Improved powder forming porous copper heat dissipation material based on surface composite copper net and preparation method of improved powder forming porous copper heat dissipation material
By pressing the multi-layer copper mesh on the porous copper surface to form a composite gradient structure, the problems of insufficient material strength and difficulty in steam separation in thermal management of porous structures are solved, and higher boiling and convective heat exchange performance are achieved, and thermal management efficiency is improved. And reduce production costs.
Patent Information
- Application Number
- CN202410998302.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-08
AI Technical Summary
The existing porous structures have problems such as insufficient material strength, easy deformation and difficulty in steam disengagement in thermal management, which limits their effectiveness and efficiency in practical applications.
By pressing a multi-layer copper mesh on the porous copper surface, a composite gradient structure is formed, the bubble disengagement rate and boiling heat exchange coefficient are improved, the peak value of the convective heat exchange coefficient is increased, and the heat exchange efficiency is improved.
Higher boiling heat exchange performance and convection heat exchange efficiency are achieved, the initial overheat is reduced, the heat flow density value is improved, the preparation process is simplified and the production cost is reduced.
Smart Images

Figure CN118905227A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material synthesis methods, and specifically relates to an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh and a preparation method thereof. Background Art
[0002] Heat transfer processes are widely present in nature and engineering, especially in the field of electronic information. However, due to factors such as smaller size, faster operation speed, higher packaging density, and higher working power, the heat generation and heat flux density in electronic devices increase dramatically, resulting in higher temperatures. When electronic devices exceed the rated temperature, many negative effects will occur, and even damage will occur. Therefore, effective thermal management of electronic devices restricts the rapid development of industry, and the development of efficient heat dissipation technology is imminent. Porous structure design is a common passive strengthening method. Tang et al. and Lu et al. prepared nanoporous copper surfaces with pore sizes between 50 and 200 nanometers using a hot dip galvanizing / alloying process. The results showed that the initial superheat was reduced by 63.3% and the boiling Heat Transfer Coefficient (HTC) value was increased by 172.7%. Manetti et al. found that compared with ordinary smooth surfaces, foam copper surfaces can better absorb and diffuse fluids, thereby enhancing boiling heat transfer. Yang et al. studied the boiling heat transfer performance of welding foam copper to a copper heating substrate. The study found that compared with the smooth copper boiling surface, the copper foam reduced the initial superheat and reduced the starting point of nucleate boiling with water as the liquid working fluid. Manetti et al. studied the pool boiling heat transfer of ultra-light porous foam metal surfaces using deionized water as the working fluid and found that the boiling heat transfer coefficient of the metal foam surface was about 2 to 3 times that of the ordinary surface. Xu et al. studied the boiling heat transfer performance of the sintered copper powder surface and the smooth surface. Due to the increase in nucleation sites, the sintered surface has better performance in nucleate boiling.
[0003] At present, a lot of research results have been obtained on porous structures such as foam metal, powder sintering and porous wire mesh in enhancing boiling heat transfer. However, these porous structures have their own limitations. For foam metal, although its large heat transfer area is conducive to heat transfer, the pore size is relatively large due to the limitation of the preparation process. The porous wire mesh provides abundant nucleation sites for boiling heat transfer with its tiny mesh. However, it has problems such as relatively small heat transfer area, insufficient material strength and easy deformation, which limit its application in actual production and life. In contrast, the dense pores of the powder sintering porous structure not only provide a large number of nucleation sites for boiling, but also the tiny pores formed during the sintering process are not available in foam metal. However, its dense pores bring a large number of nucleation sites for boiling, but also seriously hinder the detachment of steam. In response to this problem, at present, the focus at home and abroad is mainly on enhancing its heat transfer performance by constructing different geometric structures on its surface to separate gas and liquid and promote the detachment of steam. However, this method is complex and the enhancement effect is still poor. Summary of the invention
[0004] The purpose of the present invention is to provide an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh and a preparation method thereof. The preparation method is simple, the raw materials are inexpensive, and the production cost can be reduced. The bubble detachment rate and boiling heat transfer coefficient can be increased by pressing multiple layers of copper mesh on the porous copper surface, and the heat flux density value corresponding to the peak value of the convection heat transfer coefficient can be increased, thereby enhancing the heat exchange efficiency.
