Sintered metal porous material and preparation method and application thereof

Through the preparation of sintered metal porous materials, the synergistic effect of Ni and Hf elements is used to solve the problem of poor versatility of nickel alloy anode materials in alkaline water electrolysis, and efficient hydrogen production and electrolytic efficiency improvement are achieved.

CN118905221APending Publication Date: 2024-11-08SICHUAN SIDANENG ENVIRONMENTAL PROTECTION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410948347.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the prior art, nickel alloy anode materials have problems such as poor versatility, high overpotential, poor voltage stability and poor corrosion resistance in alkaline water electrolysis, making it difficult to achieve efficient hydrogen production.

Method used

Using sintered metal porous materials, a material with multi-layer structure and micron-scale pores is prepared through the synergistic action of Ni and Hf elements, which is used as anode material to improve catalytic activity and stability, and is optimized through a special heating and cooling process. The structure of the material.

Benefits of technology

It realizes high-efficiency electrolysis in alkaline water bodies, reduces the energy barrier of water cracking reaction, improves electrolytic efficiency and corrosion resistance, shows good versatility and stability, and is suitable for oxygen evolution and chlorine evolution reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118905221A_ABST
    Figure CN118905221A_ABST
Patent Text Reader

Abstract

The invention discloses a sintered metal porous material and a preparation method and application thereof. The technical problems that in the prior art, a nickel alloy anode material is poor in universality, high in overpotential, poor in voltage stability and poor in corrosion resistance are solved. The sintered metal porous material is provided with three metal layers and a layered structure composed of the three metal layers, the three metal layers are all composed of Ni elements and Hf elements, and the proportions of the Ni elements and the Hf elements in the three metal layers are different. The preparation method of the sintered metal porous material comprises the steps that Ni powder and Hf powder are subjected to ball milling and mixing, and mixed powder is obtained; adding a forming aid into the mixed powder, and then granulating and sieving to obtain formed particles; pressing and forming the formed particles to obtain a green body; carrying out segmented heating sintering treatment on the green body; and the blank is subjected to segmented cooling treatment, and the sintered metal porous material is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater purification, and in particular to a sintered metal porous material and a preparation method and application thereof. Background Art

[0002] A large amount of wastewater is generated in people's daily life and industrial production. Most of these wastewaters contain pollutants that exceed the standard and need to be treated before discharge. With the development of the hydrogen energy industry, the demand for hydrogen in society is gradually increasing, and large-scale and cheap production of hydrogen is an important prerequisite for the development and utilization of hydrogen energy. If the above wastewater can be used to produce hydrogen, it is expected to turn the burden into power.

[0003] Among the many hydrogen production methods, the cost of hydrogen production by electrolysis of wastewater is low, the product is pollution-free, and the technical advantages are obvious, but there are still the following problems to be solved. The traditional wastewater hydrogen production process first needs to purify and treat the organic matter in the wastewater (usually biochemical reactions and Fenton oxidation reactions), which can reduce the adverse effects of organic matter on the use of electrode materials, but this will result in a longer water treatment process and higher energy consumption.

[0004] In the process of electrolyzing wastewater to produce hydrogen, the cathode generally produces hydrogen, and the anode can produce oxygen, chlorine, carbon dioxide, sulfur dioxide and other gases depending on the electrolyte. The ideal anode material should first be versatile and be able to exhibit good electrochemical properties in various electrolytes. For example, it can be used to precipitate both oxygen and chlorine. Secondly, in order to obtain the highest possible current density and the smallest overpotential under a certain amount of electrical energy, the electrode material needs to have high surface area, high conductivity, good catalytic activity, long-term mechanical and chemical stability, and low cost and safety.

[0005] Generally, precious metals such as Pt, Pd, and Au are considered to be electrode materials with excellent and efficient electrocatalytic performance. However, the electrolysis process in alkaline water involves multi-process water dissociation, and the electrolysis efficiency is far less than that in acidic water. Even if precious metal electrodes are used, the improvement in the electrolysis efficiency of alkaline water is very limited. In addition, the sources of precious metals are scarce and expensive, making it impossible to achieve large-scale industrial production.

[0006] Therefore, it is necessary to develop highly active and stable non-precious metal anode materials suitable for electrolysis of alkaline water. Nickel alloy is one of the most studied anode materials due to its simple preparation method, rich variety and excellent catalytic performance. However, the current nickel alloy materials have poor versatility, high overpotential, poor voltage stability and poor corrosion resistance, and are still not suitable for electrolysis of alkaline water. Summary of the invention

[0007] In the first aspect, the main purpose of the present invention is to provide a sintered metal porous material and a preparation method and application thereof, so as to solve the technical problems of poor versatility, high overpotential, poor voltage stability and poor corrosion resistance of nickel alloy anode materials in the prior art.

[0008] In order to achieve the purpose of the first aspect above, the present invention first provides a sintered metal porous material and a preparation method thereof, and the technical scheme is as follows:

[0009] The sintered metal porous material has three metal layers and a layered structure formed by them. The three metal layers are all composed of Ni elements and Hf elements, and the proportions of Ni elements and Hf elements in the three metal layers are different.

