solid content of the titanium phosphate solid electrolyte precursor slurry is 20-50%.
7. The preparation method according to claim 6, characterized in that: In the step (2), the inlet temperature of the spray drying is 200-240°C, the outlet temperature is 90-130°C, and the spray particle size is 10-30 μm; the temperature of the solid phase sintering is 600-1000°C, and the solid phase sintering time is 8-14 hours; the crushing method is mechanical crushing or air flow crushing, and the particle size of the titanium phosphate solid electrolyte powder after crushing is 1-6 μm.
8. The preparation method according to claim 1 or 7, characterized in that: The dosage of the second dispersant is 1-6% of the weight of the titanium phosphate solid electrolyte powder, and the dosage ratio of the second dispersant to water is 20-60 g: 2000 mL; The amount of the colorless transparent sol is 1-10% of the weight of the titanium phosphate solid electrolyte powder.
9. The preparation method according to claim 8, characterized in that: The shear dispersion time is 1 to 5 hours, the shear dispersion frequency is 10 to 30 Hz, and the aging time is 1 to 6 hours; The inlet temperature of the second spray drying is 200-240°C, the outlet temperature is 90-130°C, and the particle size of the spray is 4-10 μm; The second solid-phase sintering is performed in an inert gas, which includes argon or nitrogen; the temperature of the second solid-phase sintering is 500-900° C., and the time of the second solid-phase sintering is 6-13 hours.
10. The carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The chemical formula of lithium lanthanum zirconium gallium oxygen in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 7-3X La3Zr2Ga X O 12 , where 0.1≤X≤0.3; The chemical formula of the titanium phosphate solid electrolyte in the carbon-coated lithium lanthanum zirconium gallium oxygen-coated titanium phosphate solid electrolyte is Li 1+Y Al Y Ti 2-Y (PO4)3, where 0.1≤Y≤0.5; The coating amount of the lithium lanthanum zirconium gallium oxygen coated titanium phosphate solid electrolyte is 1-10%.
Citation Information
Cited By
Gradient-coated graphite composite negative electrode material, preparation method thereof and lithium ion battery