[0005] To achieve the above object, the present invention is implemented by the following technical solutions:
[0006] A method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh comprises the following steps:
[0007] (1) cutting the copper mesh into copper mesh discs according to the specification requirements, then ultrasonically cleaning the copper mesh discs with anhydrous ethanol to remove oil stains, then using hydrochloric acid to remove oxides, then rinsing with deionized water and vacuum drying the copper mesh discs;
[0008] (2) using sodium chloride particles as a pore-forming agent, drying the sodium chloride particles and mixing them with electrolytic copper powder in a certain ratio in a ball mill to obtain a copper salt mixture;
[0009] (3) placing a certain mass of the copper salt mixture into a stainless steel mold, first manually compacting it to form a loose structure, then laying multiple layers of copper mesh on the loose structure, and finally pressing and forming a pressed sheet; the multiple layers of copper mesh are copper meshes of the same mesh number or copper meshes of different mesh numbers. When the multiple layers of copper mesh are copper meshes of different mesh numbers, they are laid on the surface of the loose structure in order from small to large mesh numbers and from top to bottom to form a composite gradient copper mesh;
[0010] (4) The pressed tablets obtained in step (3) are sequentially vacuum sintered, cleaned, and dried to obtain an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh.
[0011] Preferably, in step (3), the multi-layer copper mesh is two layers; the two layers of copper mesh are both 80 mesh copper mesh, or one layer of 60 mesh copper mesh and one layer of 80 mesh copper mesh, or one layer of 80 mesh copper mesh and one layer of 100 mesh copper mesh.
[0012] Preferably, in step (3), the multi-layer copper mesh is a layer of 60-mesh copper mesh and a layer of 80-mesh copper mesh.
[0013] Preferably, in step (2), the sodium chloride particles are sieved through an 80-mesh sieve; and the sodium chloride particles are dried in a vacuum drying oven at 50°C.
[0014] Preferably, in step (2), the particle size of the electrolytic copper powder is 5 μm; and the mass ratio of the dried sodium chloride particles to the electrolytic copper powder is 1:(4-5).
[0015] Preferably, in step (2), the dried sodium chloride particles are placed in a grinding jar together with the electrolytic copper powder, and then the grinding jar is placed in a planetary ball mill for thorough mixing; the ball milling time is 25-35 min, and the rotation speed is 150-180 rpm.
[0016] Preferably, in step (3), the tablet is finally pressed by a tablet press to obtain a tablet, the tablet press is set to a pressure of 240-280 MPa, and the holding time is 180-200 s.
[0017] Preferably, in step (4), the pressed tablet is placed in a tubular furnace for vacuum sintering, the heating rate is 8-12°C / min, and the sintering temperature is 650-850°C.
[0018] Preferably, in step (1), the diameter of the copper mesh disc is 30 mm and the concentration of hydrochloric acid is 0.1 mol / L.
[0019] To achieve the above object, the present invention also provides an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh prepared by the above preparation method.
[0020] The present invention presses a multi-layer copper mesh onto a powder-molded porous copper sheet with optimal heat transfer. When the porous copper surface is compounded with a double-layer copper mesh, the arrangement order of the copper mesh affects the performance of the sample. The newly added vaporization cores between the copper meshes and the resistance to bubble escape jointly determine the boiling heat transfer performance of the sample. When the powder-molded porous copper surface is compounded with 60-mesh and 80-mesh copper meshes from top to bottom, its boiling heat transfer performance reaches the best. This is because a structure similar to a "micro chimney" is formed between the 80-mesh copper mesh and the 60-mesh copper mesh. This structure effectively accelerates the detachment of bubbles, thereby improving the heat exchange efficiency. Its ONB is 1.2°C and the maximum heat transfer coefficient is 69301W·m -2 ·K -1 , which is 1.4 times that of porous copper in uncompounded copper mesh.
