Method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag
Lithium phosphate is generated by alkali leaching, acid leaching and neutralizing precipitation treatment of electrolytic aluminum overhaul slag and carbon slag, which solves the problem of low resource utilization of lithium elements and achieves efficient recycling and low-cost treatment effects.
Patent Information
- Application Number
- CN202411209263.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-08-30
AI Technical Summary
During aluminum electrolysis, lithium oxide or other lithium salts react with molten electrolyte to form lithium fluoride, causing the lithium element water electrolyte to penetrate into the cathode liner or carbon slag, causing the problem of low resource utilization.
By pre-treatment and post-mixing of electrolytic aluminum overhaul and carbon slag, alkali leaching, cyanide removal and acid leaching treatment, then neutralization and solid-liquid separation are carried out to obtain lithium sulfate, and lithium phosphate is generated by heating reaction.
It has achieved harmless treatment of electrolytic aluminum overhaul and carbon slag with low lithium content, efficient recycling of lithium elements, reduced processing costs, simple and convenient operation, and significant economic benefits.
Smart Images

Figure CN118908168A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium phosphate, and in particular to a method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag. Background Art
[0002] Electrolytic aluminum overhaul slag is a kind of solid waste generated in the production process of electrolytic aluminum. That is, in the process of aluminum electrolysis, bauxite undergoes high-temperature smelting and electrolysis reaction to obtain aluminum metal. When the electrolytic cell is maintained, fault repaired or the electrolyte is replaced, a large amount of solid waste will be generated, which is electrolytic aluminum overhaul slag. Electrolytic aluminum overhaul slag often contains chemical components such as incompletely electrolyzed aluminum. Therefore, after treatment and extraction, it can be recycled again. The aluminum electrolysis by-products in the waste slag must be properly treated to reduce its impact and damage to the environment.
[0003] Based on the above situation, it can be found that electrolytic aluminum overhaul slag is an inevitable by-product of electrolytic aluminum production, so how to more efficiently treat and utilize electrolytic aluminum overhaul slag is crucial. At present, after the solid waste such as aluminum electrolytic overhaul slag and carbon slag is purified, the remaining residue is mainly treated by pyrolysis or landfill, resulting in a large loss of fluorine, aluminum, lithium and other elements, resulting in resource waste and environmental pollution, which has always been a problem that has plagued industrial electrolytic aluminum production technology.
[0004] Based on this, in order to recycle the electrolytic aluminum overhaul slag to a greater extent and expand the reuse of the electrolytic aluminum overhaul slag more efficiently and feasibly, it is urgent to find a treatment measure that can both reduce the waste of waste resources and control the emission of harmful substances that pollute the environment. Summary of the invention
[0005] The technical problems to be solved by the present invention are:
[0006] During the process of aluminum electrolysis, lithium oxide or other added lithium salts in alumina react with AlF3 or Na3AlF6 in the molten electrolyte at high temperature to form lithium fluoride. With the periodic addition of lithium-rich alumina or other lithium salts, lithium oxide continuously enters the electrolyte, causing the lithium element aqueous electrolyte to penetrate into the cathode lining, refractory materials or carbon slag, etc., resulting in problems such as low effective resource utilization.
[0007] The technical solution adopted by the present invention is:
[0008] The present invention provides a method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag, comprising the following steps:
[0009] S1 takes electrolytic aluminum overhaul slag and carbon slag respectively, performs pre-treatment, mixes the treated electrolytic aluminum overhaul slag and carbon slag to obtain a mixed material;
[0010] S2: slurrying the mixture, sequentially performing alkali leaching and cyanide removal treatment, and solid-liquid separation to obtain a mixture alkali leaching liquid and a mixture alkali leaching residue;
[0011] S3 takes the mixed material alkali leaching residue, washes it, performs acid leaching treatment, and separates the solid and liquid to obtain the mixed material acid leaching liquid and the mixed material acid leaching residue;
[0012] S4: mixing the mixed alkaline leaching solution in step S2 with the mixed acid leaching solution in step S3, performing neutralization precipitation, solid-liquid separation, taking the supernatant, removing impurities, and obtaining a purified lithium sulfate solution;
[0013] S5: adding trisodium sulfate to the purified lithium sulfate solution, heating for reaction, and obtaining the lithium phosphate.