[0010] As a further improvement of the above-mentioned sintered metal porous material: the phases in the XRD spectrum of the sintered metal porous material include HfNi3 intermetallic compound, Hf3Ni7 intermetallic compound, Hf single substance and Ni single substance.

[0011] As a further improvement of the above sintered metal porous material: the sintered metal porous material comprises a first metal layer, a second metal layer wrapping the first metal layer and a third metal layer wrapping the second metal layer, and the Ni element content is: first metal layer>second metal layer>third metal layer.

[0012] As a further improvement of the above-mentioned sintered metal porous material: the first metal layer is multiple and arranged at intervals.

[0013] The method for preparing a sintered metal porous material comprises the following steps:

[0014] The Ni powder and the Hf powder are ball-milled to obtain a mixed powder;

[0015] Adding a forming aid to the mixed powder, followed by granulation and sieving to obtain formed particles;

[0016] Pressing the formed particles into a shape to obtain a green body;

[0017] The green body is subjected to staged temperature-raising sintering treatment;

[0018] The green body is subjected to a staged cooling treatment to obtain a sintered metal porous material.

[0019] As a further improvement of the preparation method of the above-mentioned sintered metal porous material: the staged temperature rising sintering treatment is carried out under vacuum, and the heating process is specifically as follows: starting from room temperature to the sintering temperature, keeping the temperature for 40 to 80 minutes after each temperature rise of 50 to 150°C, and keeping the temperature for 150 to 200 minutes after reaching the sintering temperature. The sintering temperature is 1250 to 1350°C, and the heating rate of each temperature rise is 4 to 7°C / min.

[0020] As a further improvement of the above-mentioned method for preparing the sintered porous metal material, the stepwise temperature-raising sintering process is as follows:

[0021] The first stage is to heat from room temperature to 400°C and keep it for 60 minutes;

[0022] The second stage is to continue heating to 500℃ and keep it for 60min;

[0023] The third stage is to continue heating to 600℃ and keep it for 60min;

[0024] The fourth stage is to continue heating to 700℃ and keep it for 60min;

[0025] The fifth stage is to continue heating to 800°C and keep warm for 60 minutes;

[0026] The sixth stage is to continue heating to 900°C and keep it for 60 minutes;

[0027] The seventh stage is to continue heating to 1000°C and keep warm for 60 minutes;

[0028] The eighth stage is to continue heating to 1100°C and keep warm for 60 minutes;

[0029] The ninth stage is to continue heating to 1300°C and keep it warm for 18 minutes.

[0030] As a further improvement of the above-mentioned method for preparing the sintered porous metal material: the segmented cooling treatment is carried out under vacuum, and the cooling process is specifically as follows:

[0031] The first stage is to cool down from the sintering temperature to 800-9000℃, with a cooling rate of 10-15℃ / min;

[0032] The second stage is to continue cooling to 400-500°C, with a cooling rate of 4-7°C / min;

[0033] The third stage is to continue cooling to below 100°C at a cooling rate of 15-20°C / min, thereby obtaining a sintered metal porous material.

[0034] In order to achieve the purpose of the first aspect above, the present invention secondly provides an electrolytic hydrogen production device and an electrolytic hydrogen production method, and the technical scheme is as follows:

[0035] The electrolytic hydrogen production device comprises an anode, wherein the anode is made of the sintered metal porous material described in the first aspect.

[0036] The electrolytic hydrogen production method adopts the above-mentioned electrolytic hydrogen production device to electrolyze alkaline water.

[0037] The sintered metal porous material and its preparation method and application described in the first aspect have the following advantages:

[0038] (1) In the present invention, Hf (hafnium) is in group 3 and is an early transition metal element, and Ni is in group 10 and is a late transition metal element. The water splitting activity of perovskite oxides is closely related to the number of d-orbital electrons in the transition metal ions, that is, the activity of early transition metal oxides is relatively low, and the activity of late transition metal oxides is relatively high. The present invention effectively reduces the reaction energy barrier of important intermediates (OH*, O*, OOH*) through the synergistic effect of early transition metal elements and late transition metal elements, thereby greatly improving the overall water splitting efficiency.

[0039] (2) The sintered metal porous material of the present invention contains almost no solid solution alloys, and the metal elements mainly exist in the form of intermetallic compounds. Due to the mixed bond form of metallic bonds and covalent bonds, the electronic structure of the material can be further optimized. On the one hand, it has significantly better strength and corrosion resistance. On the other hand, it can promote the adsorption and release of ions during electrolysis, reduce the dissociation energy barrier of water in the electrolyte system, improve the electrolysis efficiency, and show good catalytic activity and stability.

[0040] (3) The sintered metal porous material prepared by the element powder reaction synthesis method of the present invention has micron-sized pores, which can greatly increase the specific surface area of ​​the material and provide sufficient active sites. At the same time, the micron-sized pores provide channels for gas escape, avoiding the enrichment of gas on the electrode surface and covering the catalytic active sites.

