Flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings and combined inhibitor

By using a combination of ammonium chloride, sodium sulfide, and sodium carbonate inhibitors, along with oxalic acid and hypochlorous acid to adjust the pH, the problems of low zinc oxide recovery and foam control in lead-zinc sulfide tailings were solved, achieving efficient separation and recovery of zinc oxide minerals and improving the simplicity and recovery rate of flotation operations.

CN118904528APending Publication Date: 2024-11-08YUNNAN CHIHONG ZN & GE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410973429.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing technologies for recovering zinc oxide from lead-zinc sulfide tailings suffer from problems such as poor adaptability to ore properties, complex flotation operations, low recovery rates, and difficulty in controlling foam. In particular, high-pressure water flushing cannot effectively solve the problem of foam floating, which affects normal production.

Method used

A method using a combination of ammonium chloride, sodium sulfide, and sodium carbonate inhibitors, along with oxalic acid and hypochlorous acid to adjust the pH value, is employed to separate zinc oxide ore from gangue minerals through reverse flotation. The combination of oxalic acid and hypochlorous acid is used to adjust the pulp pH to 7.5-8.5, weakening the foaming ability of the collector, preferentially desorbing zinc oxide minerals, reducing foam volume, and improving recovery rate.

Benefits of technology

It effectively improves the recovery rate of zinc oxide, enhances the adaptability to ore properties, simplifies flotation operations, and solves the problem of difficult foam elimination, thus achieving efficient zinc oxide mineral recovery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118904528A_ABST
    Figure CN118904528A_ABST
Patent Text Reader

Abstract

The invention relates to a flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings and a combined inhibitor, and belongs to the technical field of lead-zinc oxide ore beneficiation. The flotation method comprises the steps that when flotation is conducted on the lead-zinc sulfide ore tailings, ammonium chloride, sodium sulfide and sodium carbonate are added into lead-zinc sulfide ore tailing pulp to serve as a combined inhibitor of zinc oxide ore, then a gangue mineral collecting agent is added for reverse flotation roughing, and roughing tailings and roughing concentrate are obtained; oxalic acid and hypochlorous acid are added into roughing tailings to adjust the pH value of ore pulp to 7.5-8.5, then scavenging is conducted, scavenged concentrate and zinc tailings are obtained, and the scavenged concentrate is returned to reverse flotation roughing; and a gangue mineral collecting agent is added into the roughing concentrate for concentration, and zinc concentrate is obtained. The combined inhibitor is utilized, the reverse flotation technological process is combined, and the pH is adjusted through a special reagent in the scavenging process, so that the recovery rate of zinc oxide is effectively increased, and the combined inhibitor has great economic significance for increasing the flotation level of complex zinc oxide ore in China and the comprehensive utilization rate of resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of lead-zinc oxide ore beneficiation, and specifically, relates to a flotation method and a combined inhibitor for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings. Background Art

[0002] With the depletion of zinc sulfide resources, it is necessary to develop and utilize tailings resources to recover zinc oxide. Lead-zinc sulfide tailings are usually the remaining part of lead-zinc sulfide ores after beneficiation or other comprehensive utilization. They contain useful zinc oxide resources. Recovering zinc oxide from lead-zinc sulfide tailings is an inevitable choice for sustainable development.

[0003] At present, the recovery of zinc oxide minerals usually adopts sulfide-amine flotation, sulfide-xanthate flotation, chloramine catalyzed sulfide-xanthate flotation and other methods.

[0004] However, the sulfide-amine flotation method is extremely sensitive to ore slime and consumes a large amount of reagents. In particular, the inevitable ore slime in industrial production will make the production process difficult to control and make the production unable to proceed normally. Therefore, desliming is necessary. The loss of a large amount of fine-grained zinc minerals during the desliming process is the fundamental reason why the comprehensive index of mineral processing in the sulfide-amine flotation of zinc oxide ore is not high.

