Forming method of infrared radiation heating curing fiber reinforced resin matrix composite and product

By using infrared radiation nanorods in fiber reinforced resin composites, the problems of uneven temperature and high energy consumption during the curing process of composite materials are solved, and efficient infrared heating curing is achieved, which significantly improves mechanical properties and production efficiency. In the manufacturing of large and complex curved surface parts.

CN118906490APending Publication Date: 2024-11-08HUAZHONG UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411208070.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing composite material curing process has problems such as uneven temperature, high energy consumption, limited product size and low safety, which limits its widespread use in industrial applications.

Method used

By using infrared radiation heating curing method, by adding infrared radiation nanorods to the fiber-reinforced resin composite, the efficient infrared absorption characteristics of the nanorods are used to achieve uniform heating of the composite material, shortening the curing time and improving mechanical properties.

Benefits of technology

It realizes uniform heating of composite materials, shortens curing time, improves mechanical properties, especially interlayer shear strength and bending strength, and is suitable for the manufacturing of large and complex curved surface parts, reducing energy consumption and production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118906490A_ABST
    Figure CN118906490A_ABST
Patent Text Reader

Abstract

The invention belongs to the related technical field of fiber-reinforced resin-based composite materials, and discloses a forming method and a product of an infrared radiation heating curing fiber-reinforced resin-based composite material. The method comprises the following steps: S1, selecting fibers, resin and an infrared radiation material as raw materials; s2, the fibers are flatly laid and placed in a mold, resin and infrared radiation material nanorods are injected into the mold, so that the fibers are completely infiltrated and coated with the resin, and a prefabricated product of a fiber reinforced resin composite material is obtained; s3, the prefabricated product in the mold is heated and cured through infrared radiation, and the needed fiber reinforced resin composite material is obtained after curing. The invention further discloses a product obtained through the forming method. The curing time is shortened, and the mechanical property of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field related to fiber-reinforced resin-based composite materials, and more specifically, relates to a forming method and a product of a fiber-reinforced resin-based composite material cured by infrared radiation heating. Background Art

[0002] Fiber-reinforced polymer composites have mechanical properties such as high strength-to-weight and stiffness-to-weight ratios, corrosion resistance, and wear resistance, and have been widely used in industries such as aerospace, marine transportation, wind turbine blades, sporting goods, and building reinforcement. However, designing efficient and reasonable rapid curing schemes in industry remains a challenge. Traditional curing process schemes have obvious advantages in the manufacture of small composite materials. In recent years, advanced curing technologies have shown excellent processing efficiency in the manufacture of large composite materials, and the curing time has been greatly reduced. However, the long manufacturing cycle time of large structural parts makes them only suitable for small and medium-sized batch production, and their application in large-scale production is limited. Therefore, in actual industrial applications, considering the cost of the curing process, the processability of large composite materials, and the impact on the mechanical properties of composite materials, it is particularly important to develop an economically reasonable and technically feasible curing process scheme.

[0003] In a large number of studies on the optimization of curing processes, fast-curing resin systems and advanced curing technologies for polymer composites (including mold heating curing, oven heating curing, resistance heating curing, microwave heating curing, infrared radiation curing, etc.) are regarded as the main means to shorten processing time and reduce energy consumption. The energy consumption of mold heating and oven heating curing processes is high, and energy loss will increase with the complexity of the material structure and the size scale, resulting in low heating efficiency. In addition, for materials with a certain thickness, the outer layer of material that first contacts the heating layer will cure faster than the inner layer. The skin-core effect caused by the advancement of the curing process will lead to stress concentration and irreversible strain. More seriously, it will eventually cause microcracks and deformation of the material. The existing resistance heating curing heating effect is not obvious, and there are inevitably problems such as low electrothermal conversion efficiency and easy fatigue. The uniformity of microwave heating curing depends on the stability of the electromagnetic field, which is difficult to control. The uneven electromagnetic field will bring about the phenomenon of uneven radiation penetration depth, which will produce a temperature difference in the thickness direction of the composite material, making it difficult to achieve uniform curing, and its versatility is very poor. Some scholars pointed out that photopolymerization is one of the fastest methods to generate three-dimensional networks, and radiation curing has a wide range of applications in the curing of polymer composites, so infrared radiation (IR) will be a suitable alternative to traditional curing. Although microwave and infrared curing mechanisms are based on electromagnetic radiation, they are considered to be thermal processes due to their low ionization frequencies. Infrared curing is a composite curing method that has emerged due to its high energy efficiency, predictable heating rate (temperature change per unit time) and volumetric heating mechanism. However, it is often used for the heating of thermoplastic materials, which requires rapid heating rather than long-term complex curing states, including different heating rates and dwelling temperatures. However, existing infrared radiators still have obvious light that can easily burn the human body. In addition, their radiation range is relatively small, and the size of the composite material that can be prepared is severely limited; the curing time of the existing infrared radiation curing process has not been significantly shortened, resulting in the advantages of infrared not being brought into play, and the infrared lamp has high energy consumption and is not suitable for large-scale applications, which makes the infrared radiation curing process not widely used in industry.

