Application of preparation method of N, P-CQDs / WO3-x composite photoelectrode
By loading nitrogen and phosphorus doping carbon quantum doped on tungsten trioxide to form a composite photoelectrode, the challenging problems of oxygen vacancy engineering in the improvement of catalyst performance are solved, and the stability and photoelectric catalytic performance are improved, which is suitable for wastewater treatment. .
Patent Information
- Application Number
- CN202410789128.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-06-18
AI Technical Summary
In the field of photoelectrocatalysis, it is difficult for oxygen vacancies to distinguish and allocate the electronic structure regulation of active sites and the electron transport of catalysts, resulting in challenging improvement of catalytic performance.
Nitrogen-phosphorus doped carbon quantum dots (N, P-CQDs) were prepared by hydrothermal method, and oxygen-containing tungsten trioxide (WO3-x) was prepared by hydrothermal method and surface reduction method, and nitrogen-phosphorus doped carbon quantum was doped by nitrogen-phosphorus. Point loading onto the tungsten trioxide at the oxygen-containing vacant position forms a composite photoelectrode.
A composite photoelectrode with strong stability and good photoelectric catalytic performance was prepared for wastewater treatment, which significantly improved the degradation efficiency of toxic and harmful pollutants.
Smart Images

Figure HSA0000299542570000011 
Figure HSA0000299542570000021 
Figure HSA0000299542570000031
Abstract
Description
Technical Field
[0001] The invention belongs to the field of photoelectric catalysis and is a method for preparing a composite photoelectrode. Background Art
[0002] Photoelectrocatalysis refers to an advanced oxidation reaction that uses light and electricity to participate in the reaction. The structure of this system is consistent with that of electrocatalysis technology, and it also requires three parts: electrode, counter electrode and electrolyte. The difference is that this system also requires the use of an additional light source to illuminate the reaction cell.
[0003] Carbon quantum dots are a new type of nanoparticles, which are spherical in shape and less than 10 nanometers in diameter. They are widely used in ion detection, photoelectrocatalysis and other fields. The main high-quality properties of this nanomaterial include excitation wavelength-dependent photoluminescence (PL), chemical inertness and low toxicity, small particle size, good biocompatibility, and photoinduced electron transfer. Carbon quantum dots have very good physical and chemical properties. They not only have high fluorescence intensity but also excellent photoelectric properties. They have broad application prospects in the field of photoelectrocatalysis. At this stage, people have made use of the advantages of carbon quantum dots and have conducted extensive research and applications on them.
[0004] Tungsten trioxide (WO3) is a wide bandgap n-type semiconductor. Its excellent sensitivity and selectivity make it an important metal oxide gas-sensitive material. Tungsten trioxide has a strong absorption capacity for electromagnetic waves and can be used as an excellent solar energy absorption material and hidden material. In addition, the bandgap energy of tungsten trioxide is about 2.5eV, and it has potential photocatalytic ability in visible light with a wavelength of less than 500nm. Therefore, tungsten trioxide has potential application prospects in the treatment of water contaminated by organic dyes.
[0005] Oxygen vacancies are a common and important catalyst defect, which is formed by removing oxygen atoms from the metal oxide lattice. The introduction of such defects often helps to control the electronic and chemical properties of materials, change the adsorption energy, and enhance the intrinsic activity of their active sites, thereby improving catalytic performance. For example, studies have shown that the abundant oxygen vacancies in metal hydroxides are conducive to the adsorption of oxygen-containing intermediates on the active centers, thereby significantly improving their OER activity. Oxygen vacancy engineering has been demonstrated to be an effective catalyst modification strategy, which has advantages in constructing low-coordination metal sites and regulating the adsorption energy of OER intermediates. However, the two effects of oxygen vacancy engineering - regulating the catalyst electronic structure and serving as additional active sites - often exist simultaneously, which makes it challenging to distinguish and assign the electronic structure regulation of active sites and the electron transport of catalysts. Therefore, clarifying the contribution of each part and elucidating the key role of oxygen vacancy engineering is crucial to understand the electrocatalytic mechanism and design effective OER catalysts.
[0006] The present invention uses a hydrothermal method to prepare nitrogen and phosphorus doped carbon quantum dots (N, P-CQDs), and then uses a hydrothermal method and a surface reduction method to prepare tungsten trioxide (WO) containing oxygen vacancies. 3-x ), and finally the nitrogen-phosphorus-doped carbon quantum dots and tungsten trioxide containing oxygen vacancies were combined by hydrothermal method (N,P-CQDs / WO 3-x ) to obtain a composite photoelectrode. Summary of the invention
[0007] The present invention uses bagasse as a matrix, prepares nitrogen and phosphorus doped carbon quantum dots by a hydrothermal method, and then prepares tungsten trioxide containing oxygen vacancies as a carrier, loads the nitrogen and phosphorus doped carbon quantum dots onto the tungsten trioxide containing oxygen vacancies, and prepares a composite photoelectrode with strong stability, good photoelectrocatalytic performance, safety and non-toxicity, and the composite photoelectrode is used to degrade wastewater.