[0005] For the sulfidation-xanthate flotation method, the quality of the sulfidation effect is crucial in the xanthate flotation of zinc oxide ore. To achieve effective sulfidation of zinc oxide minerals and obtain a stable artificial zinc sulfide surface, it has become the key to the sulfidation-xanthate flotation of zinc oxide ore. Finding a better sulfidation method and how to achieve an enhanced sulfidation process are still long-term concerns of mineral processing workers and researchers. Since the sulfidation effect at room temperature is not good, this method requires heating during the sulfidation process. But even with heated sulfidation, the flotation recovery rate is relatively low, and it is generally difficult to exceed 70%.

[0006] The chloramine catalytic sulfidation-xanthate flotation method also requires an enhanced sulfidation process and often targets fine-grade ore slime for targeted recovery.

[0007] In summary, the existing flotation methods for zinc oxide ore generally have the problem of poor adaptability to ore properties. How to provide a flotation method with strong adaptability to raw materials, simple flotation operation and high recovery rate has always been a technical problem that technicians in this field need to solve urgently.

[0008] In addition, foam is a thorny problem that must be faced during the flotation process. If the foam is large, viscous, and has poor fluidity, it will be difficult to break the foam for a long time, which will have a negative impact on the mineral processing process indicators. At present, the conventional method of eliminating foam is to use high-pressure water flushing, but when dealing with oxidized ores, high-pressure water flushing cannot effectively solve the problem, causing the foam to break away from the foam tank and float around the workshop, making normal production impossible. Another method is to use a large amount of defoaming agent in a conventional foam tank to defoam, but the existing defoaming agent has the problem of slow defoaming speed, making it difficult to achieve timely defoaming and continuous flotation operations, which in turn affects the properties of the flotation slurry and the final flotation effect. Summary of the invention

[0009] In order to overcome the problems existing in the background technology, one of the purposes of this application is to provide a flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings, which has strong adaptability to raw materials, simple flotation operation, can effectively suppress flotation foam during the flotation process, and has a high recovery rate of zinc oxide.

[0010] The second purpose of the present application is to provide a combined depressant, which is used to carry out flotation separation of zinc oxide ore and gangue minerals such as calcite.

[0011] To achieve the above objectives, this application is implemented through the following technical solutions:

[0012] A flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide tailings, comprising: adding ammonium chloride, sodium sulfide and sodium carbonate as a combined inhibitor of zinc oxide ore to the lead-zinc sulfide tailings slurry during flotation of the lead-zinc sulfide tailings, and then adding a gangue mineral collector for reverse flotation roughing to obtain roughing tailings and roughing concentrate;

[0013] Oxalic acid and hypochlorous acid are added to the roughing tailings to adjust the pH value of the pulp to 7.5-8.5, and then scavenging is carried out to obtain scavenging concentrate and zinc tailings. The scavenging concentrate is returned to the reverse flotation roughing;

[0014] The rougher concentrate is added with a gangue mineral collector for concentration to obtain zinc concentrate.

[0015] Optionally, the combined inhibitor is added in the following order: ammonium chloride, sodium sulfide, and sodium carbonate. First, ammonium chloride is added, then sodium sulfide is added, and finally sodium carbonate is added.

[0016] Specifically, the ammonium chloride in the combined inhibitor in the present application mainly plays its role in corroding and cleaning the minerals. The pretreatment of sodium sulfide and sodium carbonate can increase the relative content of zinc atoms on the surface of zinc oxide ore, especially for silicon-containing hemimorphite. In addition, since the lead-zinc sulfide ore tailings contain a large amount of gangue minerals such as calcite and dolomite, ammonium chloride has a certain acidity and has a cleaning effect on the calcium and magnesium ions precipitated on the surface of zinc oxide ore, thereby exposing the fresh surface. The pretreatment of ammonium chloride causes physical and chemical adsorption on the surface of zinc oxide, thereby increasing the difference in floatability between zinc oxide ore and gangue minerals such as calcite under the fatty acid system.

[0017] In particular, by using a combination of oxalic acid and hypochlorous acid to adjust the pH of the slurry during scavenging to 7.5-8.5, the foaming and collecting capabilities of the fatty acid system collector are weakened, the adsorption of the collector on the surface of the zinc oxide mineral is preferentially reduced, the desorption of the zinc oxide mineral and the collector is achieved, the amount of foam is greatly reduced, and better recovery of zinc is achieved.