[0021] Compared with the prior art, the preparation method of the present invention is simple, the raw materials are cheap, and the production cost is reduced; by pressing multiple layers of copper mesh on the porous copper surface to increase the bubble detachment rate and boiling heat transfer coefficient, the heat flux density value corresponding to the peak value of the convection heat transfer coefficient is increased, thereby enhancing the heat exchange efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The microstructure diagrams of powder-formed porous copper composites with different copper meshes are shown in (a) Comparative Example 2 and (b) Example 1.
[0023] Figure 2 are microstructure diagrams under optical mode, (a) embodiment 2, (b) embodiment 1;
[0024] Figure 3 Pool boiling heat transfer curves prepared from samples of comparative examples 1 to 4, (a) curve of heat flux density changing with wall superheat, (b) curve of heat transfer coefficient changing with heat flux density;
[0025] Figure 4 Pool boiling heat transfer curves of samples prepared in Comparative Example 1, Comparative Example 2, and Example 1, (a) curve of heat flux density changing with wall superheat, (b) curve of heat transfer coefficient changing with heat flux density;
[0026] Figure 5 Pool boiling heat transfer curves of samples prepared in comparative example 1, example 1, example 2 and example 3, (a) curve of heat flux density changing with wall superheat, (b) curve of heat transfer coefficient changing with heat flux density. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] Comparative Example 1
[0029] A method for preparing a powder-molded porous copper heat dissipation material comprises the following steps:
[0030] (1) Sodium chloride particles sieved through an 80-mesh sieve are used as pore-forming agents. The sodium chloride particles are placed in a vacuum drying oven at 50° C. and dried. After drying, 1.14 g of the sodium chloride particles are weighed and placed in a grinding jar together with electrolytic copper powder with a particle size of 5 μm and a mass of 4.73 g. The grinding jar is then placed in a planetary ball mill for thorough mixing to obtain a copper salt mixture. The ball milling time is 30 min and the rotation speed is 160 rpm.
[0031] (2) Weigh 5 g of the copper salt mixture and put it into a stainless steel mold, and press it into a powder-molded porous copper tablet.
[0032] The tablet was tested to have a thickness of 1.5 mm and a porosity of 50%. The boiling onset temperature (ONB) of the tablet reached 1.6°C and the heat transfer performance was up to 49407 W·m -2 ·K -1 , which is 3 times that of smooth copper under the same heat flux density, and 1.25-2 times that of foam copper under the same thickness.
[0033] Comparative Example 2
[0034] A method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite single-layer copper mesh comprises the following steps:
[0035] (1) Cut the copper mesh into a copper mesh disc with a diameter of 30 mm according to the specification requirements, then use anhydrous ethanol ultrasonic cleaning to remove oil stains, then use 0.1 mol / L hydrochloric acid to remove oxides, then rinse with deionized water and vacuum dry the copper mesh disc;
[0036] (2) Sodium chloride particles sieved through an 80-mesh sieve were used as pore-forming agents. The sodium chloride particles were placed in a vacuum drying oven at 50° C. and dried. After drying, 1.14 g of the sodium chloride particles were weighed and placed in a grinding jar together with electrolytic copper powder with a particle size of 5 μm and a mass of 4.73 g. The grinding jar was then placed in a planetary ball mill for thorough mixing to obtain a copper salt mixture. The ball milling time was 30 min and the rotation speed was 160 rpm.
[0037] (3) Weigh 5 g of the copper salt mixture and put it into a stainless steel mold. First, manually compact it to form a loose structure. Then, lay a layer of 60-mesh copper mesh on the loose structure. Finally, press it into a tablet by a tablet press. The tablet press is set to a pressure of 250 MPa and a holding time of 180 s.