[0041] (4) The sintered metal porous material of the present invention has a layered structure with different Ni content distributions, wherein the inner layer has a higher Ni content, which is beneficial to improving corrosion resistance, and the outer layer has a lower Ni content, which can provide sufficient soluble metal ions, thereby helping to balance the stability and reactivity of the anode material. In addition, the multilayer structure and the gradient distribution of Ni content are conducive to establishing a potential gradient on the electrode surface, promoting ion transport and electrochemical reactions, and can achieve fine control of the electrochemical process and improve electrolysis efficiency.

[0042] (5) The sintered metal porous material of the present invention has good versatility and can be used for both oxygen evolution reaction and chlorine evolution reaction, and both can be carried out in alkaline electrolyte. It exhibits the advantages of small oxygen evolution overpotential, good voltage stability, good corrosion resistance, etc., and is an anode material that can be widely used.

[0043] (6) The sintering process of the present invention adopts a special heating process. First, it ensures that the phases formed by sufficient sintering are as much as possible intermetallic compounds, and reduces the content of other impurities such as solid solution alloys, carbon single substance, carbides, and carbon oxides, so that the structure is single, the composition is uniform, and the distribution of various constituent elements is uniform without segregation. Second, it ensures that the material does not deform, shrinks or expands in equal proportions, and does not melt locally or bend. Third, it ensures that a large number of pores are generated in the material to increase the specific surface area, thereby improving the reaction efficiency.

[0044] (7) The sintering process of the present invention adopts a special cooling process, which fully considers the phase change and reaction characteristics of Hf-Ni alloy in different temperature ranges. A faster cooling rate is used in the high temperature stage, which is conducive to maintaining the basic shape and dimensional stability of the sintered body and avoiding excessive thermal deformation at high temperature; a slower cooling rate is used in the medium temperature stage, which can reduce thermal stress, promote the diffusion reaction between Ni and Hf, and optimize the organizational structure; a faster cooling rate is used in the low temperature stage, which can not only reduce the long-term heat retention at low temperature, thereby avoiding thermal deformation and organizational coarsening again, but also help to lock the optimized organizational structure that has been formed. Therefore, by regulating the cooling rate, the organizational optimization of the alloy can be promoted while maintaining the shape stability of the sintered body, and finally a sintered metal porous material with good performance is obtained.

[0045] Secondly, the main purpose of the present invention is to provide a water treatment method and a water treatment system to solve the technical problems of long wastewater treatment process and high energy consumption in the prior art.

[0046] In order to achieve the purpose of the second aspect above, the present invention first provides a water treatment method, and the technical scheme is as follows:

[0047] A water treatment method comprising the steps of:

[0048] Pre-treating the wastewater to obtain an electrolyte whose solid content, salt content and pH meet the electrolysis requirements;

[0049] The electrolyte is passed into the electrolytic cell of the electrolytic hydrogen production device for electrolytic treatment to decompose organic matter and ammonia nitrogen in the electrolyte and generate hydrogen;

[0050] Wherein, the anode of the electrolytic hydrogen production device adopts the sintered metal porous material described in the first aspect above.

[0051] As a further improvement of the above water treatment method:

[0052] Treat the wastewater by any of air flotation treatment, filtration treatment, and flocculation sedimentation treatment to obtain an electrolyte with a solid content that meets electrolysis requirements;

[0053] Treat the wastewater by any of softening treatment, membrane separation treatment, ion exchange treatment and electrodialysis treatment to obtain an electrolyte whose salt content meets the electrolysis requirements;

[0054] The wastewater is treated with an acidic or alkaline reagent to obtain an electrolyte whose pH meets the electrolysis requirements.

[0055] As a further improvement of the above water treatment method: the solid content of the electrolyte is ≤1 mg / L, the salt content is ≤15 g / L, and the pH is 12-14.

[0056] As a further improvement of the above water treatment method: it also includes performing membrane separation treatment after the electrolysis treatment.

[0057] In order to achieve the purpose of the second aspect above, the present invention secondly provides a water treatment system, and the technical solution is as follows:

[0058] Water treatment system, including:

[0059] A pretreatment unit, used to pretreat the wastewater to obtain an electrolyte whose solid content, salt content and pH meet the electrolysis requirements;

[0060] An electrolytic hydrogen production unit is used to electrolyze the electrolyte to decompose organic matter and ammonia nitrogen in the electrolyte and produce hydrogen; the electrolytic hydrogen production unit includes an electrolytic hydrogen production device, and the electrolytic hydrogen production device includes an electrolytic cell shell, an anode and a cathode;

[0061] Wherein, the anode of the electrolytic hydrogen production device adopts the sintered metal porous material described in the first aspect above.

[0062] The water treatment method and water treatment system described in the second aspect have the following advantages:

[0063] Firstly, the present invention directly utilizes an electrolytic hydrogen production device to electrolyze the electrolyte. The acid radical ions in the electrolyte lose electrons at the anode and become gas. The gas can be further converted into highly active free radicals such as hydroxyl radical OH, sulfoxide radical SO and chlorine radical Cl, which can deeply oxidize and remove organic matter and ammonia nitrogen. At the same time, water undergoes a reduction reaction at the cathode to generate clean energy hydrogen, which can generate more economic benefits. Green electricity can fully meet the demand with low electricity bills. Therefore, the overall economic benefits can be significantly improved while purifying the water body.

