Top plate of cooking stove, glass ceramic substrate processing method and stove comprising top plate

By using chemically enhanced glass ceramic substrate on the top plate of the induction heating stove, an uneven structure of 0.1μm to 1.0μm is formed, which solves the scratch problem at high temperature, improves scratch resistance and hardness, and reduces the friction coefficient and visibility. , achieves beautiful and durable effects.

CN118900827APending Publication Date: 2024-11-05SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380021499.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-08
Filing Date
2023-04-13
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

The roof of the induction heating stove is prone to scratches at high temperatures, causing contaminants to enter the scratches, affecting the cleaning and aesthetics, and existing materials are difficult to provide sufficient scratch resistance and high strength.

Method used

Using a chemically enhanced glass ceramic substrate, KNO3 and NaNO3 are used to form an uneven structure of 0.1 μm to 1.0 μm on the surface and include elements such as Li2O, Al2O3, SiO2, V, Mg, P, Fe, Ti and Zr. Ion exchange, improve surface hardness and scratch resistance.

Benefits of technology

The friction coefficient is significantly reduced, the surface hardness and scratch resistance are improved, and the uneven structure makes the substrate translucent and reduces visibility, providing an aesthetic appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118900827A_ABST
    Figure CN118900827A_ABST
Patent Text Reader

Abstract

The cooking hob top plate of the present invention may include a glass ceramic substrate having an average surface roughness (Ra) of 0.1 [mu] m to 1.0 [mu] m and including chemically enhanced uneven portions. A cooking container heated by the cooking hob may be placed on the top plate. The glass ceramic substrate manufacturing method may include forming a top plate having an uneven portion, and chemically enhancing the top plate having the uneven portion. The induction heating hob may include a top plate of the cooking hob and a plurality of induction heating coils for heating a cooking vessel placed on the top plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a cooking range top plate having high strength and low glossiness, having an uneven structure having a preset surface roughness on a surface, a method for manufacturing the cooking range top plate, and a range including the cooking range top plate. Background Art

[0002] The induction heating cooker is a cooking cooker for heating and cooking food by using the principle of induction heating. The induction heating cooker includes a cooking cooker top plate on which a cooking container is placed and an induction coil configured to generate a magnetic field by current applied thereto.

[0003] The magnetic field generated by the current supplied to the coil induces a secondary current, and thus generates Joule heat through the resistance of the cooking container. Therefore, the cooking container is heated by the high-frequency current, and food contained in the cooking container is cooked.

[0004] Although the thermal efficiency (for heating a cooking container) of a gas cooker is about 45%, an induction heating cooker having a high thermal efficiency of about 90% can reduce cooking time.

[0005] Furthermore, since the cooking container itself is used as a heat source in the induction heating cooker, the induction heating cooker does not generate harmful gas, is safe without fire risk, and is easy to clean due to a non-stick property, compared to a gas cooker or a kerosene cooker that uses heat obtained by burning fossil fuels to heat the cooking container, and thus a recent market for the induction heating cooker is expanding.

[0006] Meanwhile, although the top plate of the induction heating cooker is formed of tempered glass such as glass ceramic to prevent the top plate from being broken due to frequent friction with the cooking container, scratches are formed when a load is applied thereto at high temperature. Once scratches are formed, contaminants enter the scratches, resulting in problems of deterioration of cleanability and aesthetics. Therefore, it is necessary to develop a material for forming the top plate with improved scratch resistance and high strength. Summary of the invention

[0007]

Technical issues

[0008] Provided are a high-strength and low-gloss glass-ceramic substrate having improved scratch resistance and increased surface hardness and reduced friction coefficient by forming an uneven structure satisfying a preset surface roughness on a surface of glass-ceramic and chemically strengthening the surface, and a method for manufacturing the glass-ceramic substrate. The glass-ceramic substrate can be applied to an external cooking range top plate requiring heat resistance or an external material requiring scratch resistance.

[0009] However, the technical problems to be solved by the present disclosure are not limited to the above-mentioned problems, and any other technical problems not mentioned herein will be clearly understood by those skilled in the art to which the present disclosure belongs from the following description.

[0010]

Technical solution

[0011] According to an aspect of the present disclosure, a cooking hob includes a glass ceramic substrate having a chemically enhanced top surface having an uneven structure having an average surface roughness (Ra) of 0.1 μm to 1.0 μm.

[0012] In addition, the glass ceramic substrate may include Li 2 O、Al 2 O 3 and SiO 2 As a basic component, the glass ceramic substrate may include at least one crystal phase selected from β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. The glass ceramic substrate may further include at least one element selected from V, Mg, P, Fe, Ti and Zr.

[0013] In addition, the surface of the glass ceramic substrate can be formed by contacting with a KNO 3 and NaNO 3 At least one enhancing salt in the sample is chemically enhanced by exchanging ions.

[0014] In addition, the glass ceramic substrate may have a Vickers hardness of 950 Hv to 1200 Hv. The glass ceramic substrate may have a friction coefficient of 0.42 to 0.71.

[0015] In addition, the cooking stove top plate further comprises a printing layer below the glass ceramic substrate. The printing layer may comprise a background printing layer and a shielding printing layer below the background printing layer.