[0018] Optionally, the gangue mineral collector may specifically be a common reagent such as oxidized paraffin 731 that can capture gangue minerals.

[0019] Furthermore, the mass ratio of the oxalic acid to the hypochlorous acid is 1:1.

[0020] Optionally, the above-mentioned zinc oxide ore is ferrospinite, willemite, hemimorphite or zincite.

[0021] Optionally, the reverse flotation roughing selection is performed once; the fine selection is performed twice; and the scavenging selection is performed twice.

[0022] The present application also provides a combined inhibitor comprising ammonium chloride, sodium sulfide and sodium carbonate.

[0023] Optionally, the mass ratio of the ammonium chloride, the sodium sulfide and the sodium carbonate is 1:6:3.

[0024] It should be noted that the total amount of oxidized paraffin soap 731, the total amount of ammonium chloride, sodium sulfide, sodium carbonate, and the total amount of oxalic acid and hypochlorous acid added are all closely related to the content of gangue minerals in the original ore and are added according to actual conditions. The total amount of oxidized paraffin soap 731 is 20-500g / t, the total amount of ammonium chloride, sodium sulfide, and sodium carbonate is 2000-6000g / t, and the total amount of oxalic acid and hypochlorous acid is 200-2000g / t.

[0025] Beneficial effects of this application:

[0026] 1. In the present application, when zinc oxide is recovered by flotation from lead-zinc sulfide ore tailings, a combined inhibitor consisting of ammonium chloride, sodium sulfide and sodium carbonate is first used in combination with a reverse flotation method to inhibit the zinc oxide ore, thereby achieving effective separation of zinc oxide minerals and gangue minerals such as calcite, and increasing the floatability difference between zinc oxide ore and gangue minerals such as calcite; then the rougher concentrate is fined. In particular, during the scavenging process of the rougher tailings, a combination of oxalic acid and hypochlorous acid is specially added to adjust the pH of the pulp to 7.5-8.5 during the scavenging process, weaken the foaming and collecting ability of the fatty acid system collector, preferentially reduce the adsorption of the collector on the surface of the zinc oxide mineral, achieve desorption of the zinc oxide mineral and the collector, greatly reduce the amount of foam, and thus achieve better recovery of zinc; the concentrate obtained after scavenging is returned to the concentration process for further concentration; by utilizing the combined inhibitor in the present application, combining the reverse flotation process, and adjusting the pH with a special reagent during the scavenging process, the recovery rate of zinc oxide is effectively improved, which has great economic significance for improving the flotation level and comprehensive resource utilization rate of complex zinc oxide ores in my country.

[0027] 2. The combined inhibitors of ammonium chloride, sodium sulfide and sodium carbonate in the present application and the combined regulators of oxalic acid and hypochlorous acid have the excellent characteristics of high sorting efficiency and strong adaptability to fluctuations in ore properties.

[0028] 3. The present application adopts oxalic acid and hypochlorous acid to adjust the pH in the scavenging process, which does not affect the properties of the flotation pulp and the flotation effect, while solving the problem of difficulty in eliminating foam and avoiding the problems existing in conventional defoaming methods. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is the process flow chart of this application. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and beneficial effects of the present application clearer, the preferred embodiments of the present application will be described in detail below to facilitate the understanding of technical personnel.

[0031] Example 1

[0032] An experimental study on the reverse flotation recovery of zinc oxide was conducted on the tailings of a lead-zinc sulfide mine in Yunnan. The tailings of a lead-zinc sulfide mine contained 1.98% Zn, the main useful zinc mineral was willemite, and the gangue minerals were mainly calcite, dolomite, quartz, etc.

[0033] The combined inhibitor in this embodiment is composed of ammonium chloride, sodium sulfide, and sodium carbonate in a mass ratio of 1:6:3; the combined adjuster is composed of oxalic acid and hypochlorous acid in a mass ratio of 1:1.