[0004] Therefore, existing composite materials and curing processes have low safety factors, the size of products that can be prepared is greatly limited, and they cannot be actually applied in industry, which has become a technical problem in this field. Summary of the invention

[0005] In view of the above defects or improvement needs of the prior art, the present invention provides a forming method and product of infrared radiation heating and curing fiber-reinforced resin-based composite materials, which solves the problem of uneven temperature during the curing process of fiber-reinforced resin-based composite materials.

[0006] To achieve the above object, according to one aspect of the present invention, a forming method of a fiber-reinforced resin-based composite material cured by infrared radiation heating is provided, the method comprising the following steps:

[0007] S1 selects fiber, resin and infrared radiation material as raw materials;

[0008] S2: laying the fibers flat in a mold, injecting resin and infrared radiation material nanorods into the mold so that the resin completely infiltrates and covers the fibers, thereby obtaining a preform of a fiber-reinforced resin composite material;

[0009] S3 uses infrared radiation heating to cure the preform in the mold, and obtains the desired fiber-reinforced resin composite material after curing.

[0010] Further preferably, in step S2, an accelerator and a curing agent are added when the resin and the infrared radiation material nanorods are injected into the mold, and the masses of the accelerator and the curing agent are 1% to 3% and 1% to 5% of the mass of the resin, respectively.

[0011] Further preferably, in step S2, in the preformed product, the mass fraction of the resin material is 30% to 50%, the mass fraction of the fiber material is 40% to 60%, and the rest are infrared radiation material nanorods, and the mass fraction of the resin material is the total mass fraction of the resin, accelerator and curing agent.

[0012] Further preferably, in step S1, the infrared radiation material nanorods are one or more of silicon dioxide, titanium oxide, bismuth telluride, lead sulfide, indium antimonide, lead tin telluride, mercury cadmium telluride, triglycyl sulfate, lithium tantalate, lead germanate, magnesium oxide, tin oxide, zinc oxide, copper oxide, silicon carbide, metal nanorods, ceramics and tourmaline.

[0013] Further preferably, in step S1, the resin is one or more of epoxy resin, unsaturated polyester resin, phenolic resin, vinyl acetate resin, polyurethane, aminoplast, polyvinyl chloride, polycarbonate, polyamide, polypropylene and polyethylene.

[0014] Further preferably, in step S1, the fiber is one or more of basalt fiber, glass fiber, carbon fiber, boron fiber, aramid fiber, ceramic fiber and natural fiber.

[0015] Further preferably, steps S2 and S3 are performed in a vacuum state.

[0016] Further preferably, after the fibers are laid flat in the mold, the fibers need to be preheated, and the preheating temperature is 40° C. to 150° C. and the time is 1 hour to 5 hours.

[0017] Further preferably, in step S3, the curing temperature is 40° C. to 180° C., and the curing time is 1 h to 10 h.

[0018] According to another aspect of the present invention, there is provided a product prepared according to the above-mentioned forming method.

[0019] In general, the above technical solutions conceived by the present invention have the following beneficial effects compared with the prior art:

[0020] 1. The present invention adds infrared radiation material nanorods into the resin. When infrared rays are directly incident on the upper surface of the composite material, the molecules of the uppermost layer of material absorb the infrared rays and resonate to generate heat. This part of the heat will flow out from the top layer and be conducted layer by layer to the bottom layer. The remaining infrared rays penetrate into the resin. The infrared radiation material and the resin material molecules absorb these infrared rays and convert them into heat until they penetrate the entire composite material board, thereby achieving the purpose of uniform heating of the entire board. The infrared rays penetrate the resin and fiber to achieve the purpose of overall uniform heating.