[0016] According to another aspect of the present disclosure, a method for processing a glass ceramic substrate having a top surface may be provided. The method includes: forming the top surface to have an uneven structure having an average surface roughness (Ra) of 0.1 μm to 1.0 μm; and chemically strengthening the top surface having the uneven structure.

[0017] In addition, the glass ceramic substrate may include Li 2 O、Al 2 O 3 and SiO 2The glass ceramic substrate may include at least one crystal phase selected from β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. The glass ceramic substrate may further include at least one element selected from V, Mg, P, Fe, Ti, Cr and Zr.

[0018] In addition, the forming of the top surface to have the uneven structure may be performed by chemical etching, sand blasting, or a combination thereof.

[0019] In addition, the chemical enhancement is achieved by reacting with a KNO 3 and NaNO 3 The chemical enhancement can be carried out by ion exchange of at least one enhancing salt in the reaction mixture. The chemical enhancement can be carried out by using KNO with a concentration of 90 wt % to 100 wt %. 3 The solution was allowed to stand as an enhancing salt for 10 to 60 minutes.

[0020] According to another aspect of the present disclosure, an induction heating cooker may be provided. The induction heating cooker includes: a cooking cooker top plate on which a cooking container may be placed, the cooking cooker top plate including a glass ceramic substrate having a chemically enhanced top surface, the chemically enhanced top surface having an uneven structure with an average surface roughness (Ra) of 0.1 μm to 1.0 μm; and a plurality of induction heating coils below the cooking cooker top plate and configured to generate a magnetic field with the cooking container placed on the top surface to heat the cooking container.

[0021] In addition, the glass ceramic substrate may include Li 2 O、Al 2 O 3 and SiO 2 The glass ceramic substrate may include at least one crystal phase selected from the group consisting of a β-quartz crystal phase, a β-spodumene crystal phase, and a β-eucryptite crystal phase.

[0022] In addition, the glass ceramic substrate may have a Vickers hardness of 950 Hv to 1200 Hv and a friction coefficient of 0.42 to 0.71.

[0023]

Beneficial Effects

[0024] According to an embodiment of the present disclosure, a crystallized cooking stove top plate with high hardness and low glossiness is provided (specifically, provided by forming an uneven structure with a surface roughness in a preset range on the surface of a glass ceramic substrate used in an environment requiring heat resistance such as an induction stove), which can reduce the friction coefficient and the occurrence of scratches caused by friction of kitchen utensils.

[0025] Furthermore, the uneven surface makes the substrate translucent to reduce visibility of the substrate, so that an internal structure of the cooking hob, such as an induction heating coil, is not visible from the outside, thereby providing an aesthetically pleasing appearance.

[0026] Furthermore, by chemically reinforcing the surface of the uneven structure of the ceramic substrate, a cooking stove top plate having further improved surface strength and hardness may be provided.

[0027] Furthermore, due to the unique surface texture having the uneven structure on the surface, the glass-ceramic substrate can be applied to feature designs of exterior materials such as mobile rear cover glasses, refrigerators, etc., and top plates of cooking ranges such as induction ranges.

[0028] However, effects obtainable by the present disclosure are not limited to the above-mentioned effects, and any other effects not mentioned herein will be clearly understood from the following description by those skilled in the art to which the present disclosure pertains. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 is a cross-sectional view illustrating a structure of a top plate of a cooking range according to an embodiment of the present disclosure.

[0030] Figure 2 is a cross-sectional view illustrating an exploded view of a structure and an uneven structure of a top plate of a cooking range according to an embodiment of the present disclosure.

[0031] Figure 3 is an illustration of the uneven structure of the top plate of the cooking stove according to an embodiment of the present disclosure ( Figure 2 Decomposition diagram of chemical enhancement in area A).

[0032] Figure 4 is a view illustrating the appearance of an induction heating cooker according to an embodiment of the present disclosure.

[0033] Figure 5 is a view illustrating a state in which a main body of the induction heating cooker is separated from a top plate of the cooking cooker.

[0034] Figure 6 is an exploded perspective view illustrating the structure of a cooking cooktop top plate and an induction heating coil of an induction heating cooktop according to an embodiment of the present disclosure.

[0035] Figure 7a is a photograph of an induction range including a conventional cooking range top plate on which an uneven structure is not formed.

[0036] Figure 7b is a photograph of an induction range including a glass ceramic substrate on which an uneven structure according to an embodiment of the present disclosure is formed.

[0037] Figure 8a is a graph illustrating a friction coefficient of a conventional glass ceramic substrate on which an uneven structure is not formed under a measurement load of 5N.

[0038] Figure 8b is a graph illustrating a friction coefficient of a glass ceramic substrate on which an uneven structure according to an embodiment of the present disclosure is formed under a measured load of 5N.

[0039] Figure 9a is a graph illustrating a friction coefficient of a conventional glass ceramic substrate on which an uneven structure is not formed under a measurement load of 2N.

[0040] Figure 9b is a graph illustrating a friction coefficient of a glass ceramic substrate on which an uneven structure according to an embodiment of the present disclosure is formed under a measured load of 2N.

