Synthesis method of lead halide for perovskite solar cell
Through ball grinding pickling and dilute acid solution treatment, the poor solubility of lead halide in the solvent was solved, and high-purity lead halide was obtained, which significantly improved the performance and stability of perovskite solar cells.
Patent Information
- Application Number
- CN202410956897.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
AI Technical Summary
The poor solubility of existing lead halides in dimethylformamide/dimethylsulfoxide mixed solution leads to poor performance of perovskite solar cells and insufficient purity and stability.
The lead halide lattice is broken by ball grinding and pickling process, halogenated halide oxides, and reacted with hydroxylation through dilute acid solution to form pure phase lead halide that meets the stoichiometric ratio, and then dried at high temperature to improve purity and solubility.
High purity and good solubility lead halide was obtained, which significantly improved the photoelectric conversion efficiency and stability of perovskite solar cells.
Smart Images

Figure CN118908271A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of new energy materials, and in particular relates to a method for synthesizing lead halide for perovskite solar cells. Background Art
[0002] Organic-inorganic lead halide perovskite solar cells have attracted extensive attention due to their advantages such as high light absorption coefficient, high carrier mobility and low cost. The photoelectric conversion efficiency of single-junction perovskite solar cells has exceeded 26.1%. Lead halide is a key raw material for preparing organic-inorganic lead halide perovskite solar cells. Its use method is to dissolve it in a dimethylformamide (DMF) / dimethyl sulfoxide (DMSO) mixed solution and then make a film. The lead halide contains oxides such as H2O, PbO, and PbO2, which will cause its poor solubility in the dimethylformamide / dimethyl sulfoxide mixed solution, resulting in poor performance of the battery device. The purity of lead halide plays a vital role in the performance, stability and repeatability of perovskite solar cells. Therefore, it is very important to develop a lead halide synthesis method that has a simple process flow, is easy to operate, and can be applied to perovskite solar cells. Summary of the invention
[0003] The object of the present invention is to provide a method for synthesizing lead halide with high purity and good solubility for perovskite solar cells.
[0004] The present invention adopts the following technical solution:
[0005] A method for synthesizing lead halide for perovskite solar cells comprises the following steps:
[0006] (1) adding a certain amount of lead source into acetic acid solution and stirring to form a clear and transparent solution;
[0007] (2) adding a certain amount of potassium halide to ultrapure water and stirring to form a clear and transparent solution;
[0008] (3) While stirring, slowly add the solution obtained in step (2) to the solution obtained in step (1), a large amount of precipitate is generated, and the mixture is stirred and reacted for a period of time before filtering;
[0009] (4) placing the dilute acid solution, the grinding beads and the filter residue obtained in step (3) into a ball mill, ball milling for a period of time at room temperature, and then filtering;
[0010] (5) adding ultrapure water to the filter residue obtained in step (4), washing for more than 3 times, then filtering and collecting the solid product and placing it in an oven, and drying to obtain lead halide.
[0011] Preferably, the lead source in step (1) comprises one or more of lead acetate, lead oxide, and lead carbonate, and the concentration of the acetic acid solution is 10 to 30 wt%.
[0012] Preferably, the potassium halide in step (2) is one of potassium iodide, potassium bromide and potassium chloride, with a concentration of 1.00 mol / L to 8.00 mol / L, and the ratio of potassium halide to lead source is in the range of 1:1-1:3 (molar ratio).
[0013] Preferably, the dilute acid solution in step (4) is one of hydroiodic acid, hydrobromic acid and hydrochloric acid, and the concentration is 5 to 20 wt%.
[0014] Preferably, in step (4), the ball-to-material ratio is 1:1, and the grinding bead ratio is 6 mm:4 mm:2 mm=1:3:6.
[0015] Preferably, in step (5), the drying temperature is 80-120° C. and the drying time is 8-24 h.
[0016] The benefits and technical principles of the present invention are as follows:
[0017] The present invention introduces a ball milling and pickling process after the lead halide is prepared. Ball milling can break the lead halide lattice and better handle the impurities inside the material. First, the process can halogenate the insoluble oxides such as PbO and PbO2 inside the lead halide crystal, solving the problem that the lead halide is difficult to completely dissolve in an organic solvent; secondly, the acid solution reacts with the hydroxylated lead halide to convert Pb(OH)X (X is iodine, bromine, or chloride ion) into a pure phase lead halide that meets the stoichiometric ratio of 1:2; finally, the added dilute acid solution can be rapidly volatilized in the subsequent high-temperature drying process, and the obtained lead halide has high purity and good solubility, and can be well suitable for preparing perovskite solar cell thin films. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : X-ray diffraction pattern of lead iodide synthesized in Example 1;
[0019] Figure 2 : The microscopic morphology of the lead iodide powder synthesized in Example 1;
[0020] Figure 3 : Microscopic morphology of the lead iodide powder synthesized in Comparative Example 1;
[0021] Figure 4 : Dissolution of lead iodide synthesized in Example 1 (right) and Comparative Example 1 (left) in a mixed solution of DMF and DMSO;
[0022] Figure 5 : JV curves of FAPbI3 perovskite solar cells prepared using lead iodide in Example 1 and Comparative Example 1;
[0023] Figure 6 : X-ray diffraction pattern of the lead bromide synthesized in Example 2. DETAILED DESCRIPTION
[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention.