[0034] The flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings in this application has a process flow as follows: Figure 1 As shown, the specific operations are as follows:

[0035] When the lead-zinc sulfide tailings are flotated, the lead-zinc sulfide tailings slurry is used as feed ore; 3000g / t of combined inhibitor ammonium chloride, sodium sulfide, and sodium carbonate are added to the lead-zinc sulfide tailings slurry in sequence, and then 150g / t of collector oxidized paraffin soap 731 is added, and then reverse flotation roughing is carried out, and roughing tailings and roughing concentrates are obtained after one roughing;

[0036] 500 g / t and 250 g / t of combined adjusting agents oxalic acid and hypochlorous acid were added to the obtained roughing tailings to adjust the pulp pH to 8.5 and perform two scavenging to obtain tailings. The scavenging concentrate was returned to the reverse flotation roughing. In the scavenging process, by adding oxalic acid and hypochlorous acid, no large amount of foam was generated, the foam was defoamed quickly, and the foam viscosity was low.

[0037] 50 g / t and 25 g / t of collector oxidized paraffin soap 731 were added to the obtained rougher concentrate for two rounds of concentration to obtain zinc concentrate.

[0038] Example 2

[0039] An experimental study on the reverse flotation recovery of zinc oxide was conducted on the tailings of a lead-zinc sulfide mine in Yunnan. The tailings of a lead-zinc sulfide mine contained 3.14% Zn. The main useful zinc minerals were hemimorphite and willemite, and the gangue minerals were mainly calcite, dolomite, mica, etc.

[0040] The combined inhibitor in this embodiment is composed of ammonium chloride, sodium sulfide, and sodium carbonate in a mass ratio of 1:6:3; the combined adjuster is composed of oxalic acid and hypochlorous acid in a mass ratio of 1:1.

[0041] The flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings in this application is operated as follows:

[0042] When the lead-zinc sulfide tailings are flotated, the lead-zinc sulfide tailings slurry is used as feed ore; 5000g / t of combined inhibitor ammonium chloride, sodium sulfide, and sodium carbonate are added to the lead-zinc sulfide tailings slurry in sequence, and then 250g / t of collector oxidized paraffin soap 731 is added, and then reverse flotation roughing is carried out, and roughing tailings and roughing concentrates are obtained after one roughing;

[0043] 1500 g / t (first scavenging) and 500 g / t (second scavenging) of combined adjusting agents oxalic acid and hypochlorous acid were added to the obtained roughing tailings to adjust the pulp pH to 7.5 (before adjustment, the pulp pH was 10), and two scavengings were performed to obtain tailings, and the scavenged concentrate was returned to the reverse flotation roughing;

[0044] 80 g / t and 40 g / t of collector oxidized paraffin soap 731 were added to the obtained rougher concentrate for two rounds of concentration to obtain zinc concentrate.

[0045] Example 3

[0046] An experimental study on the reverse flotation recovery of zinc oxide was conducted on the tailings of a lead-zinc sulfide mine in Guizhou. The tailings of a lead-zinc sulfide mine contained 0.95% Zn, the main useful zinc mineral was willemite, and the gangue minerals were mainly calcite, dolomite, quartz, etc.

[0047] The combined inhibitor in this embodiment is composed of ammonium chloride, sodium sulfide, and sodium carbonate in a mass ratio of 1:6:3; the adjusting agent is composed of oxalic acid and hypochlorous acid in a mass ratio of 1:1.

[0048] The flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings in this application is operated as follows:

[0049] When the lead-zinc sulfide tailings are flotated, the lead-zinc sulfide tailings slurry is used as feed; 4500g / t of combined inhibitor ammonium chloride, sodium sulfide, and sodium carbonate are added to the lead-zinc sulfide tailings slurry in sequence, and then 80g / t of collector oxidized paraffin soap 731 is added, and then reverse flotation roughing is carried out, and roughing tailings and roughing concentrates are obtained after one roughing;

[0050] 900g / t and 450g / t of combined adjusting agents oxalic acid and hypochlorous acid were added to the roughing tailings to adjust the pulp pH to 8.0, and two scavenging operations were performed to obtain tailings. The scavenging concentrate was returned to the reverse flotation roughing;

[0051] 20 g / t and 10 g / t of collector oxidized paraffin soap 731 were added to the obtained rougher concentrate for two rounds of concentration to obtain zinc concentrate.