[0038] (4) placing the pressed tablet obtained in step (3) into a tubular furnace for vacuum sintering to improve the structural strength of the pressed sample, with a heating rate of 10°C / min and a sintering temperature of 750°C; waiting for the tubular furnace to cool naturally to room temperature, then taking out the sample, placing the taken sample in an ultrasonic cleaning machine, first ultrasonically cleaning it with deionized water and anhydrous ethanol until no white particles are precipitated on the surface of the sample when cleaning with anhydrous ethanol; after cleaning, moving the sample to a drying oven for vacuum drying for 4 hours; after drying, weighing the sample mass using an electronic balance and comparing it with the mass of the electrolytic copper powder initially used in step (2); if the mass difference between the two is within 3%, the cleaning and drying steps are completed, otherwise, ultrasonic cleaning and drying treatment shall be continued until the quality requirements are met to obtain an improved powder-molded porous copper heat dissipation material based on a surface composite single-layer copper mesh.
[0039] Figure 1 (a) is a SEM image of the heat dissipation material prepared by laying a single layer of 80-mesh copper mesh on a loose structure. It can be seen from the figure that the copper mesh is tightly bonded to the porous copper surface, which greatly reduces the contact thermal resistance between the porous copper and the copper mesh. At the same time, after the copper mesh has undergone cold pressing, its grid line structure remains relatively intact and the pore size distribution is also very uniform, which indicates that the cold pressing process has not caused significant damage to the grid structure of the copper mesh. In addition, the wire diameter of the copper mesh after pressing has increased and the pore size has decreased, which increases the contact area between the copper mesh and the porous copper, which has a positive effect on improving the boiling heat transfer performance.
[0040] Comparative Example 3
[0041] The difference between this comparative example and comparative example 2 lies in step (3). Step (3) in this comparative example is to lay a layer of 80-mesh copper mesh on the loose structure, and the other steps remain the same as comparative example 2.
[0042] Comparative Example 4
[0043] The difference between this comparative example and comparative example 2 lies in step (3). Step (3) in this comparative example is to lay a layer of 100-mesh copper mesh on the loose structure, and the other steps remain the same as those of comparative example 2.
[0044] like Figure 3 As shown in the figure, when a layer of copper mesh with different meshes is added to the porous copper surface, the boiling starting point is further reduced under the same heat flux density, the boiling heat transfer coefficient is improved, and the heat flux density corresponding to the peak value of the convection heat transfer coefficient is increased. 5 W·m -2 When the heat flux density is higher than that, the heat transfer characteristics of the porous copper with a single-layer composite 80-mesh copper mesh are generally higher than those of the porous copper with 60 and 100 meshes.
[0045] Embodiment 1
[0046] A method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh comprises the following steps:
[0047] (1) Cut the copper mesh into a copper mesh disc with a diameter of 30 mm according to the specification requirements, then use anhydrous ethanol ultrasonic cleaning to remove oil stains, then use 0.1 mol / L hydrochloric acid to remove oxides, then rinse with deionized water and vacuum dry the copper mesh disc;
[0048] (2) Sodium chloride particles sieved through an 80-mesh sieve were used as pore-forming agents. The sodium chloride particles were placed in a vacuum drying oven at 50° C. and dried. After drying, 1.14 g of the sodium chloride particles were weighed and placed in a grinding jar together with electrolytic copper powder with a particle size of 5 μm and a mass of 4.73 g. The grinding jar was then placed in a planetary ball mill for thorough mixing to obtain a copper salt mixture. The ball milling time was 30 min and the rotation speed was 160 rpm.
[0049] (3) Weigh 5 g of the copper salt mixture and put it into a stainless steel mold. First, manually compact it to form a loose structure. Then, lay two layers of copper mesh with a mesh size of 80 on the loose structure. Finally, press it into a tablet by a tablet press. The tablet press is set to a pressure of 250 MPa and a holding time of 180 s.
[0050] (4) placing the pressed tablet obtained in step (3) into a tubular furnace for vacuum sintering to improve the structural strength of the pressed sample, with a heating rate of 10°C / min and a sintering temperature of 750°C; waiting for the tubular furnace to cool naturally to room temperature, then taking out the sample, placing the taken sample in an ultrasonic cleaning machine, first ultrasonically cleaning it with deionized water and anhydrous ethanol until no white particles are precipitated on the surface of the sample when cleaning with anhydrous ethanol; after cleaning, moving the sample to a drying oven for vacuum drying for 4 hours; after drying, weighing the sample mass using an electronic balance and comparing it with the mass of the electrolytic copper powder initially used in step (2); if the mass difference between the two is within 3%, the cleaning and drying steps are completed, otherwise, ultrasonic cleaning and drying treatments need to be continued until the quality requirements are met.