[0041] Fig.10 This is a graph illustrating the surface hardness depending on the conditions of the chemically strengthened glass-ceramic substrate.

[0042] Fig.11 : is a graph showing an example of the friction coefficient related to the surface roughness of the glass ceramic substrate.

[0043] Fig.12 This is a graph illustrating the surface hardness in relation to the chemical strengthening time. DETAILED DESCRIPTION

[0044] Hereinafter, the embodiments of the present disclosure will be described in detail. However, the present disclosure can be implemented in many different forms and should not be interpreted as being limited to the exemplary embodiments set forth herein; on the contrary, these embodiments are provided to make the present disclosure comprehensive and complete and to fully convey the concepts of the present disclosure to those of ordinary skill in the art.

[0045] Furthermore, the terms used in the present disclosure are for describing specific embodiments only. Expressions used in the singular include expressions in the plural unless they have obviously different meanings in the context.

[0046] In addition, it should be understood that terms such as "including", "having", etc. used in this document are intended to indicate the existence of the features, operations, functions, components, or a combination thereof disclosed in the specification, and are not intended to exclude the possibility that one or more other features, operations, functions, components, or a combination thereof may exist or may be added.

[0047] Meanwhile, unless otherwise defined, all terms used herein have the same meanings as those generally understood by those of ordinary skill in the art to which the present disclosure belongs. Unless clearly defined herein, these terms should not be interpreted in an idealized or overly formal sense. As used herein, the singular form is intended to also include the plural form, unless the context clearly indicates otherwise.

[0048] The terms "approximately", "substantially" and the like used throughout the specification mean that when natural manufacturing and material tolerances are proposed, such tolerances correspond to the value or are similar to the value, and such values ​​are for the purpose of clearly understanding the contents of the present disclosure or preventing unintentional infringers from illegally using the contents of the present disclosure.

[0049] In addition, the terms “first”, “second”, etc. are used to distinguish one component from other components, and thus, these components are not limited by these terms.

[0050] In addition, the terms “unit,” “device,” “block,” “member,” and “module” refer to a unit for processing at least one function or operation.

[0051] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. In the accompanying drawings, the same reference numerals will be assigned to the same elements or components having substantially the same functions.

[0052] Figure 1 and Figure 2 is a cross-sectional view illustrating a structure of a top plate of a cooking range according to an embodiment of the present disclosure.

[0053] In the following, reference will be made to Figure 1 and Figure 2 The processing method of the cooking range top plate and the glass ceramic substrate is described in detail.

[0054] refer to Figure 1 and Figure 2 , a cooking range top plate (20) includes a glass ceramic substrate (24) having a chemically enhanced uneven structure (24a) on a top surface.

[0055] According to an embodiment of the present disclosure, comprising Li 2 O、Al 2 O 3 and SiO 2Crystallized glass based on lithium aluminum silicon as a basic composition can be used in the glass ceramic substrate (24) to obtain heat resistance. In addition, according to the color to be achieved, the glass ceramic substrate (24) may further contain at least one element selected from V, Mg, P, Fe, Ti, Cr and Zr, but is not limited thereto. More specifically, the color to be achieved can be changed according to the content of the elements contained in the achieved glass ceramic substrate (24), and the V content can be increased to achieve black, and the content of P, Zr, etc. can be increased to achieve white.

[0056] Furthermore, the glass ceramic substrate may include at least one crystal phase selected from the group consisting of a β-quartz crystal phase, a β-spodumene crystal phase, and a β-eucryptite crystal phase.

[0057] The crystal phase of the glass ceramic substrate (24) can change according to the crystallization temperature, and the color of the glass ceramic substrate (24) can change according to the crystal phase. For example, the glass ceramic substrate (24) can include at least one crystal phase selected from β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. More specifically, the glass ceramic including the β-quartz crystal phase can achieve a transparent color, and the glass ceramic including the β-spodumene crystal phase can achieve a white color.

[0058] refer to Figure 1 and Figure 2 An uneven structure (24a) is formed on the top surface of the glass ceramic substrate (24) to improve scratch resistance and reduce visibility and friction coefficient. Generally speaking, it is known that the formation of an uneven surface increases the friction coefficient, but it has been found that the friction coefficient can be reduced by adjusting the surface roughness of the uneven structure within a predetermined range in the present disclosure.

[0059] According to the embodiment, since the glass ceramic substrate (24) has an average surface roughness (Ra) in the range of 0.1 μm to 1.0 μm, preferably 0.3 μm to 0.9 μm, due to the uneven structure (24a) formed on the surface, the friction coefficient is reduced and scratches and visibility can be reduced. In particular, in the case where the surface roughness exceeds the upper limit, a higher friction coefficient than before the uneven structure is formed is obtained, and thus the surface roughness can be 1.0 μm or less. Specifically, before the uneven structure is formed, the friction coefficient of the surface of the glass ceramic substrate is about 0.75 μm, but by forming the uneven structure on the surface of the glass ceramic substrate, the friction coefficient can be reduced to 0.42 μm to 0.71 μm, and thus soft toughness can be obtained. In addition, the visibility of the cooking stove top plate (20) can be reduced and become translucent with low gloss to prevent the internal structure of the stove from being visible in an area that is difficult to be blocked by the printed layer to be described below.