[0064] Secondly, the present invention can achieve a higher electrolysis efficiency by controlling the solid content, salt content and pH of the wastewater only through pretreatment before electrolysis. There is no need for a complicated, time-consuming, high-energy consumption and space-consuming pretreatment process. The overall water consumption is small, the cost of chemicals and subsequent treatment costs are saved, and no other metal ions are introduced.

[0065] It has been verified that the water treatment method and water treatment system of the present invention can reduce the concentrations of COD, BOD, and ammonia nitrogen in the electrolyte to meet the emission standards, and can improve the subsequent valuable resource recovery efficiency and / or impurity removal efficiency.

[0066] On the third aspect, the main purpose of the present invention is to provide a treatment system for paint production wastewater to solve the technical problems of long process and high energy consumption in the prior art for paint production wastewater treatment.

[0067] A treatment system for paint production wastewater includes: a filtration unit connected in sequence, the filtration unit is used to filter the paint production wastewater and output a first liquid; a flocculation and sedimentation unit, the flocculation and sedimentation unit is used to flocculate and sediment the first liquid and output a second liquid; the flocculation and sedimentation unit includes a first regulating tank and a first sedimentation tank connected in sequence, and a reagent dosing component is provided in the first regulating tank; a softening unit, the softening unit is used to soften the second liquid and output an electrolyte; the softening unit includes a second regulating tank and a second sedimentation tank, and a first alkali solution dosing device is provided in the second regulating tank; an electrolytic hydrogen production unit, the electrolytic hydrogen production unit is used to electrolyze the electrolyte and output a third liquid; the electrolytic hydrogen production unit includes an electrolytic hydrogen production device.

[0068] As a further improvement of the above-mentioned system for treating paint production wastewater: the filtering unit includes a grid and an ultrafiltration device connected in sequence.

[0069] As a further improvement of the above-mentioned system for treating paint production wastewater: the flocculation and sedimentation unit also includes a first filter press device.

[0070] As a further improvement of the above-mentioned system for treating paint production wastewater: there are two first sedimentation tanks.

[0071] As a further improvement of the above-mentioned coating production wastewater treatment system: the reagent dosing component includes a PAC dosing device, a PAM dosing device and a demulsifier dosing device.

[0072] As a further improvement of the above-mentioned system for treating paint production wastewater: a first pH detection device is also provided in the second regulating tank.

[0073] As a further improvement of the above-mentioned system for treating paint production wastewater: the softening unit also includes a second filter press device.

[0074] As a further improvement of the above-mentioned coating production wastewater treatment system: it also includes a pH adjustment unit, which includes a third adjustment tank, a second pH detection device, a second alkali solution dosing device and an acid solution dosing device, and the third adjustment tank is used to store electrolyte and output electrolyte to the electrolytic hydrogen production unit.

[0075] As a further improvement of the above-mentioned system for treating paint production wastewater: it also includes a reverse osmosis membrane device for performing membrane separation treatment on the third liquid.

[0076] The coating production wastewater treatment system described in the third aspect has the following advantages:

[0077] The traditional treatment system for paint production wastewater adopts Fenton oxidation treatment first and then biochemical treatment (hydrolysis acidification + UBF + two-stage A / O). The biochemical unit has a large load and it is difficult to deeply remove pollutants in the water.

[0078] The treatment system of the present invention uses an electrolytic hydrogen production device to replace the complex Fenton oxidation treatment and biochemical treatment, which not only significantly reduces the investment and operating costs, but also effectively removes organic matter and ammonia nitrogen and generates hydrogen resources, which is green and environmentally friendly and has significantly improved economic benefits. Before the electrolytic hydrogen production device, only the filtration unit, flocculation sedimentation unit and softening unit are used to meet the electrolysis requirements, which occupies a small area and has a low investment cost. It can be seen that compared with the traditional treatment system, the treatment system of the present invention has a simple structure, significantly reduces the area, energy consumption and dosage of reagents, significantly improves the economic benefits and environmental protection, and has significantly stronger practicality.

[0079] The embodiments of the invention provided in this specification are further described below in conjunction with the accompanying drawings and specific implementation methods. Additional aspects and advantages of the embodiments of the invention provided in this specification will be partially given in the following description, and partially will become apparent from the following description, or will be understood through the practice of the embodiments of the invention provided in this specification. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] The drawings that constitute part of the embodiments of the inventions provided in this specification are used to assist in understanding the embodiments of the inventions provided in this specification. The contents provided in the drawings and their related descriptions in the embodiments of the inventions provided in this specification can be used to explain the embodiments of the inventions provided in this specification, but do not constitute improper limitations on the embodiments of the inventions provided in this specification.

[0081] Figure 1 This is a SEM photo of the sintered porous metal material according to an embodiment of the present invention.

[0082] Figure 2 This is an energy dispersive X-ray spectrum of the first metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention.

[0083] Figure 3 FIG. 1 is an energy dispersive X-ray spectrum of the second metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention.