[0051] Figure 1 (b) is a SEM image of a heat dissipation material prepared by laying two layers of 80-mesh copper mesh on a loose structure. It can be seen from the figure that as the number of composite copper mesh layers increases, the number of contact points between grid lines also increases. At the same time, more flat spots appear on the high points of each wire diameter. These newly added contact points and flat spots can provide additional vaporization core points for the boiling heat transfer process, thereby enhancing the heat transfer effect.
[0052] Figure 2 (b) is the microstructure diagram of the heat dissipation material under the optical mode, which is prepared by laying two layers of copper mesh with a mesh size of 80 on a loose structure. It can be seen from the figure that the 50%-1.5mm-double layer 80 mesh does not have a structure with gradually increasing pore size, but more flat spots are observed at the same unit area, and these flat spots are good nucleation sites.
[0053] like Figure 4 As shown in the figure, after the porous copper surface is composited with copper mesh, under the same heat flux density, the boiling starting point is further reduced, the boiling heat transfer coefficient is improved, and the heat flux density value corresponding to the peak value of the convective heat transfer coefficient is increased. The change trend of its boiling curve is similar to that of powder-formed porous copper, both of which first increase and then decrease with the increase of heat flux density. With the increase of the number of layers of surface composite copper mesh, the boiling heat transfer performance is improved. Under the same heat flux density, when the number of layers of surface composite copper mesh increases from one layer to two layers, the superheat of the surface composite copper mesh porous copper will decrease, and the boiling heat transfer coefficient will be improved. At a heat flux density of 257154W·m -2 When the surface is composited with two layers of 80-mesh copper mesh, the heat transfer coefficient of the powder-molded porous copper reaches up to 65159 W·m -2 ·K -1 , which is about 1.4 times that of the uncomposite copper mesh, indicating that the composite wire mesh can enhance the heat transfer performance of powder-formed porous copper.
[0054] Embodiment 2
[0055] The difference between this embodiment and embodiment 1 lies in step (3). Step (3) in this embodiment is to lay a layer of 80-mesh copper mesh and a layer of 60-mesh copper mesh on the loose structure from bottom to top, and the other steps remain consistent with embodiment 1.
[0056] Figure 2 (a) is a microscopic structure diagram of the heat dissipation material prepared by laying a layer of 80-mesh copper mesh and a layer of 60-mesh copper mesh from bottom to top on a loose structure. It can be seen from the figure that a structure with gradually increasing apertures between large meshes and small meshes is clearly observed on the 60-mesh-80-mesh-50%-1.5mm sample. This structure is consistent with the trend of the diameter changing from small to large during the process of bubble growth and detachment, which can significantly reduce the resistance of bubble detachment.
[0057] like Figure 5As shown in the figure, the different arrangement order of the copper mesh affects the boiling heat transfer performance of the sample to a certain extent. When a layer of 60-mesh copper mesh is compounded on the powder-molded porous copper with an 80-mesh copper mesh on the surface, the mesh diameter between the wire meshes will suddenly increase. This gradually increasing structure helps the bubbles to detach smoothly. In this process, the grid-like structure suddenly expands, forming a unique "micro-chimney effect". This effect promotes the detachment of bubbles, significantly reduces the superheat, and thus improves the heat transfer efficiency. Compared with the other two samples, its heat transfer performance advantage becomes more obvious when the heat flux density is higher. Its ONB is 1.2℃, and at a heat flux density of 231124W·m -2 The heat transfer coefficient is as high as 69301W·m -2 ·K -1 , which is 1.4 times that of the uncompounded copper mesh porous copper, and far exceeds the smooth copper, about 4 times, and the heat transfer characteristics of the surface composite 60-80 mesh gradient copper mesh porous copper are generally higher than the surface composite double-layer 80 mesh copper mesh porous copper.