[0021] 2. Compared with the traditional room temperature curing process, the infrared radiation curing process proposed by the present invention shortens the curing time of the composite material by 91%, and shortens it by 86% compared with the oven curing; at the same time, it also greatly improves its mechanical properties. Specifically, the interlaminar shear strength and bending strength of the composite laminate are increased by 36% and 28% respectively. Therefore, the present invention provides a new idea for the curing process design of large and complex composite curved surface parts, and has broad application prospects in the fields of wind power generation, aerospace, and transportation;

[0022] 3. The infrared radiation material nanorods used in the present invention have excellent infrared absorption characteristics, can absorb infrared radiation more effectively, and convert it into heat energy, thereby improving the heating efficiency of the resin and accelerating the curing speed; since the nanorod material can efficiently absorb and convert infrared radiation, the energy utilization rate in the curing process is higher, thereby reducing the overall energy consumption; the uniform distribution of the nanorod material in the resin can ensure that the infrared radiation is evenly distributed throughout the resin material, avoiding local overheating or uncured phenomena, and improving the uniformity and quality of curing; during the curing process, the nanorod material can form a good interface with the resin matrix, thereby improving the mechanical properties and thermal stability of the cured resin material; by adjusting the concentration, distribution and intensity of the nanorod material and the infrared radiation, the curing process can be precisely controlled to meet the specific needs of different application scenarios;

[0023] 4. The present invention changes the process of slowly heating to the curing temperature of the composite material and performing isothermal curing for dozens of hours in the traditional heating curing process into a process of rapidly heating to a specific temperature and performing a shorter heat preservation process. By gradually approaching the curing temperature of the composite material, the heat generated by the exothermic curing reaction is slowly released, and the originally long and locally intense curing reaction is transformed into a relatively short and gentle curing process. This process makes the overall curing temperature of the composite material more uniform, and the product size that can be prepared is also not limited, which greatly improves the curing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a flow chart of a forming method of infrared radiation heating curing fiber reinforced resin-based composite material constructed according to a preferred embodiment of the present invention;

[0025] Figure 2 This is a 200-fold magnified SEM photograph of the surface of a composite material prepared by the infrared radiation curing process constructed according to the preferred embodiment 1 of the present invention;

[0026] Figure 3 This is a SEM photograph of a cross section of a composite material prepared by the infrared radiation curing process constructed according to the preferred embodiment 1 of the present invention, magnified 150 times;

[0027] Figure 4 is a graph showing the test results of interlaminar shear strength of a composite material prepared by the infrared radiation curing process constructed according to the preferred embodiment 1 of the present invention;

[0028] Figure 5 It is a curve chart of the bending strength test results of the composite material prepared by the infrared radiation curing process constructed according to the preferred embodiment 1 of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0030] A forming method of a fiber-reinforced resin-based composite material using infrared radiation heating and curing, comprising the following steps:

[0031] (1) Prepare the mold: Make sure the mold surface is clean and free of dust and impurities. Apply release agent evenly on the mold surface to prevent the finished product from sticking to the mold.

[0032] (2) Prepare fiber reinforcement materials: Cut the fibers according to the design requirements to ensure accurate size and shape. Lay the cut fiber materials on the mold layer by layer according to the design requirements to ensure that each layer of material is neatly arranged.

[0033] (3) Preparation of nanorod materials:

[0034] The preparation method of the nanorods can be a sol-gel method, a hydrothermal method, a microemulsion method, a template method, an electrophoretic deposition method, and a chemical vapor deposition method. The nanorod material can be one or more of silicon dioxide, titanium oxide, bismuth telluride, lead sulfide, indium antimonide, lead tin telluride, mercury cadmium telluride, triglycyl sulfate, lithium tantalate, lead germanate, magnesium oxide, tin oxide, zinc oxide, copper oxide, silicon carbide, metal nanorods, ceramics, and tourmaline.

[0035] (4) Arrange the injection system: Lay a release cloth and a guide net above the fiber material to promote uniform distribution of the resin. Set the resin injection port and exhaust port at the appropriate position of the mold, and install the resin infusion pipeline and vacuum air pipeline.