[0084] Figure 4This is an energy dispersive X-ray spectrum of the third metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention.

[0085] Figure 5 This is an energy dispersive X-ray spectrum of white spots in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention.

[0086] Figure 6 This is an X-ray diffraction pattern of the sintered metal porous material according to an embodiment of the present invention.

[0087] Figure 7 1 is the anodic polarization curve of the sintered porous metal material according to an embodiment of the present invention.

[0088] Figure 8 This is the anode constant current polarization stability curve of the sintered metal porous material according to an embodiment of the present invention.

[0089] Fig. 9 It is a schematic diagram of the structure of a system for treating paint production wastewater according to an embodiment of the present invention. DETAILED DESCRIPTION

[0090] The following is a clear and complete description of the embodiments of the inventions provided in this specification in conjunction with the accompanying drawings. A person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification based on these descriptions. Before describing the embodiments of the inventions provided in this specification in conjunction with the accompanying drawings, it should be particularly noted that:

[0091] The technical solutions and technical features provided in each part of the embodiments of the invention provided in this specification, including the following description, may be combined with each other if there is no conflict.

[0092] In addition, the embodiments of the embodiments of the inventions provided in this specification involved in the following description are generally only a partial embodiment of the embodiments of the inventions provided in this specification rather than all the embodiments. Therefore, based on the embodiments of the embodiments of the inventions provided in this specification, all other embodiments obtained by ordinary technicians in this field without making any creative work should fall within the scope of protection of the embodiments of the inventions provided in this specification.

[0093] Regarding the terms and units in the embodiments of the inventions provided in this specification: The terms "including", "comprising", "having" and any variations thereof in the descriptions and claims of the embodiments of the inventions provided in this specification and in the related parts are intended to cover non-exclusive inclusions. In addition, other relevant terms and units in the embodiments of the inventions provided in this specification can be reasonably interpreted based on the relevant contents of the embodiments of the inventions provided in this specification.

[0094] Figure 1 This is a SEM photo of the sintered porous metal material according to an embodiment of the present invention.

[0095] like Figure 1 As shown, the sintered metal porous material of the present invention has three metal layers and a layered structure formed by them, and the materials in the three metal layers are uniform; the three metal layers are all composed of Ni elements and Hf elements, and the proportions of Ni elements and Hf elements in the three metal layers are different. The three metal layers are respectively a first metal layer, a second metal layer wrapping the first metal layer, and a third metal layer wrapping the second metal layer, and the first metal layer is multiple and arranged at intervals. The sintered metal porous material also has white spots, which are discretely distributed in the three metal layers.

[0096] Figure 2 This is an energy dispersive X-ray spectrum of the first metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention. Figure 3 FIG. 1 is an energy dispersive X-ray spectrum of the second metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention. Figure 4 This is an energy dispersive X-ray spectrum of the third metal layer in the SEM photograph of the sintered metal porous material according to an embodiment of the present invention. Figure 5 The energy dispersive X-ray spectrum of the white spot in the SEM photo of the sintered metal porous material according to the embodiment of the present invention is shown in Table 1. The atomic concentrations of the first metal layer, the second metal layer, the third metal layer and the white spot are shown in Table 1.

[0097] Table 1

[0098] Element Symbols First metal layer Second metal layer The third metal layer White spots Ni 54.60% 41.63% 35.17% 0 Hf 45.40% 58.37% 64.83% 100%

[0099] like Figure 2-5 As shown in Table 1, the Ni element content is: the first metal layer> the second metal layer> the third metal layer, and the white spots are Hf alone.

[0100] Figure 6 This is an X-ray diffraction pattern of the sintered metal porous material according to an embodiment of the present invention.

[0101] like Figure 6 As shown, the XRD spectrum of the sintered metal porous material contains phases including HfNi3 intermetallic compound, Hf3Ni7 intermetallic compound, Hf single substance and Ni single substance, wherein the single substance phase content is very small and does not contain a solid solution alloy phase.

[0102] The method for preparing the sintered porous metal material according to the embodiment of the present invention comprises the following steps:

[0103] (1) Ni powder and Hf powder are ball-milled to obtain a mixed powder; wherein the particle sizes of the Ni powder and the Hf powder are both 3-5 μm, the mass ratio of the Ni powder to the Hf powder is 44:56, and the ball milling time is 12 h.

[0104] (2) Adding a forming aid to the mixed powder, followed by granulation and sieving to obtain formed particles; wherein the forming aid is PVB (polyvinyl butyral), the amount of the forming aid is 4% of the mass of the mixed powder, and a 60-mesh screen is used for sieving.

[0105] (3) Pressing the formed particles into a green body; wherein, under a pressure of 200 MPa, the pressing time is controlled to be 50 seconds and the holding time is controlled to be 70 seconds, that is, 2 g of the formed particles are pressed into a rectangular green body with a size of 25*8*2 mm.

[0106] (4) performing a staged heating and sintering treatment on the green body;

[0107] (5) The green body is subjected to a staged cooling treatment to obtain a sintered metal porous material.