[0014] Preferably, in step S1, in the pre-treatment, the electrolytic aluminum overhaul slag and the carbon slag are ground to 100-325 mesh.
[0015] Preferably, in step S1, electrolytic aluminum overhaul slag and carbon slag are mixed in a mass ratio of 10:1-2.
[0016] Preferably, in step S2, during the alkali leaching treatment, alkali solution is added to the mixture, mixed, and the solid-liquid ratio is controlled to be 1:4-6 and the pH value is 12-14.
[0017] Preferably, the alkali leaching treatment is carried out at a temperature of 100-160° C., a pressure of 0.1-0.5 MPa, and a time of 3-5 h.
[0018] Preferably, in step S3, washing the mixed alkali leaching residue comprises the following steps: placing the alkali leaching residue in water, controlling the solid-liquid ratio to be 1:2-5, washing, and then solid-liquid separation, the separated filtrate is used for slurry adjustment of the mixed material in step S2, and the separated filter residue is used as the mixed alkali leaching residue for acid leaching.
[0019] Preferably, in step S3, acid solution is added to the washed mixed alkali leaching residue, mixed, and the solid-liquid ratio is controlled to be 1:5-10, the pH value is 2-3, and hydrogen peroxide is added to perform acid leaching.
[0020] Preferably, the acid leaching treatment is carried out at a temperature of 85°C or above and for a time of 3-5 hours.
[0021] Preferably, in step S4, the pH value of the mixed slurry is controlled to be 4.5-5.0, and the molar mass ratio of fluorine to aluminum in the slurry is 1.6-1.65:1.
[0022] Preferably, the lithium concentration in the lithium sulfate purified solution is 1-4 g / L.
[0023] The beneficial effects of the present invention are as follows:
[0024] The method for preparing lithium phosphate by using aluminum electrolysis overhaul slag and carbon slag provided by the present invention can realize harmless treatment of aluminum electrolysis overhaul slag and carbon slag with low lithium content, and efficiently recycle lithium elements, and reduce the treatment cost of aluminum electrolysis overhaul slag and carbon slag. The operation is simple and convenient, the controllability of the operation process is high, the treatment cost is low, and the economic benefit is significant. It can be widely promoted in the industrialized electrolytic aluminum recycling production. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a process flow chart for preparing lithium phosphate from the aluminum electrolysis overhaul slag and carbon slag in Example 1. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0027] In the process of aluminum electrolysis, lithium oxide or other added lithium salts in alumina react with AlF3 or Na3AlF6 in molten electrolyte at high temperature to generate lithium fluoride. With the periodic addition of lithium-rich alumina or other lithium salts, lithium oxide continuously enters the electrolyte, causing lithium element aqueous electrolyte to penetrate into the cathode lining, refractory materials or carbon slag, etc., resulting in low resource utilization efficiency and other problems. Based on this, the present invention provides a method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag, comprising the following steps:
[0028] (1) The electrolytic aluminum overhaul slag is manually sorted to initially separate steel bars and aluminum blocks, and then multi-stage crushing, grinding, and magnetic separation are performed to remove iron; the carbon slag is taken and ground.
[0029] Among them, the grinding particle size of electrolytic aluminum overhaul slag and carbon powder is 100-325 mesh, which is conducive to improving the leaching rate of valuable elements such as fluorine and lithium in the mixture, effectively controlling production costs, and achieving a greater degree of lithium leaching and recycling. Specifically, if the overhaul slag particle size is too large, it will reduce the leaching rate of valuable elements such as fluorine and lithium in the overhaul slag. If the overhaul slag particle size is too small, it will cause the problem of excessive load on the ball mill equipment, increasing production losses and costs.