[0060] Figure 7aA cooking hob top plate formed of a glass ceramic substrate having no uneven structure formed thereon is shown. Figure 7b A cooking hob formed of a glass ceramic substrate on which an uneven structure is formed is shown. Figure 7a As shown in FIG. 1 , the glass ceramic substrate on which the uneven structure is not formed has high gloss and high visibility, while Figure 7b , the glass ceramic substrate on which the uneven structure is formed has low gloss and low visibility.

[0061] According to the embodiment, the uneven structure (24a) can be formed by chemical etching, sandblasting or any combination thereof. Chemical etching can be performed by using an acidic solution containing fluorine as an etchant, and for example, hydrofluoric acid (HF), fluorosilicic acid (F 6 H 2 Si) can be used as an etchant, but is not limited thereto. Particles with high hardness (such as boron carbide, industrial diamond, Al 2 O 3 , silicon carbide, glass beads, zirconium oxide and stainless steel shot) as sandblasting surface treatment media for sandblasting. In addition, if necessary, chemical etching and sandblasting can be combined, for example, chemical etching can be further performed after sandblasting, but the present disclosure is not limited thereto.

[0062] The surface of the glass ceramic substrate (24) on which an uneven structure is formed to improve surface hardness and strength is chemically strengthened. 3 and NaNO 3 The surface of the glass ceramic substrate (24) is chemically enhanced by at least one of the enhancing salts. + ) and the cation of the enhancing salt (K + and / or Na + ) and is chemically enhanced by ion exchange between them. Figure 3 It is an example Figure 2 A magnified view of area A showing the use of KNO 3 In the case of chemically enhancing the uneven structure on the surface of the glass ceramic substrate (24), the ion exchange state between the glass ceramic substrate (24) and the enhancing salt.

[0063] According to an embodiment, 90 wt % to 100 wt % of KNO may be used. 3As strengthening salt, chemical strengthening treatment is carried out for 10 minutes or more than 10 minutes, preferably 10 minutes to 60 minutes in terms of efficiency and productivity of the process. In the present disclosure, even when chemical strengthening is applied for a short time, high strength and high surface hardness can be obtained. As is well known, because the migration and displacement of ions are interrupted by internal crystallinity, the chemical strengthening process should be carried out on glass ceramics for about 8 hours to about 24 hours. However, because there is no significant difference in surface hardness between carrying out long-term chemical strengthening for more than 8 hours and carrying out short-time chemical strengthening for less than 1 hour, so in terms of efficiency and productivity of the process, it is desirable to carry out short-time chemical strengthening.

[0064] Since friction is continuously generated on the top surface of the cooking stove top plate (24), it is necessary to increase the surface hardness and strength, especially to reduce the impact strength and scratches of the surface. Specifically, the glass ceramic substrate (24) may have a Vickers hardness of 950 Hv or more, preferably 950 Hv to 1200 Hv, and more preferably 1000 Hv to 1200 Hv.

[0065] At the same time, reference Figure 2 , a printed layer (25) may be further disposed below the glass ceramic substrate (24) to achieve a desired color or to prevent the internal structure of the induction cooker from being visible from the outside.

[0066] The printing layer (25) may include a polyester-based polymer material as a base material and may further contain titanium oxide (TiO 2 ), silicon oxide (SiO 2 ), glass beads, Si, Cr, Mg, etc. A large amount of inorganic materials and metal pigments can be added to obtain the heat resistance of the ink. In addition, cyclohexane, trimethylbenzene, methyl methacrylate, etc. can be used as solvents and hardeners, but are not limited thereto.

[0067] In an embodiment, the printed layer (25) may include a background printed layer (25-1), for example, the background printed layer (25-1) may be provided under the translucent glass ceramic substrate (24) to distinguish the design by achieving a color visible from the outside or to display a guide mark to guide the user to the location of the heating cooking container.

[0068] Meanwhile, in another embodiment, a guide mark for guiding a user to a position for heating a cooking container can be formed separately on an uneven structure (24a) of a glass ceramic substrate (24) by glass printing. Glass printing is performed by applying a design with glass printing ink to the glass ceramic and heating the design at a preset temperature so that the ink penetrates into the glass ceramic. Any material known as an ink for glass printing can be used for glass printing without limitation.

[0069] In an embodiment, the printed layer (25) may include a shielding printed layer (25-2). For example, the shielding printed layer (25-2) may be disposed below the background printed layer (25-1) to prevent the internal structure of the cooker from being visible to the user.