[0108] The staged heating sintering process is carried out under vacuum, and the heating process is as follows: heating from room temperature to sintering temperature, keeping the temperature for 40 to 80 minutes after each 50 to 150°C heating, and keeping the temperature for 150 to 200 minutes after reaching the sintering temperature. The sintering temperature is 1250 to 1350°C, and the heating rate for each heating is 4 to 7°C / min. Specifically, the staged heating sintering process is as follows:

[0109] The first stage is to heat from room temperature to 400°C and keep it for 60 minutes;

[0110] The second stage is to continue heating to 500℃ and keep it for 60min;

[0111] The third stage is to continue heating to 600℃ and keep it for 60min;

[0112] The fourth stage is to continue heating to 700℃ and keep it for 60min;

[0113] The fifth stage is to continue heating to 800°C and keep warm for 60 minutes;

[0114] The sixth stage is to continue heating to 900°C and keep it for 60 minutes;

[0115] The seventh stage is to continue heating to 1000°C and keep warm for 60 minutes;

[0116] The eighth stage is to continue heating to 1100°C and keep warm for 60 minutes;

[0117] The ninth stage is to continue heating to 1300°C and keep it warm for 18 minutes.

[0118] The segmented cooling process is carried out under vacuum, and the cooling process is as follows:

[0119] The first stage is to cool down from the sintering temperature to 800-9000℃, with a cooling rate of 10-15℃ / min;

[0120] The second stage is to continue cooling to 400-500°C, with a cooling rate of 4-7°C / min;

[0121] The third stage is to continue cooling to below 100°C at a cooling rate of 15-20°C / min, thereby obtaining a sintered metal porous material.

[0122] The embodiment of the electrolytic hydrogen production device of the present invention comprises an anode, and the anode is made of the above-mentioned sintered metal porous material.

[0123] The embodiment of the method for producing hydrogen by electrolysis of the present invention is to use the above-mentioned hydrogen production by electrolysis device to electrolyze alkaline water.

[0124] In order to verify the electrochemical performance of the sintered porous metal material of the embodiment of the present invention, an electrochemical workstation was used to test the electrochemical performance of the material, as follows:

[0125] The working electrode of the three-electrode system used is the prepared sintered metal porous material (referred to as NiHf electrode), the reference electrode is a mercury / mercury oxide electrode, the reference electrode is aligned with the center of the working electrode test surface through a Lu capillary (salt bridge) and is 1-2 mm apart, the auxiliary electrode is a platinum sheet (10mm×10mm×0.2mm), and it is carried out in a 1M KOH solution (pH 14). Before the electrochemical test, the working electrode is sealed, and the working electrode surface exposes a working area of ​​0.64 square centimeters. The non-working surface is encapsulated with waterproof raw tape and 704 silicone rubber, which ensures that the current value automatically collected by the computer is the required current density. All electrochemical test data are carried out in a constant temperature water bath. Before the effective data test, the open circuit potential of the working electrode is measured by the three-electrode test method. The open circuit potential of the NiHf electrode is stable at about -0.574V within 30 minutes. After the open circuit potential is stable, the electrode is tested for corresponding data.

[0126] The anode overpotential test process is as follows: select the stable value of the open circuit potential as the first vertex potential, and the value of the open circuit potential rising by 2V as the second vertex potential, that is, the polarization test range is 2V, the scanning rate is 4mV / s, the electrolytic cell parameters select the reference electrode parameters corresponding to mercury / mercury oxide, and then start the test.

[0127] Figure 7 : is the anodic polarization curve of the sintered metal porous material of the embodiment of the present invention. Figure 7As shown, NiHf electrode at 10mA / cm 2 The overpotential is 313 mV, which is close to the data of the commercial Pt / C electrode, indicating that the NiHf electrode of the present invention has excellent oxygen evolution performance when used as an anode in a strong alkaline electrolyte.

[0128] The anode constant current polarization stability test process is as follows: select the constant current polarization mode test and set the constant current density to 100mA / cm 2 The polarization time is 12h. The potential of the sample is tested for a long time and the state of the sample is observed at the same time.

[0129] Figure 8 : is the anode constant current polarization stability curve of the sintered metal porous material of the embodiment of the present invention. Figure 8 As shown, the voltage fluctuation of the NiHf electrode does not exceed 6.84%, indicating that the oxygen evolution performance of the NiHf electrode of the present invention as an anode material in a strong alkaline electrolyte remains stable.

[0130] The corrosion resistance test is as follows: the open circuit potential in 1M KOH is used to represent the material. The more positive the potential value, the better the corrosion resistance of the material. After testing, the corrosion resistance potential of the NiHf electrode is -0.574V, which has good corrosion resistance.

[0131] The above results show that the sintered metal porous material of the embodiment of the present invention has the advantages of small overpotential, good voltage stability, good corrosion resistance, etc. when used as an anode in a strong alkaline solution, and is a widely used anode material for electrolytic hydrogen production devices.

