Petal spherical magnesium oxide as well as preparation method and application thereof

By hydrothermal reaction and calcining of magnesium sulfate and sodium bicarbonate in an alkaline environment, petal spherical magnesium oxide was prepared, which solved the problem of insufficient thermal conductivity of magnesium oxide, and achieved high purity and high thermal conductivity preparation of magnesium oxide. Suitable for the preparation of thermal inks.

CN118908247APending Publication Date: 2024-11-08YUNFU HONGZHI NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411007702.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing magnesium oxide preparation technology, the obtained magnesium oxide has insufficient thermal conductivity, resulting in insufficient quality of the electronic ink.

Method used

Mix magnesium sulfate aqueous solution and sodium bicarbonate aqueous solution to adjust it to an alkaline environment, conduct high-temperature hydrothermal reaction and calcination, and prepare petal spherical magnesium oxide, remove impurities through the hydrothermal process and form a uniform particle size and shape to improve heat conductivity. sex.

Benefits of technology

The prepared petal spherical magnesium oxide has better thermal conductivity and high purity, small particle size, and is suitable for thermal conductivity fillers in thermal inks, significantly improving the thermal conductivity effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908247A_ABST
    Figure CN118908247A_ABST
Patent Text Reader

Abstract

The invention discloses petal spherical magnesium oxide as well as a preparation method and application thereof. The preparation method of the petal spherical magnesium oxide comprises the following steps: mixing a magnesium sulfate aqueous solution and a sodium bicarbonate aqueous solution, and then adding ammonia water to adjust the pH value to be alkaline; putting the mixed solution into a hydrothermal reaction kettle for high-temperature hydrothermal reaction to obtain basic magnesium carbonate; and calcining at 650-750 DEG C in the atmosphere to obtain the petal spherical magnesium oxide. The petal spherical magnesium oxide is high in purity and small in particle size, the minimum particle size can reach 500nm, the petal spherical magnesium oxide has a larger specific surface area, and the petal spherical magnesium oxide is used as a heat-conducting filler during preparation of heat-conducting ink, so that the heat-conducting effect is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to petal-shaped spherical magnesium oxide and a preparation method and application thereof. Background Art

[0002] Nano magnesium oxide products are white powders, odorless, non-toxic, with small particle size and large specific surface area. They have optical, electrical, magnetic and chemical properties different from those of the bulk material, and have high hardness, high purity and high melting point. It is precisely because of the chemical properties of nano magnesium oxide combined with its physical properties that nano magnesium oxide has excellent electrical insulation, thermal conductivity and heat resistance. It can be used as a raw material for refractory materials, insulating materials for heaters, grinding materials, vulcanization accelerators for rubber, pigments for coatings / inks and other industrial materials for various purposes.

[0003] In the existing magnesium oxide preparation technology, the magnesium oxide prepared is mostly ordinary spherical nano magnesium oxide, which has insufficient thermal conductivity when used to prepare thermally conductive electronic ink, resulting in the electronic ink having poor quality. Summary of the invention

[0004] In view of this, the main technical problem solved by the present invention is to prepare a petal-shaped spherical magnesium oxide, which has better thermal conductivity, high purity and small particle size.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0006] A method for preparing petal-shaped spherical magnesium oxide comprises the following steps:

[0007] Mixing an aqueous solution of magnesium sulfate and an aqueous solution of sodium bicarbonate, and then adjusting the mixed solution to be alkaline;

[0008] The mixed solution is placed in a hydrothermal reactor for high-temperature hydrothermal reaction to obtain basic magnesium carbonate;

[0009] The petal-shaped spherical magnesium oxide is obtained by calcining at 650-750°C in an atmospheric atmosphere.

[0010] In the present invention, after the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution are mixed, since the environment of the mixed solution is an alkaline environment, the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution initially generate basic magnesium carbonate under this environmental condition, and in a further hydrothermal process, the basic magnesium carbonate is recrystallized, impurities are removed and basic magnesium carbonate with relatively uniform shape and particle size is formed, and finally magnesium oxide with uniform particle size in the shape of petals is obtained through calcination.