[0058] Embodiment 3
[0059] The difference between this embodiment and embodiment 1 lies in step (3). Step (3) in this embodiment is to lay a layer of 100-mesh copper mesh and a layer of 80-mesh copper mesh on the loose structure from bottom to top, and the other steps remain consistent with embodiment 1.
[0060] like Figure 5 As shown in the figure, when the surface is composited with 80-100 mesh gradient copper mesh, its boiling starting point is reduced and the heat transfer coefficient is improved, but because its structure is a smaller pore size, it does not conform to the bubble growth law. Its heat transfer coefficient shows a trend of first rising and then falling with the increase of heat flux density, and the overall downward trend is higher than that of 60-80 mesh. At the same heat flux density, its heat transfer coefficient is also generally lower than that of porous copper composited with 60-80 mesh gradient copper mesh on the surface.
Claims
1. A method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh, characterized in that: The following steps are involved: (1) cutting the copper mesh into copper mesh discs according to the specification requirements, then ultrasonically cleaning the copper mesh discs with anhydrous ethanol to remove oil stains, then using hydrochloric acid to remove oxides, then rinsing with deionized water and vacuum drying the copper mesh discs; (2) using sodium chloride particles as a pore-forming agent, drying the sodium chloride particles and mixing them with electrolytic copper powder in a certain ratio in a ball mill to obtain a copper salt mixture; (3) placing a certain mass of the copper salt mixture into a stainless steel mold, first manually compacting it to form a loose structure, then laying multiple layers of copper mesh on the loose structure, and finally pressing and forming a pressed sheet; the multiple layers of copper mesh are copper meshes of the same mesh number or copper meshes of different mesh numbers. When the multiple layers of copper mesh are copper meshes of different mesh numbers, they are laid on the surface of the loose structure in order from small to large mesh numbers and from top to bottom to form a composite gradient copper mesh; (4) The pressed tablets obtained in step (3) are sequentially vacuum sintered, cleaned, and dried to obtain an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh.
2. The method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1, characterized in that: In step (3), the multi-layer copper mesh is two layers; the two layers of copper mesh are copper meshes with a mesh number of 80 mesh, or a layer of 60 mesh copper mesh and a layer of 80 mesh copper mesh, or a layer of 80 mesh copper mesh and a layer of 100 mesh copper mesh.
3. The method for preparing a modified powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 2, characterized in that: In step (3), the multi-layer copper mesh is a layer of 60-mesh copper mesh and a layer of 80-mesh copper mesh.
4. The method for preparing a modified powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1 or 2, characterized in that: In step (2), the sodium chloride particles are sieved through an 80-mesh sieve; and the sodium chloride particles are dried in a vacuum drying oven at 50°C.
5. The method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1 or 2, characterized in that: In step (2), the particle size of the electrolytic copper powder is 5 μm; the mass ratio of the dried sodium chloride particles to the electrolytic copper powder is 1:(4-5).
6. The method for preparing the improved powder-molded porous copper heat dissipation material based on the surface composite copper mesh according to claim 1 or 2, characterized in that: In step (2), the dried sodium chloride particles are placed in a grinding jar together with the electrolytic copper powder, and then the grinding jar is placed in a planetary ball mill for thorough mixing; the ball milling time is 25-35 minutes, and the rotation speed is 150-180 rpm.
7. The method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1 or 2, characterized in that: In step (3), the tablet is finally pressed by a tablet press to obtain a tablet, the tablet press is set to a pressure of 240-280 MPa, and the pressure holding time is 180-200 s.
8. The method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1 or 2, characterized in that: In step (4), the pressed tablet is placed in a tubular furnace for vacuum sintering, the heating rate is 8-12°C / min, and the sintering temperature is 650-850°C.
9. The method for preparing an improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh according to claim 1 or 2, characterized in that: In step (1), the diameter of the copper mesh disc is 30 mm, and the concentration of hydrochloric acid is 0.1 mol / L.
10. An improved powder-molded porous copper heat dissipation material based on a surface composite copper mesh prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Cited By
Preparation method of cold plate, cold plate and two-phase heat exchanger
CN122210052A