[0030] The treated electrolytic aluminum overhaul slag and carbon slag are mixed at a mass ratio of 10:1-2 and stirred evenly to obtain a mixture. Mixing within this ratio range can effectively adjust the ratio of fluorine to aluminum in the mixture, which is beneficial to the synthesis of fluorine aluminum precursor Al2F in the leachate. 3.24 (OH) 2.76 ·H2O.
[0031] After iron removal and mixing, the amount of iron entering the system can be reduced, and the fluorine-aluminum ratio in the overhaul slag and carbon slag mixture can be adjusted, which is beneficial to the subsequent leaching effect of the mixture, thereby increasing the leaching rate of lithium in the mixture.
[0032] (2) The mixed material is slurried, and alkali leaching and cyanide removal treatment are performed in sequence, and solid-liquid separation is performed to obtain a mixed material alkali leaching liquid and a mixed material alkali leaching residue.
[0033] Among them, the alkali leaching conditions are: solid-liquid ratio is 1:4-6, pH value is 12-14, temperature is 100-160°C, pressure is 0.1-0.5MPa, and alkali leaching time is 3-5h.
[0034] Specifically, if the solid-liquid ratio of the mixture in alkaline leaching is too large, it will affect the leaching rate of valuable elements such as fluorine and lithium in the mixture, and increase the viscosity of the slurry, causing blockage of pumping pipelines, etc. If the solid-liquid ratio of the mixture in alkaline leaching is too small, it will cause a large amount of alkali solution consumption, increase production costs, and subsequently aggravate the impact on the environment.
[0035] Alkali leaching treatment can use alkaline solutions such as sodium hydroxide solution, and control the pH value to 12-14. This is because: if the concentration of the alkaline solution is too low, it will affect the leaching rate of valuable elements such as fluorine and lithium in the mixture; if the concentration of the alkaline solution is too high, it will increase the equipment anti-corrosion requirements and increase production costs.
[0036] Cyanide removal can be achieved by adding a cyanide removal agent, such as hydrogen peroxide, which can reduce the cyanide content after reaction.
[0037] (3) Washing the mixed material alkali leaching residue, recovering the soluble sodium hydroxide, sodium fluoride, etc. remaining in the mixed material alkali leaching residue, separating the solid and liquid, the filtrate after washing can be used for the mixed material slurry in the previous step, and the filter residue is subjected to the next step of acid leaching treatment.
[0038] The solid-liquid ratio during washing is 1:2-5. After testing, washing with a solid-liquid ratio of 1:2 and then washing with 300m 2 The backwashing of the plate and frame filter press can achieve a recovery rate of 80-90% for sodium hydroxide and sodium fluoride.
[0039] The washed mixed alkali leaching residue is subjected to acid leaching treatment to dissolve out the element components such as fluorine, aluminum and lithium in the mixed alkali leaching residue, and the mixed acid leaching liquid and the mixed acid leaching residue are obtained through solid-liquid separation.
[0040] The main chemical reactions involved in the acid leaching process are as follows:
[0041] 2LiF+H2SO4→Li2SO4+2HF↑ (1);
[0042] Li2O+H2O→2LiOH (2);
[0043] 2LiOH+H2SO4=Li2SO4+H2O (3);
[0044] Li2C2+2H2O=2LiOH+C2H2 (4);
[0045] 2LiOH+H2SO4=Li2SO4+H2O (5);
[0046] The acid leaching conditions are: solid-liquid ratio of 1:5-10, temperature above 85°C, sulfuric acid is added to a pH of 2-3, and 3-5‰ hydrogen peroxide is added to the total volume of the slurry, and the acid leaching time is 3-5h. After acid leaching under this condition, the fluorine leaching rate can reach more than 90%, the aluminum leaching rate can reach more than 80%, and the lithium leaching rate can reach more than 95%. The addition of hydrogen peroxide can oxidize the dissolved divalent iron ions in the slurry into trivalent iron ions, and the trivalent iron ions form yellow sodium iron alum [NaFe3(SO4)2(OH)6] with the sodium sulfate in the slurry. n , reducing the iron content in the mixed acid leaching solution, the reaction principle is as follows:
[0047] 3Fe2(SO4)3+12H2O+Na2SO4 = Na2Fe6(SO4)4(OH) 12 ↓+6H2SO4 (6).