[0070] Meanwhile, although the surface hardness and scratch resistance can be improved by forming the uneven structure (24a) on the surface of the glass ceramic substrate (24), the cleanability and antifouling property may be slightly deteriorated. Therefore, an antifouling layer (not shown) may be further formed on the glass ceramic substrate (24) on which the uneven structure (24a) is formed to improve the cleanability and antifouling property of the cooking stove top plate (20). The antifouling layer may include, for example, zirconium oxide (ZrO 2 ) and titanium oxide (TiO 2 ) to improve surface slip and heat resistance, but the embodiment is not limited thereto. In addition, the antifouling layer may include an anti-fingerprint (AF) coating. For example, the anti-fingerprint coating may have a structure in which perfluoropolyether (PFPE) is bonded to a silane matrix used as a coupling agent, and may also include zirconium oxide (ZrO 2 ) and titanium oxide (TiO 2 ) is an inorganic material used to improve heat resistance.

[0071] In an embodiment, the above-mentioned cooking stove top plate may be used as a top plate of an induction heating stove.

[0072] Figure 4 is a view illustrating the appearance of an induction heating cooker according to an embodiment of the present disclosure.

[0073] refer to Figure 4 The induction heating cooker (1) comprises a main body (10), which constitutes the appearance of the induction heating cooker (1) and is used to install various components of the induction heating cooker (1). The main body (10) can be provided in a box shape with an open top surface.

[0074] A cooking stove top plate (20) having a flat plate shape on which a cooking container is to be placed may be provided on the top surface of the body (10).

[0075] Conventionally, heat-resistant glass having a lower thermal expansion coefficient than ordinary glass has been used as a material for the top plate of an induction heating cooker (ie, the cooking cooker top plate (20)). However, due to the low degree of freedom of the external pattern, the design of the pattern of the transparent heat-resistant glass is limited.

[0076] Meanwhile, the material applied to the top plate of the induction heating cooker should have a low thermal expansion coefficient to prevent thermal shock. In the present disclosure, glass ceramics is used as a substrate to maintain heat resistance required in the induction heating cooker.

[0077] Hereinafter, the glass ceramic substrate (24) and the printed layer (25) constituting the cooking stove top plate (20) will be described.

[0078] Figure 6 : is an exploded perspective view illustrating the structure of a cooking cooktop and an induction heating coil of an induction heating cooktop according to an embodiment of the present disclosure. Figure 6 , the printed layer (25) is bonded to the bottom surface of the glass ceramic substrate (24).

[0079] The glass ceramic substrate (24) may have a flat plate shape to allow a cooking container to be placed thereon and may be formed of a material having a low thermal expansion coefficient. For example, the glass ceramic substrate (24) may be formed of a material that satisfies the heat resistance conditions required as a material for a cooking stove top plate of an induction heating stove.

[0080] The glass ceramic substrate (24) includes a chemically enhanced uneven structure (24a) on the top surface, and the uneven structure (24a) has an average surface roughness (Ra) of 0.1 μm to 1.0 μm. The description of the glass ceramic substrate (24) is the same as the above description of the cooking stove top plate (20), and therefore will not be repeated.

[0081] At the same time, reference Figure 2 , the printed layer (25) may include a background printed layer (25-1) below the translucent glass ceramic substrate (24) to display a guide mark to distinguish the design by realizing a color visible from the outside, or to guide the user to the location of heating the cooking container. In addition, a shielding printed layer (25-2) may be further provided below the background printed layer (25-1) to prevent the internal structure of the cooker from being visible to the user. The description of the printed layer (25) is the same as the above description of the top plate of the cooking cooker and will not be repeated.

[0082] According to another embodiment, guide marks (21-1, 21-2, 22) for guiding a user to a position for heating a cooking container may be additionally formed on a glass ceramic substrate (24) provided with an uneven structure (24a) on its top surface. In this regard, the guide marks (21-1, 21-2, 22) may be formed by glass printing, which is performed by applying glass printing ink in a pattern to the surface of the uneven structure of the glass ceramic substrate (24), and heating the pattern at a preset temperature so that the ink penetrates into the glass ceramic. In addition, any material known as an ink for glass printing may be used for glass printing without limitation.

[0083] According to an embodiment, an antifouling layer (not shown) may be further formed on the glass ceramic substrate (24). For example, the antifouling layer may be formed on a glass printed glass ceramic substrate (24). In the case where the antifouling layer is formed on the glass ceramic substrate (24) on which the uneven structure (24a) is formed, the cleanability and antifouling properties of the cooking stove top plate (20) may be improved. For example, the antifouling layer may include a zirconium oxide (ZrO 2 ) and titanium oxide (TiO 2 ) to improve surface slip and heat resistance, but is not limited thereto. In addition, the antifouling layer may include an anti-fingerprint (AF) coating. For example, the anti-fingerprint coating may have a structure in which perfluoropolyether is bonded to a silane matrix used as a coupling agent, and may also include a zirconium oxide (ZrO 2 ) and titanium oxide (TiO 2 ) to improve heat resistance.

[0084] Hereinafter, three guide marks will be described, but the number of guide marks is not limited thereto, and two or more guide marks may be included without limitation.

[0085] In addition, a user interface (23) may be provided on a region of the cooking stove top plate (20), the user interface (23) being configured to receive a control command from a user and to display information about the operation of the induction heating stove (1) to the user. However, the position of the user interface (23) is not limited to the cooking stove top plate (20), and the user interface (23) may also be provided at various positions of the main body (10), such as the front surface and / or the side surface.