[0036] (5) Packing the vacuum bag: Cover the vacuum bag film on the mold and the laid material, making sure the bag film is large enough to cover the entire mold. Use sealing tape to seal the edge of the vacuum bag film to the edge of the mold to ensure there is no air leakage.

[0037] (6) Establish a vacuum system: Connect the vacuum pump to the exhaust port of the vacuum bag, start the vacuum pump, and gradually extract the air in the bag until the bag film is tightly attached to the fiber material. Ensure that there is no leakage in the vacuum bag and the vacuum degree meets the requirements.

[0038] (7) Preheating: Turn on the infrared radiation heating equipment to preheat the fiber at a certain temperature (40-150°C) and time (1-5h).

[0039] (8) Prepare the resin: turn off the infrared heating equipment, prepare the resin according to the formula requirements, add appropriate accelerator (1% to 3% of the resin mass), curing agent (1% to 5% of the resin mass), resin main agent, and then add infrared radiation material nanorods, and stir evenly. Inject the mixed resin solution into the vacuum bag through the injection port. Under the action of vacuum pressure, the resin gradually penetrates the fiber material to obtain a preformed product. The mass fraction of the resin material (including resin, accelerator and curing agent) is 30% to 50%, the mass fraction of the fiber material is 40% to 60%, and the rest is infrared radiation material nanorods. Monitor the flow and penetration of the resin in real time to ensure that the resin is evenly distributed without dry spots and bubbles.

[0040] (9) Curing: Continue to maintain a high vacuum degree, turn on the infrared radiation heating equipment, and perform heating and curing according to the designed infrared curing process parameters.

[0041] Among them, the manufacture of infrared radiation heating equipment can be found in another invention patent applied by our team (a photonic crystal infrared electric heating film and its preparation method).

[0042] (10) Demolding: After the material cools to room temperature, carefully remove the vacuum bag film and sealing tape, and take the cured fiber-reinforced resin-based composite material out of the mold.

[0043] Among them, the fiber-reinforced resin-based composite material components include infrared radiation material nanorods, uniformly mixed resin materials, and fiber materials.

[0044] Preferably, the infrared radiation material includes nanorod materials such as silicon dioxide, titanium oxide, bismuth telluride, lead sulfide, indium antimonide, lead tin telluride, mercury cadmium telluride, triglyceline sulfate, lithium tantalate, lead germanate, magnesium oxide, ceramics, tourmaline, etc.; the resin material includes liquid resins such as epoxy resin, unsaturated polyester resin, phenolic resin, vinyl acetate resin, polyurethane, aminoplast, polyvinyl chloride, polycarbonate, polyamide, polypropylene and polyethylene; the fiber material includes basalt fiber, glass fiber, carbon fiber, boron fiber, aramid fiber, ceramic fiber and various natural fibers, etc.

[0045] Preferably, the preparation method of infrared radiation material nanorods includes sol-gel method, hydrothermal method, microemulsion method, template method, electrophoretic deposition method, and chemical vapor deposition method.

[0046] The present invention will be further described below with reference to specific embodiments.

[0047] Example 1

[0048] Taking silicon dioxide nanorods, unsaturated polyester resin and glass fiber synthesized by sol-gel method as an example, the method described in the present invention is used to process and shape a high-performance glass fiber reinforced polyester resin-based composite material sample.

[0049] The specific steps are as follows:

[0050] (1) Prepare the mold: Make sure the mold surface is clean and free of dust and impurities. Apply release agent evenly on the mold surface to prevent the finished product from sticking to the mold.

[0051] (2) Prepare fiber reinforcement materials: Cut the fibers according to the design requirements to ensure accurate size and shape. Lay the cut fiber materials on the mold layer by layer according to the design requirements to ensure that each layer of material is neatly arranged.

[0052] (3) Preparation of nanorod materials:

[0053] Solution preparation: Dissolve a certain amount of TEOS in anhydrous ethanol to form a TEOS solution. Dissolve a certain amount of CTAB in deionized water to form a CTAB solution. Add an appropriate amount of ammonia water to the CTAB solution as a catalyst.