[0048] (4) The above-mentioned mixed alkaline leaching solution and the mixed acid leaching solution are mixed for neutralization precipitation. The neutralization reaction conditions are: reaction temperature 60-80°C, pH value 4.5-5.0, molar mass ratio of fluorine to aluminum in the slurry is 1.6-1.65:1, and reaction time is 3-5h; then solid-liquid separation is performed and the supernatant is taken.
[0049] In the above reaction process, if the pH value is too low, the neutralization precipitation reaction will be incomplete, and if the pH value is too high, cryolite phase will be produced, affecting the product purity of aluminum fluoride and aluminum oxide.
[0050] After neutralization and precipitation, fluoride ions and aluminum ions can react under the above conditions at a mass ratio of 1.62:1 to form fluorine aluminum precursor Al2F 3.24 (OH) 2.76 H2O can realize the resource utilization of valuable elements such as fluorine and aluminum in aluminum electrolysis overhaul slag and carbon slag. The reaction principle is as follows: 0.76Al 3+ +3.24AlF2++2H + +7.52NaOH→2Al2F 3.24 (OH) 2.76 ·H2O↓+7.52Na + (7).
[0051] The supernatant is sequentially treated for iron removal, silicon removal, calcium removal, magnesium removal, etc., and the impurity removal conditions are as follows: first add hydrogen peroxide with a volume fraction of 3-5‰ to the neutralized liquid, then add lime, adjust the pH value to 8±0.2, react for 1-2 hours, separate the solid and liquid, take the separated clear liquid, add sodium hydroxide to a pH value of 10.5-11.5, react for 1-2 hours, separate the solid and liquid again, take the separated filtrate, and adjust the pH value to 7-8.
[0052] After neutralization, there are still unreacted fluorine, aluminum, iron, silicon, calcium, magnesium and other impurity elements in the liquid. Therefore, hydrogen peroxide is added to the supernatant to oxidize the divalent iron ions into trivalent iron ions, and the pH value is adjusted with lime. After solid-liquid separation, fluorine, aluminum, iron, silicon and other impurities are removed. Sodium hydroxide is added to react and solid-liquid separation is performed to remove impurities such as calcium and magnesium in the liquid after neutralization. Finally, the pH value is adjusted to obtain a mixed purified liquid containing lithium sulfate and sodium sulfate.
[0053] Then, after reverse osmosis membrane filtration and concentration, the system membrane pressure is 7-8MPa, the volume ratio of fresh water to concentrated water is about 4:6, and the lithium concentration in the purified liquid can be increased by about 1.5-2 times; then it is placed at 0-3℃ for freezing and crystallization, which can remove a large amount of sodium sulfate Na2SO4·10H2O and further increase the lithium concentration in the purified liquid by about 1.2-1.3 times to obtain lithium sulfate purified liquid, and the lithium ion concentration in the lithium sulfate purified liquid is as high as 1g / L or more.
[0054] The alkaline leaching solution is mixed with the acid leaching solution for neutralization and precipitation, and the fluorine and aluminum elements in the leaching solution are recovered and utilized. After the obtained supernatant is purified by impurities, it is concentrated by reverse osmosis membrane filtration and frozen crystallization to remove the mirabilite, which can effectively increase the lithium ion concentration in the purified liquid and reduce the sodium sulfate concentration.