[0132] The water treatment method according to the embodiment of the present invention comprises the following steps:

[0133] Treat the wastewater by any of flotation treatment, filtration treatment, and flocculation sedimentation treatment to obtain an electrolyte whose solid content meets the electrolysis requirements; the solid content of the electrolyte is ≤1mg / L;

[0134] Treat the wastewater by any of softening treatment, membrane separation treatment, ion exchange treatment and electrodialysis treatment to obtain an electrolyte whose salt content meets the electrolysis requirements; the salt content of the electrolyte is ≤15g / L;

[0135] Treating wastewater with an acidic or alkaline reagent to obtain an electrolyte whose pH meets electrolysis requirements; the pH of the electrolyte is 12 to 14;

[0136] The electrolyte is passed into the electrolytic cell of the electrolytic hydrogen production device for electrolytic treatment to decompose organic matter and ammonia nitrogen in the electrolyte and generate hydrogen;

[0137] The electrolysis treatment is followed by membrane separation treatment.

[0138] The water treatment system of the embodiment of the present invention comprises:

[0139] A pretreatment unit, used to pretreat the wastewater to obtain an electrolyte whose solid content, salt content and pH meet the electrolysis requirements;

[0140] An electrolytic hydrogen production unit is used to electrolyze the electrolyte to decompose organic matter and ammonia nitrogen in the electrolyte and produce hydrogen; the electrolytic hydrogen production unit includes an electrolytic hydrogen production device, and the electrolytic hydrogen production device includes an electrolytic cell shell, an anode and a cathode;

[0141] In the above-mentioned water treatment method and water treatment system, the electrolysis hydrogen production device adopts a wastewater electrolysis hydrogen production device with the application number of 2023117301217 published in the Chinese invention patent.

[0142] The following are application examples of the water treatment method and water treatment system of the present invention.

[0143] The wastewater generated by three large paint factories was collected. The wastewater mainly comes from the reaction water in the resin production process and the cleaning water generated by the cleaning equipment, pipelines and finished product tanks in the production process. The water quality parameters are shown in Table 2-4 below.

[0144] It can be seen from Table 2-4 that the COD of the three types of paint production wastewater is relatively high, and some also contain high levels of BOD and ammonia nitrogen, all of which are high-concentration organic wastewater.

[0145] Table 2. Water quality parameters of wastewater discharge from a coating factory 1

[0146]

[0147] Table 3. Water quality parameters of wastewater discharge from a paint factory 2

[0148] category pH COD(mg / L) BOD(mg / L) SS(mg / L) Resin and curing agent wastewater 2.5~3.0 200000 40000 ≤500 Building paint wastewater 6~7 20000 2000 =10000 Comprehensive wastewater 6~9 8000~10000 2000~4000 ≤200

[0149] Table 4. Water quality parameters of wastewater discharge from a coating factory 3

[0150]

[0151] Fig. 9 It is a schematic diagram of the structure of a system for treating paint production wastewater according to an embodiment of the present invention.

[0152] like Fig. 9 As shown, the treatment system for coating production wastewater includes a filtration unit 100, a flocculation and sedimentation unit 200, a softening unit 300, a pH adjustment unit 400, an electrolytic hydrogen production unit 500 and a membrane separation unit 600 which are connected in sequence.

[0153] The filtering unit 100 is used to filter the paint production wastewater and output a first liquid; the filtering unit 100 includes a grid and an ultrafiltration device connected in sequence.

[0154] The flocculation and sedimentation unit 200 is used to perform flocculation and sedimentation treatment on the first liquid output by the filtration unit 100 and output a second liquid; the flocculation and sedimentation unit 200 includes a first regulating tank, a first sedimentation tank and a first filter press connected in sequence; a reagent dosing component is provided in the first regulating tank; there are two first sedimentation tanks, and the supernatant in the second-stage sedimentation tank is the second liquid; the reagent dosing component includes a PAC dosing device, a PAM dosing device and a demulsifier dosing device; the liquid filtered by the first filter press is refluxed to the water inlet end of the grid, and the solid residue obtained enters the solid waste treatment unit.

[0155] The softening unit 300 is used to soften the second liquid output by the flocculation and sedimentation unit 200 and output an electrolyte; the softening unit 300 includes a second regulating tank, a second sedimentation tank and a second filter press; the second regulating tank is provided with a first alkali solution dosing device and a first pH detection device; the supernatant in the second sedimentation tank is an electrolyte; the liquid filtered by the second filter press flows back to the water inlet end of the grid, and the obtained solid residue enters the solid waste treatment unit.

[0156] The pH adjusting unit 400 is used to adjust the pH of the electrolyte output by the softening unit 300; the pH adjusting unit 400 includes a third adjusting tank, a second pH detection device, a second alkali solution adding device and an acid solution adding device, and the third adjusting tank is used to store the electrolyte and output the electrolyte with the pH meeting the requirements to the electrolytic hydrogen production unit 500. When the second pH detection device detects that the pH of the electrolyte does not meet the requirements of 12 to 14, the second alkali solution adding device or the acid solution adding device can be used to add alkali solution or acid solution for adjustment.

[0157] The electrolytic hydrogen production unit 500 is used to electrolyze the electrolyte output by the pH adjustment unit 400 and output a third liquid.