[0054] Sol formation: Add TEOS solution dropwise into CTAB solution and stir continuously to form a uniform sol. Control the reaction temperature between 25-60℃.

[0055] Gel formation: After a period of sol reaction, gel is formed. The reaction time is usually 12-36 hours.

[0056] Aging and drying: The formed gel is aged to ensure the morphology of the silica nanorods is stable.

[0057] The aging time is 126 hours. After aging, the gel is dried, which can be done by natural drying or heating, and the drying temperature is usually between 50-100°C.

[0058] Calcination: The dried sample is placed in a muffle furnace for calcination to remove the surfactant and further enhance the stability of the nanorods. The calcination temperature is generally 400-600°C and the calcination time is 1-6 hours.

[0059] (4) Arrange the injection system: Lay a release cloth and a guide net above the fiber material to promote uniform distribution of the resin. Set the resin injection port and exhaust port at the appropriate position of the mold, and install the resin infusion pipeline and vacuum air pipeline.

[0060] (5) Packing the vacuum bag: Cover the vacuum bag film on the mold and the laid material, making sure the bag film is large enough to cover the entire mold. Use sealing tape to seal the edge of the vacuum bag film to the edge of the mold to ensure there is no air leakage.

[0061] (6) Establish a vacuum system: Connect the vacuum pump to the exhaust port of the vacuum bag, start the vacuum pump, and gradually extract the air in the bag until the bag film is tightly attached to the fiber material. Ensure that there is no leakage in the vacuum bag and the vacuum degree meets the requirements.

[0062] (7) Preheating: Turn on the infrared heating equipment and preheat the glass fiber at 40°C for 1 hour.

[0063] (8) Prepare resin: Turn off the infrared heating equipment, prepare the resin according to the formula requirements, add appropriate accelerator (mass is 2% of the resin mass), curing agent (mass is 3% of the resin mass), polyester resin, and then add silica nanorods and stir evenly. Inject the mixed resin solution into the vacuum bag through the injection port. Under the action of vacuum pressure, the resin gradually penetrates the fiber material to obtain a preformed product, in which the resin material accounts for 40% of the total mass, the fiber material accounts for 55% of the total mass, and the infrared radiation material nanorods account for 5% of the total mass. Monitor the flow and penetration of the resin in real time to ensure that the resin is evenly distributed without dry spots and bubbles.

[0064] (9) Curing: Continue to maintain a high vacuum degree, turn on the infrared radiation heating equipment, and heat and cure according to the infrared curing process plan of first heating to 40°C and keeping it for 1 hour, and then heating to 100°C and keeping it for 4 hours.

[0065] (10) Demolding: After the material cools to room temperature, carefully remove the vacuum bag film and sealing tape, and take the cured fiber-reinforced resin-based composite material out of the mold.

[0066] (11) The prepared glass fiber reinforced composite material is used for mechanical property testing.

[0067] Example 2

[0068] The steps of this embodiment are the same as those of embodiment 1, except that:

[0069] (1) In the preform, the resin material accounts for 30% of the total mass, the fiber material accounts for 60% of the total mass, and the infrared radiation material nanorods account for 10% of the total mass. In the resin material, the added accelerator is 1wt% of the resin mass, and the curing agent is 5wt% of the resin mass.

[0070] (2) The glass fiber was preheated at 100°C for 3 h under infrared equipment.

[0071] (3) Heat curing is carried out according to the infrared curing process parameter scheme of directly heating to 40°C and keeping the temperature for 10 hours.

[0072] Example 3

[0073] The steps of this embodiment are the same as those of embodiment 1, except that:

[0074] (1) In the preform, the resin material accounts for 50% of the total mass, the fiber material accounts for 40% of the total mass, and the infrared radiation material nanorods account for 10% of the total mass. In the resin material, the added accelerator is 3wt% of the resin mass, and the curing agent is 1wt% of the resin mass.

[0075] (2) The glass fiber was preheated at 150°C for 5 h under infrared equipment.

[0076] (3) Heat curing is performed according to the infrared curing process parameter scheme of first heating to 60°C and keeping the temperature for 0.5 h, and then heating to 180°C and keeping the temperature for 0.5 h.