[0055] (5) According to the stoichiometric ratio of the reaction, trisodium phosphate is added to the lithium sulfate purified liquid with a lithium concentration of about 1-4 g / L. The amount of trisodium phosphate added can be controlled to be 1-1.2 times of the stoichiometric ratio so that the reaction can be fully carried out during the actual operation. The reaction is placed at 80-90° C. for 1-2 hours. After solid-liquid separation and washing, lithium phosphate with a purity of up to 98-99.5% is obtained, and the yield is about 90% or more.
[0056] The above reaction principle is as follows:
[0057] 3Li2SO4+2Na3PO4=2Li3PO4↓+3Na2SO4 (8).
[0058] In the above reaction process, trisodium phosphate can be added directly as solid Na3PO4·12H2O, or solid Na3PO4·12H2O can be dissolved into a solution and then added in the form of a solution. Na3PO4·12H2O can be prepared from phosphate recovered in the process of preparing lithium carbonate from lithium phosphate, so as to achieve the recycling of trisodium phosphate and improve the level of comprehensive resource utilization.
[0059] The present invention, through the above-mentioned processing steps, can achieve harmless treatment of electrolytic aluminum overhaul slag and carbon slag with low lithium content, and efficiently recycle lithium elements. The operation is simple and convenient, the operation process is highly controllable, the processing cost is low, and the economic benefit is significant. It can be widely promoted in industrial electrolytic aluminum recycling and reuse production.
[0060] Example 1
[0061] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.31%, and the lithium content in the carbon slag is 0.29%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 200±50 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0062] Step 2: Use sodium hydroxide solution with a pH value of 12 to adjust the mixture, control the solid-liquid ratio of the mixture slurry to 1:6, then pressurize it to 0.3MPa, heat it to 120°C, and alkali-leach it for 3 hours; after the alkali-leach is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixed alkali leaching liquid and the mixed alkali leaching residue.
[0063] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, with the mass ratio of washing liquid to mixed alkali leaching residue being 2:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:5, the pH value to 2.0, the temperature to 85°C, acid leaching for 2 hours, and then add 3‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1 hour; after the acid leaching is completed, use a plate and frame filter press for separation to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is subjected to harmless treatment to obtain a harmless carbon material.
[0064] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 4.5, place it at 60°C for reaction for 3 hours, and filter it with a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 3‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 1 hour, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution, adjust the pH value to 10.5, react for 2 hours, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 8, and obtain a lithium sulfate purified liquid.
[0065] Step 5: The lithium sulfate purified liquid is filtered and concentrated by a reverse osmosis membrane filtration system at a membrane pressure of 7.5 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 0°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 3.6 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 90°C, reacted for 1 hour, and then filtered and separated by a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 4:1 to obtain a lithium phosphate product.
[0066] The purity of the lithium phosphate product was determined to be 98.7%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 92.4%.
[0067] Example 2
[0068] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.35%, and the lithium content in the carbon slag is 0.33%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 200±30 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0069] Step 2: Use sodium hydroxide solution with a pH value of 12.2 to adjust the mixture, control the solid-liquid ratio of the mixture slurry to 1:5, then pressurize it to 0.5MPa, heat it to 155°C, and alkali leaching for 2.2h; after the alkali leaching is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixed alkali leaching liquid and the mixed alkali leaching residue.
[0070] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, with the mass ratio of washing liquid to mixed alkali leaching residue being 2:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:5, the pH value to 2.0, the temperature to 85°C, acid leaching for 2 hours, and then add 3‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1 hour; after the acid leaching is completed, use a plate and frame filter press for separation to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is subjected to harmless treatment to obtain a harmless carbon material.
[0071] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 4.5, place it at 60°C for reaction for 3 hours, and filter it with a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 3‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 1 hour, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution, adjust the pH value to 10.5, react for 2 hours, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 8, and obtain a lithium sulfate purified liquid.
[0072] Step 5: The lithium sulfate purified liquid is filtered and concentrated by a reverse osmosis membrane filtration system at a membrane pressure of 7.5 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 0°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 3.7 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 90°C, reacted for 1 hour, and then filtered and separated by a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 4:1 to obtain a lithium phosphate product.