[0052] Comparative Example 1

[0053] The flotation and reagent system used in this comparative example is: reverse flotation process, water glass and sodium carbonate as inhibitors, and oxidized paraffin soap 731 as collector.

[0054] The same feed as in Example 1 was used to perform reverse flotation to recover zinc oxide using conventional depressants, which included water glass and sodium carbonate in a mass ratio of 1:1. The specific operation was as follows:

[0055] 3000g / t of combined depressant water glass and sodium carbonate are added to the lead-zinc sulfide ore tailings slurry in sequence, and then 150g / t of collector oxidized paraffin soap 731 is added, and then reverse flotation roughing is carried out, and roughing tailings and roughing concentrate are obtained after one roughing operation;

[0056] 500 g / t and 250 g / t of combined inhibitors of water glass and sodium carbonate were added to the obtained roughing tailings for two scavenging operations to obtain tailings, and the scavenged concentrate was returned to the reverse flotation roughing operation; a large amount of foam was generated during the scavenging process, and the foam viscosity was significantly higher than that in Example 1, and relative to the faster foam defoaming speed in Example 1, the foam in this comparative example was more difficult to eliminate;

[0057] 50 g / t and 25 g / t of collector oxidized paraffin soap 731 were added to the obtained rougher concentrate for two rounds of concentration to obtain zinc concentrate.

[0058] Comparative Example 2

[0059] The flotation and reagent system used in this comparative example is: positive flotation process, sodium sulfide as a depressant, and butyl xanthate as a collector.

[0060] The same feed as in Example 1 was used to recover zinc oxide using a positive flotation process. The specific operation was as follows:

[0061] 1000g / t sodium sulfide and 300g / t collector butyl xanthate are added to the lead-zinc sulfide ore tailings slurry in sequence, and then positive flotation roughing is carried out to obtain roughing tailings and roughing concentrate after one roughing operation;

[0062] 50g / t and 25g / t of collector butyric acid were added to the roughing tailings obtained to carry out two scavenging operations to obtain tailings, and the scavenging concentrate was returned to the flotation roughing operation; similarly, a large amount of foam that was difficult to eliminate quickly was generated in the scavenging process in this comparative example, and the foam had a large viscosity;

[0063] 100 g / t and 50 g / t sodium sulfide were added to the obtained rougher concentrate for two rounds of concentration to obtain zinc concentrate.

[0064] Comparative Example 3

[0065] The flotation and reagent system adopted in this comparative example is: a positive flotation process is adopted, no inhibitor is added, and dodecylamine is used as a collector.

[0066] The same feed as in Example 1 was used to recover zinc oxide by positive flotation. The specific operation was as follows:

[0067] 100g / t of collector dodecylamine is added to the lead-zinc sulfide ore tailings slurry, and then a direct flotation roughing operation is performed to obtain roughing tailings and roughing concentrates;

[0068] 20g / t and 10g / t of collector dodecylamine were added to the roughing tailings obtained to carry out scavenging twice to obtain tailings, and the scavenging concentrate was returned to the flotation roughing; similarly, a large amount of foam that was difficult to eliminate quickly was generated in the scavenging process in this comparative example, and the foam viscosity was large;

[0069] The rougher concentrate is subjected to two blank concentrations to obtain zinc concentrate.

[0070] Comparative Example 4

[0071] The same ore feed as in Example 1.

[0072] The difference from Example 1 is that no adjusting agent oxalic acid and hypochlorous acid are added to the roughing tailings to adjust the pH, and the rest are the same. The actual pH of the pulp is 10.

[0073] In this comparative example, a large amount of foam is generated during the sweeping process and the foam is difficult to break, and the foam viscosity is high.

[0074] Example 5

[0075] The same ore feed as in Example 1.

[0076] The difference from Example 1 is that sulfuric acid (or other substances) is added to the roughing tailings to adjust the pH of the slurry to 7.5, and the rest are the same.

[0077] Adding sulfuric acid to adjust the pH of the slurry has little defoaming effect on the foam.