[0011] As a preferred embodiment of the present invention, the substance added to adjust the mixed solution to be alkaline is preferably ammonia water, which has the advantage of not introducing other impurities after addition. In addition, in the subsequent hydrothermal step, ammonia water will have gas overflow at high temperature, increasing the pressure in the hydrothermal reactor, and the hydrothermal efficiency is higher.

[0012] As a preferred embodiment of the present invention, the molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to sodium bicarbonate in the sodium bicarbonate aqueous solution is 1:1; and the mass percentage concentration of the ammonia water is 20-23wt%.

[0013] As a preferred embodiment of the present invention, the volume ratio of the magnesium sulfate aqueous solution to the sodium bicarbonate aqueous solution is 1:1, and the process of mixing the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution is to simultaneously drop the two aqueous solutions under stirring, and the dropping method is adopted to make the precipitation crystallization of the initially generated basic magnesium carbonate more uniform, without colloid adsorption, to ensure that the particle size meets the requirements, and the quality of the basic magnesium carbonate obtained by recrystallization will also be higher; the dropping speed is preferably 20-50ml / min, and ammonia water is added dropwise to keep the pH=9.0-10.0 during the mixing process, and after the two aqueous solutions are added dropwise, the pH of the mixed fusion is continued to be adjusted to 10.5-11.0.

[0014] As a preferred embodiment of the present invention, the hydrothermal reaction kettle is at a temperature of 120 to 140° C., and the hydrothermal reaction time is 2 to 4 hours.

[0015] As a preferred embodiment of the present invention, the calcination time of basic magnesium carbonate is 1 to 3 hours.

[0016] As a preferred embodiment of the present invention, the basic magnesium carbonate is filtered and washed with water before calcination, and then dried.

[0017] The petal-shaped spherical magnesium oxide prepared by the present invention has high purity and small particle size, the particle size is mainly concentrated in the range of 220nm to 396nm, and has a larger specific surface area. It is used as a thermal conductive filler when preparing thermal conductive ink. The petal-shaped spherical structural feature can play a better connecting role, and the thermal conductive path is shorter, thereby having a better thermal conductive effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is one of the SEM images of the petal-shaped spherical magnesium oxide according to the preferred embodiment of the present invention;

[0019] Figure 2 This is the second SEM image of the petal-shaped spherical magnesium oxide according to the preferred embodiment of the present invention;

[0020] Figure 3 This is a Malvern particle size distribution instrument test result diagram of petal-shaped spherical magnesium oxide according to a preferred embodiment of the present invention;

[0021] Figure 4 This is a SEM image of magnesium oxide obtained in a comparative example of the present invention. DETAILED DESCRIPTION

[0022] In order to allow those skilled in the art to understand the present invention more clearly and intuitively, the present invention will be further described below in conjunction with the accompanying drawings.

[0023] The preparation method of petal spherical magnesium oxide of the present invention comprises the following steps:

[0024] Mixing an aqueous solution of magnesium sulfate and an aqueous solution of sodium bicarbonate, and then adding aqueous ammonia to adjust the mixed solution to be alkaline;

[0025] The mixed solution is placed in a hydrothermal reactor for high-temperature hydrothermal reaction to obtain basic magnesium carbonate;

[0026] The petal-shaped spherical magnesium oxide is obtained by calcining at 650-750°C in an atmospheric atmosphere.

[0027] The molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to sodium bicarbonate in the sodium bicarbonate aqueous solution is 1:1; and the mass percentage concentration of the ammonia water is 20-23wt%.

[0028] The volume ratio of the magnesium sulfate aqueous solution to the sodium bicarbonate aqueous solution is 1:1. The process of mixing the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution is to drop the two aqueous solutions simultaneously under stirring, the dropping speed is 20-50 ml / min, and the pH is maintained at 9.0-10.0 during the mixing process. After the two aqueous solutions are added dropwise, the pH of the mixed fusion is continuously adjusted to 10.5-11.0.

[0029] The condition of the hydrothermal reactor is 120-140°C, and the hydrothermal reaction time is 2-4 hours. In actual production, the hydrothermal temperature can be selected as 120°C, and the time can be selected as 4 hours. In addition to the above conditions, the selection of hydrothermal conditions is based on the formation of recrystallization to obtain basic magnesium carbonate with uniform shape and particle size.