[0073] The purity of the lithium phosphate product was determined to be 98.8%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 91.7%.
[0074] Example 3
[0075] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.32%, and the lithium content in the carbon slag is 0.37%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 200±50 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0076] Step 2: Use sodium hydroxide solution with a pH value of 12 to adjust the mixture, control the solid-liquid ratio of the mixture slurry to 1:6, then pressurize it to 0.3MPa, heat it to 120°C, and alkali-leach it for 3 hours; after the alkali-leach is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixed alkali leaching liquid and the mixed alkali leaching residue.
[0077] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, and the mass ratio of the washing liquid to the mixed alkali leaching residue is 3.4:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:8, the pH value to 2.1, the temperature to 90°C, acid leaching for 2.8 hours, and then add 5‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1.2 hours; after the acid leaching is completed, use a plate and frame filter press for separation to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is harmlessly treated to obtain a harmless carbon material.
[0078] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 4.5, place it at 60°C for reaction for 3 hours, and filter it with a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 3‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 1 hour, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution, adjust the pH value to 10.5, react for 2 hours, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 8, and obtain a lithium sulfate purified liquid.
[0079] Step 5: The lithium sulfate purified liquid is filtered and concentrated by a reverse osmosis membrane filtration system at a membrane pressure of 7.5 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 0°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 3.7 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 90°C, reacted for 1 hour, and then filtered and separated by a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 4:1 to obtain a lithium phosphate product.
[0080] The purity of the lithium phosphate product was determined to be 99.0%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 92.7%.
[0081] Example 4
[0082] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.45%, and the lithium content in the carbon slag is 0.34%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 180±50 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0083] Step 2: Use sodium hydroxide solution with a pH value of 12 to adjust the mixture, control the solid-liquid ratio of the mixture slurry to 1:6, then pressurize it to 0.3MPa, heat it to 120°C, and alkali-leach it for 3 hours; after the alkali-leach is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixed alkali leaching liquid and the mixed alkali leaching residue.
[0084] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, with the mass ratio of washing liquid to mixed alkali leaching residue being 2:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:5, the pH value to 2.0, the temperature to 85°C, acid leaching for 2 hours, and then add 3‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1 hour; after the acid leaching is completed, use a plate and frame filter press for separation to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is subjected to harmless treatment to obtain a harmless carbon material.
[0085] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 4.8, place it at 70°C to react for 2.8 hours, and filter it using a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 5‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 1.5 hours, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution, adjust the pH value to 11.2, react for 1.5 hours, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 7.9, and obtain a lithium sulfate purified liquid.
[0086] Step 5: The lithium sulfate purified liquid is filtered and concentrated by a reverse osmosis membrane filtration system at a membrane pressure of 7.5 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 0°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 3.9 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 90°C, reacted for 1 hour, and then filtered and separated by a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 4:1 to obtain a lithium phosphate product.
[0087] After measurement, the purity of the lithium phosphate product was 98.8%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 94.1%.
[0088] Example 5
[0089] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.39%, and the lithium content in the carbon slag is 0.41%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 200±50 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0090] Step 2: Use sodium hydroxide solution with a pH value of 12 to adjust the mixture, control the solid-liquid ratio of the mixture slurry to 1:6, then pressurize it to 0.3MPa, heat it to 120°C, and alkali-leach it for 3 hours; after the alkali-leach is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixed alkali leaching liquid and the mixed alkali leaching residue.
[0091] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, with the mass ratio of washing liquid to mixed alkali leaching residue being 2:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:5, the pH value to 2.0, the temperature to 85°C, acid leaching for 2 hours, and then add 3‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1 hour; after the acid leaching is completed, use a plate and frame filter press for separation to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is subjected to harmless treatment to obtain a harmless carbon material.
[0092] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 4.5, place it at 60°C for reaction for 3 hours, and filter it with a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 3‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 1 hour, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution, adjust the pH value to 10.5, react for 2 hours, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 8, and obtain a lithium sulfate purified liquid.