[0078] The zinc content in the zinc concentrate and tailings obtained in Examples 1-3 and Comparative Examples 1-5 was analyzed and detected. The specific flotation results are shown in Table 1 below:

[0079] Table 1 Flotation results of different embodiments and comparative examples

[0080]

[0081] The results of Examples 1-3 and Comparative Examples 1-3 show that the present application can effectively realize the comprehensive recovery of zinc oxide ore in lead-zinc sulfide ore tailings. Compared with the positive flotation process + conventional mineral processing reagents or the reverse flotation process + conventional mineral processing reagents used in the comparative examples, Examples 1-3 use reverse flotation + specific combined inhibitors and pH adjustment reagents, and the zinc grade and zinc recovery rate of the zinc concentrate obtained are significantly higher.

[0082] It can also be seen from Example 1 and Comparative Examples 4-5 that when oxalic acid and hypochlorous acid are not added to adjust the pH or sulfuric acid is used to adjust the pH during the scavenging operation of the rougher tailings, the flotation results are not as good as those of Example 1.

[0083] In particular, it can be seen from Example 1 and Comparative Example 4 that even if the combined depressant is added during the flotation process, but oxalic acid and hypochlorous acid are not added to adjust the pH, the large amount of foam generated cannot be quickly eliminated and the foam viscosity is high, which affects the final zinc grade and zinc recovery rate.

[0084] From the comparison between Example 1 and Comparative Examples 4 and 5, it can be seen that although the combined depressant is added during the flotation process, the reagent for adjusting the pH is sulfuric acid. Although the pH is controlled at the same level, it has basically no defoaming effect on the foam. The grade and recovery rate of the zinc concentrate finally obtained by flotation are still relatively low, far less than the flotation effect obtained by adjusting the pH using oxalic acid and hypochlorous acid.

[0085] It can be seen from the above description that in the present application, when the lead-zinc sulfide ore tailings are subjected to flotation treatment, the reverse flotation process, the combined inhibitor and the pH adjusting agent composed of oxalic acid and hypochlorous acid are indispensable, and their cooperation can effectively realize the separation of zinc oxide ore and calcite gangue minerals, and finally achieve the purpose of efficient and comprehensive recovery of zinc oxide.

[0086] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solution of the present application and are not intended to be limiting. Although the present application has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and section without departing from the scope defined by the claims of the present application.

Claims

1. A flotation method for comprehensively recovering zinc oxide ore from lead-zinc sulfide ore tailings, characterized in that: The method comprises adding ammonium chloride, sodium sulfide and sodium carbonate as a combined inhibitor of zinc oxide ore to the lead-zinc sulfide tailings slurry during flotation of the lead-zinc sulfide tailings, and then adding a gangue mineral collector to perform reverse flotation roughing to obtain roughing tailings and roughing concentrate; Oxalic acid and hypochlorous acid are added to the roughing tailings to adjust the pH value of the pulp to 7.5-8.5, and then scavenging is carried out to obtain scavenging concentrate and zinc tailings. The scavenging concentrate is returned to the reverse flotation roughing; The rougher concentrate is added with a gangue mineral collector for concentration to obtain zinc concentrate.

2. The flotation method according to claim 1, characterized in that: The combined inhibitor is added in the following manner: ammonium chloride, sodium sulfide, and sodium carbonate are added in sequence, and the mass ratio of sodium sulfide to the sodium carbonate is 1:6:

3.

3. The flotation method according to claim 1 or 2, characterized in that: The mass ratio of the oxalic acid to the hypochlorous acid is 1:

1.

4. The flotation method according to claim 1, characterized in that: The zinc oxide ore is ferrospinite, willemite, hemimorphite or zincite.

5. The flotation method according to claim 1, characterized in that: The gangue mineral collector is oxidized paraffin soap 731.

6. The flotation method according to claim 3, characterized in that: The reverse flotation roughing selection is performed once; the cleaning selection is performed twice; and the sweeping selection is performed twice.

7. A combined inhibitor for comprehensive recovery of zinc oxide ore from lead-zinc sulfide ore tailings, characterized in that: The combined depressant comprises ammonium chloride, sodium sulfide and sodium carbonate; the combined depressant is used for flotation separation of zinc oxide ore and gangue minerals.

8. The combined inhibitor according to claim 7, characterized in that: The mass ratio of the ammonium chloride, the sodium sulfide and the sodium carbonate is 1:6:3.