[0025] Example 1: Preparation of lead iodide
[0026] A. Add 40 g of lead oxide into a beaker, then add 195 mL of acetic acid solution (16 wt%) and stir to form a clear and transparent solution;
[0027] B. Add 63 g of potassium iodide to 78 mL of ultrapure water and stir to form a clear and transparent solution;
[0028] C. Under stirring, slowly add the solution obtained in step B to the solution obtained in step A (a large amount of precipitate is generated), continue stirring for 6 hours and then filter;
[0029] D. Put 45 mL of 10 wt% hydroiodic acid, grinding beads and the filter residue obtained in step C into a ball mill, ball mill for 6 hours at room temperature and then filter;
[0030] E. Add ultrapure water to the filter residue obtained in step D, wash it for more than 3 times, then filter and collect the solid product and place it in an oven, and dry it at 120° C. for 12 h to obtain lead iodide powder.
[0031] The X-ray diffraction results are as follows Figure 1 As shown, the final product is lead iodide microcrystalline powder, and there is no impurity phase XRD peak. For the microscopic morphology of the product, please refer to Figure 2 , after ICP testing, the product purity is 99.9992%.
[0032] Comparative Example 1: Preparation of Lead Iodide
[0033] In the preparation of lead iodide in this comparative example, compared with Example 1, step D is not performed to obtain lead iodide powder, that is, acid washing and ball milling are not performed, and the filter residue obtained in step C is directly washed with pure water and then dried. For the microscopic morphology of the product, please refer to Figure 3 After ICP testing, the product purity was 99.991%.
[0034] The lead iodide prepared in Example 1 and Comparative Example 1 was added to 10 mL of DMF:DMSO = 9:1 solvent, and the dissolution conditions were as shown in Figure 4, it can be seen that the lead iodide solution of Example 1 is clear and transparent, while the solution obtained in Comparative Example 1 contains insoluble matter. The performance of the perovskite solar cell prepared using the above solution is shown in FIG. Figure 5 , using the lead iodide of Example 1, a higher photoelectric conversion efficiency was obtained.
[0035] Example 2: Preparation of Lead Bromide
[0036] A. Add 46 g of lead carbonate into a beaker, then add 235 mL of acetic acid solution (17 wt%) and stir to form a clear solution;
[0037] B. Add 42 g potassium bromide to 80 mL ultrapure water and stir to form a clear and transparent solution;
[0038] C. Under stirring, slowly add the solution obtained in step B to the solution obtained in step A (a large amount of precipitate is generated), continue stirring for 6 hours and then filter;
[0039] D. Put 50 mL of 12 wt% hydrobromic acid solution, grinding beads and the filter residue obtained in step C into a ball mill, ball mill for 6 h at room temperature and then filter;
[0040] E. Add ultrapure water to the filter residue obtained in step D, wash it for more than 3 times, then filter and collect the solid product and place it in an oven, and dry it at 120° C. for 12 h to obtain lead bromide powder.
[0041] The X-ray diffraction results are as follows Figure 6 As shown, the final product is lead bromide microcrystalline powder, and there is no XRD peak of impurity phase. After ICP detection, the purity of the product is 99.999%.
Claims
1. A method for synthesizing lead halide for perovskite solar cells, characterized in that: The following steps are involved: (1) adding a certain amount of lead source into acetic acid solution and stirring to form a clear and transparent solution; (2) adding a certain amount of potassium halide to ultrapure water and stirring to form a clear and transparent solution; (3) slowly adding the solution obtained in step (2) to the solution obtained in step (1) under stirring, stirring and reacting for a period of time and then filtering; (4) placing the dilute acid solution, the grinding beads and the filter residue obtained in step (3) into a ball mill, ball milling for a period of time at room temperature, and then filtering; (5) adding ultrapure water to the filter residue obtained in step (4), washing for more than 3 times, then filtering and collecting the solid product and placing it in an oven, and drying to obtain lead halide.
2. The method for synthesizing lead halide for perovskite solar cells according to claim 1, characterized in that: The lead source in step (1) includes one or more of lead acetate, lead oxide, and lead carbonate, and the concentration of the acetic acid solution is 10 to 30 wt%.
3. The method for synthesizing lead halide for perovskite solar cells according to claim 1, characterized in that: The potassium halide in step (2) is one of potassium iodide, potassium bromide and potassium chloride, with a concentration of 1.00 mol / L to 8.00 mol / L, and a molar ratio of the potassium halide to the lead source is 1:1-1:
3.
4. The method for synthesizing lead halide for perovskite solar cells according to claim 1, characterized in that: The dilute acid solution in step (4) is one of hydroiodic acid, hydrobromic acid and hydrochloric acid, and the concentration is 5 to 20 wt%.
5. The method for synthesizing lead halide for perovskite solar cells according to claim 1, characterized in that: In step (4), the ball-to-material ratio is 1:1, and the grinding bead ratio is 6mm:4mm:2mm=1:3:
6.
6. The method for synthesizing lead halide for perovskite solar cells according to claim 1, characterized in that: In step (5), the drying temperature is 80-120° C. and the drying time is 8-24 h.