[0093] Step 5: The lithium sulfate purified liquid is filtered and concentrated through a reverse osmosis membrane filtration system at a membrane pressure of 8 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 2°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 4.1 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 85°C, reacted for 1.65 hours, and then filtered and separated through a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 5:1 to obtain a lithium phosphate product.
[0094] After measurement, the purity of the lithium phosphate product was 99.2%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 94.5%.
[0095] Example 6
[0096] Step 1: Take electrolytic aluminum overhaul slag and carbon slag respectively, and after measurement, the lithium content in the electrolytic aluminum overhaul slag is 0.31%, and the lithium content in the carbon slag is 0.29%. After crushing, impurity removal and grinding, the electrolytic aluminum overhaul slag and carbon slag are ball-milled to a granular powder with a particle size of 200±50 mesh. The electrolytic aluminum overhaul slag and carbon slag are evenly mixed at a mass ratio of 10:1 to obtain a mixture.
[0097] Step 2: Use 30g / L sodium hydroxide solution to slurry the mixture, control the solid-liquid ratio of the mixture slurry to 1:4, then pressurize it to 0.5MPa, heat it to 160°C, and alkali-leach it for 2h; after the alkali-leach is completed, cool and reduce the pressure, add hydrogen peroxide, mix well to remove cyanide, and filter and separate with a plate and frame filter press to obtain the mixture alkali-leach liquid and the mixture alkali-leach residue.
[0098] Step 3: Wash the mixed alkali leaching residue on a plate and frame filter press, with the mass ratio of washing liquid to mixed alkali leaching residue being 5:1; add 98% sulfuric acid solution to the washed mixed alkali leaching residue, control the solid-liquid ratio to 1:10, the pH value to 2.5, the temperature to 90°C, acid leaching for 3 hours, and then add 5‰ of hydrogen peroxide of the total volume of the slurry, and continue acid leaching for 1 hour; after the acid leaching is completed, separate by a plate and frame filter press to obtain a mixed acid leaching liquid and a mixed acid leaching residue, wherein the mixed acid leaching residue is subjected to harmless treatment to obtain a harmless carbon material.
[0099] Step 4: Take the mixed acid leaching solution, add the mixed alkaline leaching solution obtained in step 2 until the pH value is 5, place it at 70°C for reaction for 3 hours, and filter it with a plate and frame filter press to obtain a fluoroaluminum precursor and a neutralized liquid; take the neutralized liquid, add 5‰ hydrogen peroxide, and then add lime to adjust the pH value to 8, react for 2 hours, and then separate the solid and liquid, take the filtrate, add sodium hydroxide solution to adjust the pH value to 11.5, react for 1 hour, and then separate the solid and liquid, add 98% sulfuric acid solution to the filtrate until the pH value is 7, and obtain a lithium sulfate purified liquid.
[0100] Step 5: The lithium sulfate purified liquid is filtered and concentrated through a reverse osmosis membrane filtration system at a membrane pressure of 7.5 MPa to obtain a fresh water and concentrated water ratio of about 2:3. The concentrated water is frozen and crystallized at 3°C, and the sodium sulfate is removed to obtain an initial concentrated purified liquid, in which the lithium concentration is measured to be 3.2 g / L; 1.2 times the stoichiometric ratio of trisodium phosphate is added to the initial concentrated purified liquid, heated to 80°C, reacted for 2 hours, and then filtered and separated through a plate and frame filter, and washed on the plate and frame filter at a mass ratio of washing liquid to lithium phosphate of 5:1 to obtain a lithium phosphate product.
[0101] The purity of the lithium phosphate product was determined to be 99.2%, and the yield of lithium phosphate (actual amount of lithium phosphate produced / theoretical amount of lithium phosphate produced×100%) was 91.5%.