[0030] The calcination time of basic magnesium carbonate is 1 to 3 hours.

[0031] The basic magnesium carbonate is filtered and washed with water before calcination, and then dried.

[0032] Preferred Embodiments

[0033] The preparation method of petal spherical magnesium oxide in this embodiment comprises the following steps:

[0034] Dissolve magnesium sulfate in a beaker to form an aqueous solution with a concentration of 100 g / L, and dissolve sodium bicarbonate in a aqueous solution with a concentration of 70 g / L;

[0035] Add 100 ml of bottom water to a 2000 ml beaker; in the embodiment, the mixing is achieved by a stirring blade in the reactor, and the addition of bottom water can ensure that the added magnesium sulfate and sodium bicarbonate can react during the initial reaction while stirring;

[0036] Take 500ml of magnesium sulfate aqueous solution and 500ml of sodium bicarbonate aqueous solution respectively, start stirring, and add magnesium sulfate solution and sodium bicarbonate aqueous solution to the beaker in a dropwise manner at the same time, and basic magnesium carbonate will be formed in this process. The volumes of the two reactants added at the same time are equivalent, and the process reaction is more uniform and stable. Compared with the two directly poured together, the reaction fluctuation is large, and the uniformity of the synthetic particle size is poor. The particle size of the product generated by slow dropwise addition is better controlled, uniform and has good particle size concentration. The dripping rate is 40ml / min, and 20-23wt% of ammonia water is added to keep the pH value meter testing and monitoring pH=9.0-10.0 during the process. After the two are added, 20-23wt% of ammonia water is added to adjust the pH=10.5-11.0. Then put it into the hydrothermal reactor, take it out after hydrothermal heating at 120℃ for 4h, and the filter cake obtained after suction filtration and washing is dried at 105℃. The dried sample is placed in a calcining furnace and calcined at 700℃ for 2h in an atmospheric atmosphere to obtain petal spherical magnesium oxide.

[0037] In this embodiment, the magnesium sulfate raw material is purified before use to remove trace heavy metal impurities.

[0038] The test standard of the magnesium oxide product in this embodiment is: GB 1886.216-2016;

[0039] The particle size of magnesium oxide was tested by Malvern particle size distribution instrument;

[0040] The whiteness of magnesium oxide is tested by Minolta whiteness meter 2600d;

[0041] Magnesium oxide metal is tested by Shimadzu atomic absorption furnace.

[0042] The obtained petal-shaped spherical magnesium oxide was tested for purity, and the purity of the magnesium oxide reached 99.56%. The test results are shown in Table 1.

[0043] Table 1

[0044]

[0045] In addition, the petal spherical magnesium oxide was scanned by electron microscope, and the results were as follows Figure 1-2 As shown, the particle size of the petal-shaped spherical magnesium oxide prepared in this example is about 400 nm, which is close to the result of the particle size distribution instrument test.

[0046] In this embodiment, the basic magnesium carbonate generated by the mixed solution undergoes hydrothermal treatment. During this process, the basic magnesium carbonate is regrown under the conditions of high-temperature hydrothermal reaction to remove the ions adsorbed on the surface. At the same time, the basic magnesium carbonate with a spherical structure is formed during the re-growth process. The crystal re-growth can make the basic magnesium carbonate structure more compact, thereby reducing the crystal particle size and making the particle size distribution of the basic magnesium carbonate more uniform. Finally, the morphology and particle size of the magnesium oxide obtained by calcining the basic magnesium carbonate are directly affected and the quality is improved. The magnesium oxide product obtained by calcination is tested by a Malvern particle size distribution instrument, and it is found that the particle size of the magnesium oxide is mainly concentrated in the range of 220nm to 396nm (the result is shown in FIG. Figure 3 As shown in the figure, the electron microscope image of the product confirms that the nano magnesium oxide obtained after the hydrothermal treatment has better dispersibility and does not need to add a dispersant during the preparation, thus solving the problem of easy agglomeration of magnesium oxide products in the conventional preparation method.