[0077] Example 4

[0078] The steps of this embodiment are the same as those of embodiment 1, except that:

[0079] (1) In the preform, the resin material accounts for 39% of the total mass, the fiber material accounts for 60% of the total mass, and the infrared radiation material nanorods account for 1% of the total mass. In the resin material, the added accelerator is 2wt% and the curing agent is 3wt%.

[0080] (2) The glass fiber is preheated at 60°C for 2 h under infrared equipment.

[0081] (3) Heat curing is performed according to the infrared curing process parameter scheme of first heating to 40°C and keeping the temperature for 1 hour, and then heating to 120°C and keeping the temperature for 4 hours.

[0082] Example 5

[0083] The steps of this embodiment are the same as those of embodiment 1, except that:

[0084] (1) Preheat the glass fiber in an oven at 40°C for 1 h.

[0085] (2) Heat curing is performed according to the infrared curing process parameter scheme of directly heating to 180°C and keeping the temperature for 1 hour.

[0086] Example 6

[0087] The steps of this embodiment are the same as those of embodiment 1, except that:

[0088] (1) Preheat the glass fiber in an oven at 40°C for 1 h.

[0089] (2) Curing at room temperature is carried out according to the room temperature curing process parameter plan of placing it in air for 72 hours.

[0090] Example 7

[0091] The steps of this embodiment are the same as those of embodiment 1, except that:

[0092] (1) Preheat the glass fiber in an oven at 40°C for 1 h.

[0093] (2) Heat curing is performed according to the oven curing process parameter scheme of first curing at room temperature for 24 hours and then keeping it in an oven at 80°C for 24 hours.

[0094] Example 8

[0095] The steps of this embodiment are the same as those of embodiment 1, except that:

[0096] Taking titanium oxide nanorods, epoxy resin and basalt fibers synthesized by a hydrothermal method as an example, a high-performance basalt fiber reinforced polyester resin-based composite material sample was processed and formed using the method described in Example 1 of the present invention.

[0097] (1) Experimental steps for preparing titanium oxide nanorods by hydrothermal method:

[0098] Solution preparation:

[0099] Precursor solution: Add tetrabutyl titanate or isopropyl titanate into ethanol and stir evenly;

[0100] Alkaline solution: dissolve NaOH or NaF in deionized water and stir evenly;

[0101] Mixing solution: Slowly add the precursor solution into the alkaline solution while continuously stirring.

[0102] Hydrothermal reaction:

[0103] Pour the mixed solution into a polytetrafluoroethylene (PTFE) lined autoclave. Ensure a good seal to prevent solution leakage. Place in an oven and react at 180°C for 12 hours. Under high temperature and high pressure conditions, the TiO2 precursor gradually hydrolyzes and crystallizes to form a nanorod structure.

[0104] Washing and centrifugation:

[0105] After the reaction is completed, the mixture is cooled to room temperature naturally. The reaction product is taken out and washed with deionized water several times to remove unreacted precursors and other impurities. The product is centrifuged to separate solid TiO2 nanorods.

[0106] Drying and calcination:

[0107] The nanorods were dried at 70°C for 12 hours to remove excess water, and the dried nanorods were calcined at 500°C for 3 hours to improve crystallinity.

[0108] (2) Prepare the resin according to the formula requirements, weigh the epoxy resin main agent and curing agent (3wt%), then add 5% titanium oxide nanorods and stir evenly.

[0109] (3) The basalt fiber was preheated at 80°C for 1 hour under infrared equipment, and then heated and cured according to the infrared curing process parameter scheme of first heating to 80°C and keeping it for 1 hour, then heating to 120°C and keeping it for 2 hours, and finally heating to 160°C and keeping it for 2 hours.

[0110] like Figure 1The figure shows a flow chart of the forming method of infrared radiation heating curing fiber reinforced resin matrix composite material constructed in Example 1. By changing the ratio of resin material, fiber material and infrared radiation nanorod material and adjusting the curing process conditions appropriately, the mechanical property changes are explored. Preliminary testing of mechanical properties shows that the composite material under the infrared curing process of Example 1 has the best mechanical properties, which is the best infrared curing process scheme for this material.

[0111] In order to prove that the infrared radiation curing process of the present invention has the characteristics of short curing time and high efficiency, the infrared curing process of Implementation Case 1, the room temperature curing of Implementation Case 6, and the oven curing time of Implementation Case 7 were statistically analyzed. The curing time of the composite material prepared by the infrared radiation curing process is 91% shorter than that of room temperature curing, and 86% shorter than that of oven curing, as shown in the following table.