[0102] By adopting the preparation methods in Examples 1 to 6, a lithium phosphate product with a purity of more than 98% can be obtained, and the yield of lithium phosphate production is as high as more than 90%. It can be seen that the method for preparing lithium phosphate using aluminum electrolysis overhaul slag and carbon slag provided by the present invention can prepare high-purity lithium phosphate from overhaul slag and carbon slag with low lithium content, thereby achieving more full and efficient comprehensive utilization of lithium resources and alleviating the problem of low resource utilization of by-products produced in aluminum electrolysis.
[0103] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag, characterized in that: The steps include: S1 takes electrolytic aluminum overhaul slag and carbon slag respectively, performs pre-treatment, mixes the treated electrolytic aluminum overhaul slag and carbon slag to obtain a mixed material; S2: slurrying the mixture, sequentially performing alkali leaching and cyanide removal treatment, and solid-liquid separation to obtain a mixture alkali leaching liquid and a mixture alkali leaching residue; S3 takes the mixed material alkali leaching residue, washes it, performs acid leaching treatment, and separates the solid and liquid to obtain the mixed material acid leaching liquid and the mixed material acid leaching residue; S4: mixing the mixed alkaline leaching solution in step S2 with the mixed acid leaching solution in step S3, performing neutralization precipitation, solid-liquid separation, taking the supernatant, removing impurities, and obtaining a purified lithium sulfate solution; S5: adding trisodium sulfate to the purified lithium sulfate solution, heating for reaction, and obtaining the lithium phosphate.
2. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 1, characterized in that: In step S1, in the pre-treatment, the electrolytic aluminum overhaul slag and the carbon slag are ground to 100-325 mesh.
3. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 1, characterized in that: In step S1, electrolytic aluminum overhaul slag and carbon slag are mixed in a mass ratio of 10:1-2.
4. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 1, characterized in that: In step S2, during the alkali leaching treatment, alkali solution is added to the mixture, mixed, and the solid-liquid ratio is controlled to be 1:4-6 and the pH value is 12-14.
5. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 4, characterized in that: The temperature of the alkali leaching treatment is 100-160°C, the pressure is 0.1-0.5MPa, and the time is 3-5h.
6. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 1, characterized in that: In step S3, washing the mixed alkali leaching residue comprises the following steps: The alkali leaching residue is placed in water, the solid-liquid ratio is controlled to be 1:2-5, washed, and then the solid-liquid is separated. The separated filtrate is used for the mixed material slurry adjustment in step S2, and the separated filter residue is used as the mixed material alkali leaching residue for acid leaching.
7. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 1, characterized in that: In step S3, acid solution is added to the washed mixed alkali leached residue, mixed, and the solid-liquid ratio is controlled to be 1:5-10, the pH value is 2-3, and hydrogen peroxide is added to perform acid leaching.
8. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 7, characterized in that: The temperature of the acid leaching treatment is above 85°C and the time is 3-5 hours.
9. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to any one of claims 1 to 8, characterized in that: In step S4, the pH value of the mixed slurry is controlled to be 4.5-5.0, and the molar mass ratio of fluorine to aluminum in the slurry is 1.6-1.65:
1.
10. The method for preparing lithium phosphate from aluminum electrolysis overhaul slag and carbon slag according to claim 9, characterized in that: The lithium concentration in the lithium sulfate purified solution is 1-4 g / L.
Citation Information
Patent Citations
Method for enriching and extracting lithium salt from overhaul slag and carbon slag
CN115959689A
Method for comprehensively recovering carbon, lithium, aluminum and fluorine from aluminum electrolysis carbon residues
CN116903014A
Cooperative treatment and resource utilization method for aluminum electrolysis overhaul slag and carbon slag
CN117139352A
Method for improving filtering effect of overhaul slag acid leaching slurry
CN117161071A
A system for the combined acid-base treatment of aluminum electrolyte overhaul slag mixture
DE202023107219U1
Cited By
Method for synthesizing battery-grade lithium phosphate from electrolytic aluminum overhaul slag
CN119569006A
Method for resource utilization of sludge gasification slag
CN120864648A