[0047] Comparative Example

[0048] The difference between this embodiment and the preferred embodiment is that no hydrothermal treatment is performed. The specific preparation process is as follows:

[0049] Dissolve magnesium sulfate in a beaker to form an aqueous solution with a concentration of 100 g / L, and dissolve sodium bicarbonate in a aqueous solution with a concentration of 70 g / L;

[0050] Add 100ml of bottom water to a 2000ml beaker;

[0051] Take 500ml of magnesium sulfate aqueous solution and 500ml of sodium bicarbonate aqueous solution respectively, start stirring, and add the magnesium sulfate solution and sodium bicarbonate aqueous solution to the beaker in a dropwise manner. The dripping speed is 40ml / min, and 20-23wt% of ammonia water is added to maintain the pH value meter to test and monitor pH = 9.0-10.0 during the process. After the two are added, add 20-23wt% of ammonia water to adjust the pH to 10.5-11.0. The filter cake obtained after suction filtration and water washing is dried at 105℃, and the dried sample is placed in a calcining furnace and calcined at 700℃ for 2h in an atmospheric atmosphere.

[0052] In this embodiment, magnesium sulfate and sodium bicarbonate are directly used to generate basic magnesium carbonate under alkaline conditions. The basic magnesium carbonate is not subjected to hydrothermal treatment, so the structure of the basic magnesium carbonate is not uniform, the particle size is not uniform, and the structural quality of the magnesium oxide obtained by calcination is relatively poor. The magnesium oxide obtained in the comparative example is scanned by an electron microscope, and the results are as follows: Figure 4 As shown, it can be seen that the petal-shaped spherical magnesium oxide prepared without hydrothermal reaction exceeds 500nm, and strip-shaped magnesium oxide is prone to appear, which has the problem of inconsistent shape and particle size.

[0053] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing petal-shaped spherical magnesium oxide, characterized in that: The steps include: Mixing an aqueous solution of magnesium sulfate and an aqueous solution of sodium bicarbonate, and then adjusting the mixed solution to be alkaline; The mixed solution is placed in a hydrothermal reactor for high-temperature hydrothermal reaction to obtain basic magnesium carbonate; Basic magnesium carbonate is calcined at 650-750°C to obtain petal-shaped spherical magnesium oxide.

2. The preparation method according to claim 1, characterized in that: The molar ratio of magnesium sulfate in the magnesium sulfate aqueous solution to sodium bicarbonate in the sodium bicarbonate aqueous solution is 1:

1.

3. The preparation method according to claim 1, characterized in that: The mixed solution is adjusted to be alkaline by adding aqueous ammonia.

4. The preparation method according to claim 3, characterized in that: The mass percentage concentration of the ammonia water is 20-23wt%.

5. The preparation method according to claim 1, characterized in that: The volume ratio of the magnesium sulfate aqueous solution to the sodium bicarbonate aqueous solution is 1:1; The process of mixing the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution is to drop the two aqueous solutions simultaneously under stirring, the dropping speed is 20-50 ml / min, and the pH of the mixed solution is kept at 9.0-10.0 during the mixing process. After the dropwise addition of the magnesium sulfate aqueous solution and the sodium bicarbonate aqueous solution is completed, the pH of the mixed solution is continuously adjusted to 10.5-11.

0.

6. The preparation method according to claim 1, characterized in that: The hydrothermal reaction kettle temperature is 120-140°C, and the hydrothermal reaction time is 2-4 hours.

7. The preparation method according to claim 1, characterized in that: The calcination time of basic magnesium carbonate is 1 to 3 hours.

8. The preparation method according to claim 1, characterized in that: The basic magnesium carbonate is filtered and washed with water before calcination, and then dried.

9. Petal-shaped spherical magnesium oxide obtained according to the preparation method according to any one of claims 1 to 8.

10. Use of the petal-shaped spherical magnesium oxide prepared by the preparation method according to any one of claims 1 to 8 as a thermally conductive filler in the preparation of thermally conductive ink.

Citation Information

Patent Citations

  • Preparation method of flower-like magnesium oxide

    CN103803593A

  • PTC (Positive Temperature Coefficient) heat-conducting ink and preparation method thereof