[0112] Curing process Infrared curing Room temperature cure Oven curing Time (h) 6.6 72 48

[0113] In order to prove that the infrared radiation curing process of the present invention has the advantages of low energy consumption and low investment cost, the average specific energy consumption and heating equipment cost consumed by the infrared curing process in Implementation Case 1 and the curing process in the oven curing in Implementation Case 7 are compared. The specific data are shown in the following table.

[0114] Curing process Infrared curing Oven curing Average specific energy consumption 7.8kJ / g 24kJ / g Average equipment cost 5,000 yuan / m2 50,000 yuan / m2

[0115] from Figure 2 and Figure 3 It can be clearly seen that the composite material surface in Example 1 of the present invention is completely covered with resin, without defects such as holes and insufficient glue, and the surface quality is good; the resin and fiber of the composite material section are well combined. In order to prove that the product of the present invention has good mechanical properties, the mechanical properties of the infrared-cured composite material in Example 1 were tested and compared with those of the room temperature-cured composite material in Example 6. The specific data are as follows Figure 4 and Figure 5 As shown, it can be seen that the mechanical properties of the composite materials prepared by infrared radiation curing are significantly higher than those cured at room temperature, among which the interlaminar shear strength is increased by 36% and the bending strength is increased by 28%, which can be suitable for the manufacture of large and complex curved parts.

[0116] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A forming method for infrared radiation heating and curing fiber-reinforced resin-based composite materials, It is characterized in that The method comprises the following steps: S1 selects fiber, resin and infrared radiation material as raw materials; S2: laying the fibers flat in a mold, injecting resin and infrared radiation material nanorods into the mold so that the resin completely infiltrates and covers the fibers, thereby obtaining a preform of a fiber-reinforced resin composite material; S3 uses infrared radiation heating to cure the preform in the mold, and obtains the desired fiber-reinforced resin composite material after curing.

2. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1, It is characterized in that In step S2, when the resin and infrared radiation material nanorods are injected into the mold, an accelerator and a curing agent are added, and the masses of the accelerator and the curing agent are 1% to 3% and 1% to 5% of the mass of the resin, respectively.

3. A forming method of infrared radiation heating curing fiber reinforced resin matrix composite material as claimed in claim 2, It is characterized in that In step S2, in the preform, the mass fraction of the resin material is 30% to 50%, the mass fraction of the fiber material is 40% to 60%, and the rest is infrared radiation material nanorods. The mass fraction of the resin material is the total mass fraction of the resin, accelerator and curing agent.

4. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1 or 2, It is characterized in that In step S1, the infrared radiation material nanorods are one or more of silicon dioxide, titanium oxide, bismuth telluride, lead sulfide, indium antimonide, lead tin telluride, mercury cadmium telluride, triglycyl sulfate, lithium tantalate, lead germanate, magnesium oxide, tin oxide, zinc oxide, copper oxide, silicon carbide, metal nanorods, ceramics and tourmaline.

5. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 3, It is characterized in that In step S1, the resin is one or more of epoxy resin, unsaturated polyester resin, phenolic resin, vinyl acetate resin, polyurethane, aminoplast, polyvinyl chloride, polycarbonate, polyamide, polypropylene and polyethylene.

6. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1 or 3, It is characterized in that In step S1, the fiber is one or more of basalt fiber, glass fiber, carbon fiber, boron fiber, aramid fiber, ceramic fiber and natural fiber.

7. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1 or 3, It is characterized in that The steps S2 and S3 are performed in a vacuum state.

8. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1 or 3, It is characterized in that After the fibers are laid flat in the mold, they need to be preheated at a temperature of 40° C. to 150° C. and for a time of 1 h to 5 h.

9. A forming method of infrared radiation heating curing fiber reinforced resin-based composite material according to claim 1 or 3, It is characterized in that In step S3, the curing temperature is 40°C to 180°C, and the curing time is 1 hour to 10 hours.

10. A product prepared by the forming method according to any one of claims 1 to 9.

Citation Information

Cited By

  • Curing stress testing method and device suitable for light curing, heat curing and coupling curing of light curing and heat curing

    CN120629246A