[0086] Figure 5 is a view illustrating a state in which a main body is separated from a cooking cooktop in the induction heating cooker according to an embodiment of the present disclosure.

[0087] refer to Figure 5 The induction heating cooker (1) comprises a heating layer (30) arranged below a cooking cooker top plate (20) and comprising a plurality of induction heating coils (31-1, 31-2, 31-3; 31) which heat a cooking container placed on the cooking cooker top plate (20) and a main assembly (32) which implements a user interface (23) and accommodates various electronic components.

[0088] A plurality of induction heating coils (31) are heated by electromagnetic induction to heat a cooking container placed on a top plate (20) of a cooking range.

[0089] The induction heating coil (31) includes a coil wound into a substantially circular shape to generate a magnetic field in a vertical direction by a current applied thereto. The induction heating coil (31) is used as a heat source and is disposed below a cooking range top plate (20) to transfer heat to the cooking range top plate (20). A cooking container such as a pot is heated by the heat transferred to the cooking range top plate (20). Although the induction heating coil (31) is described as a heat source in the present disclosure, an induction heater using an induction heating method or a radiation heater using a resistance method may also be used as a heat source instead of the induction heating coil (31).

[0090] In this case, a plurality of induction heating coils (31) may be provided at positions corresponding to the guide marks (21-1, 21-2, 22), respectively.

[0091] Specifically, the plurality of induction heating coils (31) may include a first induction heating coil (31-1), another first induction heating coil (31-2) and a second induction heating coil (31-3).

[0092] although Figure 4 and Figure 5 Two first induction heating coils (31-1, 31-2) and one second induction heating coil (31-3) are exemplified, but the embodiment is not limited thereto. The induction heating cooker (1) may include at least one first induction heating coil (31-1) and at least one second induction heating coil (31-3).

[0093] That is, the number of the first induction heating coils (31-1, 31-2) and the second induction heating coils (31-3) included in the induction heating cooker (1) is not limited, as long as one or more than one of them is used.

[0094] Each of the plurality of induction heating coils (31) can generate a magnetic field and / or an electromagnetic field for heating the cooking container.

[0095] For example, the driving current supplied to the induction heating coil ( 31 ) may induce a magnetic field around the induction heating coil 31 .

[0096] Specifically, once a current (ie, alternating current) that changes magnitude and reverses direction over time is supplied to the induction heating coil (31), a magnetic field whose magnitude and direction change over time can be induced around the induction heating coil (31).

[0097] The magnetic field generated around the induction heating coil (31) can pass through the cooking stove top plate (20) formed of tempered glass and reach the cooking container placed on the cooking stove top plate (20).

[0098] Eddy currents circulating along the magnetic field may be generated in the cooking container by the magnetic field whose magnitude and direction vary with time. The phenomenon of generating eddy currents by the time-varying magnetic field is called electromagnetic induction. The eddy currents may generate resistive heat in the cooking container. Resistive heat is heat generated in a resistor when current flows in the resistor, also known as Joule heat. The cooking container is heated by this resistive heat, and the object to be cooked contained in the cooking container (C) may be heated.

[0099] As described above, each of the plurality of induction heating coils (31) can heat the cooking container (C) by using electromagnetic induction and resistance heat.

[0100] Furthermore, the heating layer (30) may be disposed below the user interface (23) provided at one region of the cooking stove top plate (20), and include a main component (32) configured to implement the user interface (23).

[0101] The main assembly (32) may be a printed board assembly (PBA) which includes a display, a switch element, and an integrated circuit element for realizing a user interface (23) and a printed circuit board (PCB) on which these elements are mounted.

[0102] The position of the main assembly (32) is not limited to Figure 4 , and the main component (32) can be arranged at various positions. For example, in the case where the user interface (23) is installed on the front surface of the main body (10), the main component (32) can be arranged behind the front surface separately from the heating layer (30).

[0103] A PCB assembly (not shown) configured to operate the plurality of induction heating coils (31) may be provided below the plurality of induction heating coils (31). The plurality of PCB assemblies may be provided with a driving circuit configured to supply a driving current to the plurality of induction heating coils (31) and a control circuit configured to control the operation of the plurality of induction heating coils (31).

[0104] As described above, the induction heating cooker (1) may include a cooking cooker top plate (20) having a flat plate shape on which a cooking container is placed, a plurality of induction heating coils (31) for heating the cooking container, and a driving circuit and a control circuit configured to operate the plurality of induction heating coils (31).

[0105] Meanwhile, the above-mentioned induction heating cooker is only an example of a cooker according to the embodiment. That is, the glass ceramic substrate provided with the above-mentioned uneven structure can also be applied to various types of cookers known in the art and the exterior of the above-mentioned induction heating cooker without limitation. Therefore, any cooker including the glass ceramic substrate provided with the above-mentioned uneven structure as an exterior material can be used as an example of the present disclosure.