[0158] The membrane separation unit 600 is used to perform membrane separation treatment on the third liquid output from the electrolytic hydrogen production unit 500. The membrane separation unit 600 includes a reverse osmosis membrane device, thereby further intercepting pollutants and obtaining a clear liquid that can be reused.

[0159] It has been verified that the paint production wastewater treatment system can treat the above three types of paint production wastewater and make the COD, BOD and ammonia nitrogen meet the "Comprehensive Sewage Discharge Standard" (GB 8978-1996).

[0160] Among the above pollutants:

[0161] SS (Suspended Solids) refers to solid matter suspended in water, including inorganic and organic matter insoluble in water, mud, clay, microorganisms, etc. It is one of the indicators to measure the degree of water pollution.

[0162] COD (Chemical Oxygen Demand) is the chemical oxygen demand, which refers to the amount of reducing substances that need to be oxidized in a water sample measured by chemical methods.

[0163] BOD (Biochemical Oxygen Demand) is the biochemical oxygen demand, which refers to the amount of dissolved oxygen consumed by microorganisms to decompose certain oxidizable substances (especially organic substances) in a certain volume of water within a certain period of time.

[0164] Ammonia nitrogen refers to combined nitrogen in the form of ammonia or ammonium ions, that is, free ammonia (NH3) and ammonium ions (NH4 + ) in the form of nitrogen.

[0165] The above is a description of the relevant contents of the embodiments of the inventions provided in this specification. Based on these descriptions, a person of ordinary skill in the art will be able to implement the embodiments of the inventions provided in this specification. Based on the above contents of the embodiments of the inventions provided in this specification, all other preferred implementations and embodiments obtained by a person of ordinary skill in the art without making any creative work shall fall within the scope of protection of the embodiments of the inventions provided in this specification.

Claims

1. Sintered metal porous material, characterized in that: The invention comprises three metal layers and a layered structure formed by the three metal layers. The three metal layers are all formed by Ni element and Hf element. The proportions of Ni element and Hf element in the three metal layers are different.

2. The sintered metal porous material according to claim 1, characterized in that: The phases in the XRD spectrum of the sintered metal porous material include HfNi3 intermetallic compound, Hf3Ni7 intermetallic compound, Hf single substance and Ni single substance.

3. The sintered metal porous material according to claim 1, characterized in that: The sintered metal porous material comprises a first metal layer, a second metal layer wrapping the first metal layer and a third metal layer wrapping the second metal layer, and the Ni element content is as follows: the first metal layer>the second metal layer>the third metal layer.

4. The sintered metal porous material according to claim 3, characterized in that: The first metal layers are multiple and arranged at intervals.

5. The method for preparing the sintered porous metal material according to any one of claims 1 to 4, characterized in that: Includes steps: The Ni powder and the Hf powder are ball-milled to obtain a mixed powder; Adding a forming aid to the mixed powder, followed by granulation and sieving to obtain formed particles; Pressing the formed particles into a shape to obtain a green body; The green body is subjected to staged temperature-raising sintering treatment; The green body is subjected to a staged cooling treatment to obtain a sintered metal porous material.

6. The method for preparing a sintered porous metal material according to claim 5, characterized in that: The staged heating sintering treatment is carried out under vacuum, and the heating process is specifically as follows: heating from room temperature to sintering temperature, keeping the temperature for 40 to 80 minutes after each heating of 50 to 150°C, and keeping the temperature for 150 to 200 minutes after reaching the sintering temperature. The sintering temperature is 1250 to 1350°C, and the heating rate of each heating is 4 to 7°C / min.

7. The method for preparing a sintered porous metal material according to claim 6, characterized in that: The staged heating sintering process is as follows: The first stage is to heat from room temperature to 400°C and keep it for 60 minutes; The second stage is to continue heating to 500℃ and keep it for 60min; The third stage is to continue heating to 600℃ and keep it for 60min; The fourth stage is to continue heating to 700℃ and keep it for 60min; The fifth stage is to continue heating to 800°C and keep warm for 60 minutes; The sixth stage is to continue heating to 900°C and keep it for 60 minutes; The seventh stage is to continue heating to 1000°C and keep warm for 60 minutes; The eighth stage is to continue heating to 1100°C and keep warm for 60 minutes; The ninth stage is to continue heating to 1300°C and keep it warm for 18 minutes.

8. The method for preparing a sintered porous metal material according to claim 5, characterized in that: The segmented cooling process is carried out under vacuum, and the cooling process is as follows: The first stage is to cool down from the sintering temperature to 800-9000℃, with a cooling rate of 10-15℃ / min; The second stage is to continue cooling to 400-500°C, with a cooling rate of 4-7°C / min; The third stage is to continue cooling to below 100°C at a cooling rate of 15-20°C / min, thereby obtaining a sintered metal porous material.

9. An electrolytic hydrogen production device having an anode, characterized in that: The anode is a sintered metal porous material as claimed in any one of claims 1 to 4, or a sintered metal porous material prepared by the preparation method as claimed in any one of claims 5 to 8.

10. A method for producing hydrogen by electrolysis, characterized in that: The electrolytic hydrogen production device according to claim 9 is used to electrolyze alkaline water.