[0106] According to an embodiment of the present disclosure, a cooker including a glass ceramic substrate as an outer material is provided, wherein the glass ceramic substrate includes a chemically enhanced uneven structure on a top surface, and the uneven structure has an average surface roughness (Ra) of 0.1 μm to 1.0 μm. Due to high surface hardness, the glass ceramic substrate having the above-mentioned uneven structure can be used as an outer material of a mobile rear cover glass or a household appliance (such as a refrigerator), and preferably, is applied to a cooking cooker requiring heat resistance such as an induction cooker and an oven.

[0107] Hereinafter, the present disclosure will be described in more detail with reference to the following examples. However, these examples are for illustrative purposes only, and the present disclosure is not to be construed as being limited to these examples.

[0108] [Example]

[0109] Preparation Example 1: Preparation of a glass ceramic substrate having an uneven structure on the surface

[0110] As the glass ceramic substrate, lithium aluminum silicon having a β-quartz crystal phase was used.

[0111] An uneven structure was formed on the surface of the glass ceramic substrate by sand blasting using boron carbide and industrial diamond, and the average surface roughness (Ra) in this case was 0.66 μm.

[0112] Experimental Example 1-1: Comparison of friction coefficient according to the presence of uneven structure

[0113] In order to determine the effect of the uneven structure on reducing the friction coefficient, the friction coefficient of the glass ceramic substrate before forming the uneven structure and the friction coefficient of the glass ceramic substrate having the uneven structure according to Preparation Example 1 were measured under loads of 5N and 2N, and the results are shown in Tables 1 and Figures 8a to 9b Shown in.

[0114] Table 1

[0115]

[0116] Figure 8a and Figure 8b : is a graph illustrating the friction coefficient under a load of 5N of the glass ceramic substrate before the uneven structure is formed and the glass ceramic substrate after the uneven structure is formed. Figure 9a and Figure 9b : is a graph illustrating the friction coefficient under a load of 2N of the glass ceramic substrate before the uneven structure is formed and the glass ceramic substrate after the uneven structure is formed.

[0117] Refer to Table 1 and Figures 8a to 9bBased on this experiment, it was confirmed that the friction coefficient was reduced by forming an uneven structure having a preset surface roughness on the surface of the glass ceramic substrate. Regarding the real touch, it was also confirmed that the substrate of Preparation Example 1 was softer.

[0118] Experimental Example 2-1: Comparison of scratch resistance according to the presence of uneven structure

[0119] In order to determine the effect of the uneven structure on improving scratch resistance, the glass ceramic substrate was subjected to a scratch test 1 to 10 times under a load of 1 kg before and after forming the uneven structure according to Preparation Example 1, and the results are shown in Table 2 below.

[0120] <Evaluation criteria for scratch resistance>

[0121] NG: Scratches were observed with the naked eye.

[0122] OK: No scratches are observed with the naked eye.

[0123] Table 2

[0124]

[0125] Referring to Table 2, although scratches were visually observed in the glass ceramic substrate before the uneven structure was formed, no scratches were visually observed in the glass ceramic substrate of Preparation Example 1 on which the uneven structure was formed. That is, it was confirmed that the scratch resistance of the glass ceramic substrate of Preparation Example 1 was improved only by forming the uneven structure before the chemical strengthening treatment.

[0126] Preparation Example 2: Chemical Strengthening of Glass Ceramic Substrates

[0127] In order to compare the reinforcing effects of the reinforcing conditions, a glass ceramic substrate on which an uneven structure was not formed was chemically strengthened by methods according to the following reinforcing conditions 1 to 3. Lithium aluminum silicon having a β-quartz crystal phase was used as the glass ceramic substrate.

[0128] 1) Condition 1: The substrate is in a NaNO solution with a weight ratio of 64:36. 3 With KNO 3 Chemical strengthening was carried out in a mixed solution at 400°C for 3 hours (Preparation Example 2-1).

[0129] 2) Condition 2: Substrate in 100wt% KNO 3 Chemical strengthening in solution at 420°C for 20 minutes (Preparation Example 2-2).

[0130] 3) Condition 3: The substrate is in a NaNO solution with a weight ratio of 64:36 3 With KNO 3 The mixed solution was chemically strengthened at 400 °C for 3 h and then in 100 wt% KNO 3Chemical strengthening in solution at 380°C for 20 minutes (Condition 1 + Condition 2: Preparation Example 2-3).

[0131] Experimental Example 2: Comparison of surface hardness according to strengthening conditions

[0132] In order to compare the surface hardness according to the chemical strengthening conditions, the Vickers hardness of the glass ceramic substrate before chemical strengthening and the substrate chemically strengthened by the method according to Conditions 1 to 3 in Preparation Example 2 was measured, and the measurement results are shown in the following Tables 3 and Fig.10 Shown in.

[0133] Table 3

[0134]

[0135] Refer to Table 3 and Fig.10 , confirming that under condition 2, at high temperature and high concentration of KNO 3 The substrate chemically strengthened for a short time has a maximum surface hardness of 1000 Hv or higher.

[0136] Experimental Example 3: Comparison of friction coefficient according to surface roughness

[0137] In order to compare the friction coefficient according to the surface roughness value of the uneven structure, the friction coefficient of the glass ceramic substrate was measured under a load of 5 N before and after the uneven structures having different surface roughness were formed, and is shown in the following Tables 4 and Fig.11 Shown in.

[0138] Table 4

[0139]

[0140] Refer to Table 4 and Fig.11 , it was confirmed that the lowest friction coefficient was obtained at a surface roughness (Ra) of 0.3 μm, and a friction coefficient similar to that of the glass ceramic substrate before the uneven structure was formed was obtained at a surface roughness (Ra) exceeding 1.0 μm.

[0141] Experimental Example 4: Comparison of surface hardness according to strengthening time

[0142] In order to compare the surface hardness according to the chemical strengthening time, a glass ceramic substrate having an excellent effect on improving the surface hardness was prepared according to Condition 2 of Preparation Example 2, but the chemical strengthening time was changed and its Vickers hardness was measured, and the results are shown in the following Tables 5 and Fig.12 Shown in.

[0143] Table 5

[0144]

[0145] Refer to Table 5 and Fig.12, compared with the surface hardness before chemical strengthening, by using KNO 3 Chemical strengthening significantly increases the surface hardness. However, despite the increase in strengthening time, no significant difference is observed in the surface hardness compared with the chemical strengthening for 20 minutes. Therefore, in terms of process efficiency and productivity, it may be preferred to perform chemical strengthening for a short time to increase the surface strength of the glass-ceramic substrate.

[0146] The embodiments of the present disclosure have been shown and described above with reference to the accompanying drawings. However, the disclosed embodiments are exemplary, and the scope of the present disclosure is not limited thereto. It will be appreciated by those of ordinary skill in the art that the present disclosure can be easily modified into other detailed forms without changing the technical principles or basic features of the present disclosure.

Claims

1. A top plate of a cooking stove, on which a cooking container can be placed to be heated by the cooking stove, the top plate include: A glass ceramic substrate having a chemically enhanced top surface having an uneven structure with an average surface roughness (Ra) of 0.1 μm to 1.0 μm.

2. The cooking hob top plate of claim 1, wherein the glass ceramic substrate comprises: Contains Li 2 O、Al 2 O 3 and SiO 2 A lithium aluminum silicon-based crystallized glass as a basic composition, and At least one crystal phase selected from the group consisting of β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. 3 . The cooking hob top plate according to claim 2 , wherein the glass ceramic substrate further comprises at least one element selected from the group consisting of V, Mg, P, Fe, Ti, and Zr.

4. The cooking stove top plate according to claim 1, wherein the top surface of the glass ceramic substrate is formed by contacting with a 3 and NaNO 3 The at least one enhancing salt in the catalyst is chemically enhanced by ion exchange. 5 . The cooking hob top plate of claim 1 , wherein the glass ceramic substrate has a Vickers hardness of 950 to 1200 Hv and a friction coefficient of 0.42 to 0.

71.

6. The cooking stove top plate according to claim 1, further comprising: include: A printed layer beneath the glass ceramic substrate, The printing layer includes a background printing layer and a shielding printing layer below the background printing layer.

7. A method for processing a glass ceramic substrate, the method include: forming the top surface to have an uneven structure having an average surface roughness (Ra) of 0.1 μm to 1.0 μm; as well as The top surface having the uneven structure is chemically enhanced.

8. The method of claim 7, wherein the glass-ceramic substrate comprises: Contains Li 2 O、Al 2 O 3 and SiO 2 A lithium aluminum silicon-based crystallized glass as a basic composition, and At least one crystal phase selected from the group consisting of β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. 9 . The method according to claim 8 , wherein the glass-ceramic substrate further comprises at least one element selected from the group consisting of V, Mg, P, Fe, Ti, Cr, and Zr. 10 . The method according to claim 7 , wherein the forming the top surface to have the uneven structure is performed by chemical etching, sand blasting, or a combination thereof.

11. The method according to claim 7, wherein the chemical enhancement is carried out by reacting with a 3 and NaNO 3 This is done by ion exchanging at least one enhancing salt.

12. The method according to claim 11, wherein the chemical enhancement uses KNO having a concentration of 90 wt% to 100 wt%. 3 The solution was allowed to stand as an enhancing salt for 10 to 60 minutes.

13. Induction heating cooker, include: A cooking stove top plate, on which a cooking container is placed; as well as a plurality of induction heating coils, the plurality of induction heating coils being disposed below the top plate of the cooking hob and configured to generate a magnetic field with the cooking container placed on the top plate to heat the cooking container, The cooking range top plate includes a glass ceramic substrate having a chemically enhanced uneven structure on the top surface, and the uneven structure has an average surface roughness (Ra) of 0.1 μm to 1.0 μm.

14. The induction heating cooker according to claim 13, wherein the glass ceramic substrate comprises: Contains Li 2 O、Al 2 O 3 and SiO 2 A lithium aluminum silicon-based crystallized glass as a basic composition, and At least one crystal phase selected from the group consisting of β-quartz crystal phase, β-spodumene crystal phase and β-eucryptite crystal phase. 15 . The induction heating cooker according to claim 13 , wherein the glass ceramic substrate has a Vickers hardness of 950 Hv to 1200 Hv and a friction coefficient of 0.42 to 0.71.