[0008] To achieve the above object, the present invention provides the following solutions:
[0009] (1) Preparation of nitrogen-phosphorus-doped carbon quantum dots (N,P-CQDs): Take 1.2g of fine powdered bagasse in a beaker, add 0.96g (NH4)2HPO4 and 30ml of deionized water and stir evenly, then transfer the obtained mixture into the PPL lining, and then put it into the reactor. Finally, place the reactor in a muffle furnace and react at 260°C for 12h. After the reactor cools down, take out the product in the PPL lining, filter it with a vacuum pump, and take the supernatant. Use a dialysis bag (500Da) for 12h to obtain a yellow-brown clear liquid. Replace the deionized water every 6h to obtain an N,P-CQDs solution. Freeze-dry the N,P-CQDs solution to obtain solid N,P-CQDs;
[0010] (2) Preparation of tungsten trioxide photoelectrode containing oxygen vacancies (WO 3-x ): First, 0.4g Na2WO4·2H2O and 0.2g (NH4)2C2O4 were dissolved in 33mL deionized water. Then, 9mL HCl was added to the solution, and a yellow precipitate was formed in the solution. Then, 8mL H2O2 was added to the mixed solution, and the solution became colorless and clear. Finally, 30mL anhydrous ethanol was added to the solution and stirred for 30min. At the same time, the 2×4cm 2 FTO conductive glass is placed in a beaker. The prepared solution is poured into the beaker containing FTO conductive glass and transferred to a constant temperature water bath at 85°C for 2 hours. After natural cooling, the electrode surface is repeatedly rinsed with deionized water. After WO3 is dried at room temperature, it is calcined at 500°C for 2 hours in a nitrogen atmosphere. The sample obtained is WO 3-x Photoanode;
[0011] (3) Preparation of tungsten trioxide composite photoelectrodes loaded with nitrogen and phosphorus doped carbon quantum dots containing oxygen vacancies (N,P-CQDs / WO 3-x ): Place the WO3-x photoanode in a beaker, add 15 ml of 1.5 g / L N, P-CQDs aqueous solution, seal, react at 80 ° C for 14 h, take out the solution after it cools to room temperature and put it in an oven, dry it at 60 ° C to obtain N, P-CQDs / WO 3-x .
[0012] 1. Preferably, the mass ratio of the bagasse, diammonium hydrogen phosphate and water in step (1) is 5:4:125.
[0013] 2. Preferably, the heating reaction temperature of the nitrogen and phosphorus doped carbon quantum dots in step (1) is 260°C.
[0014] 3. Specifically: The heating reaction time of the nitrogen and phosphorus doped carbon quantum dots described in step (1) is 12 hours.
[0015] 4. Preferably, the heating reaction temperature in step (2) is 85°C.
[0016] 5. Preferably, the heating reaction time in step (2) is 2 h.
[0017] 6. Specifically: the atmosphere of the high temperature calcination in step (2) is nitrogen.
[0018] 7. Specifically: the concentration of the nitrogen and phosphorus doped carbon quantum dot solution in step (3) is 1.5 g / L.
[0019] 8. Preferably, the heating reaction temperature in step (3) is 80°C.
[0020] 9. Preferably, the heating reaction time in step (3) is 14 hours.
[0021] 10. Preferably, the immobilization time in step (3) is 10 h.
[0022] N,P-CQDs / WO prepared by the present invention 3-x The composite photoelectrode is uniform in size and has good photoelectrocatalytic performance. It retains the characteristics of tungsten trioxide and has high stability. It has strong reusability and can be used in the photoelectrocatalytic wastewater treatment industry to treat toxic and harmful wastewater. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 N,P-CQDs / WO 3-x Effect diagram of photoanodic degradation of 4-chlorophenol;
[0024] Figure 2 WO3、WO 3-x and N,P-CQDs / WO 3-x Photoelectric degradation effect diagram of 4-chlorophenol;
[0025] Figure 3 WO3、WO 3-x and N,P-CQDs / WO 3-x XRD pattern of the surface;
[0026] Figure 4 WO3、WO 3-x and N,P-CQDs / WO 3-x UV-Vis diffuse reflectance spectrum;
[0027] Figure 5 WO3、WO 3-x and N,P-CQDs / WO 3-x Tauc curve graph; DETAILED DESCRIPTION
[0028] The present invention is further described below with reference to examples:
[0029] Example 1
[0030] A N,P-CQDs / WO 3-x The preparation method of the composite photoelectrode comprises the following steps:
[0031] 1) Preparation of nitrogen and phosphorus-doped carbon quantum dots (N,P-CQDs): Take 1.2g of fine powdered bagasse in a beaker, add 0.96g (NH4)2HPO4, 30ml of deionized water and stir evenly, then transfer the obtained mixture into the PPL lining, and then put it into the reactor. Finally, place the reactor in a muffle furnace and react at 260°C for 12h. After the reactor cools down, take out the product in the PPL lining, filter it with a vacuum pump, and take the supernatant. Use a dialysis bag (500Da) for 12h to obtain a yellow-brown clear liquid. Replace the deionized water every 6h to obtain an N,P-CQDs solution. Freeze-dry the N,P-CQDs solution to obtain solid N,P-CQDs;
[0032] (2) Preparation of tungsten trioxide photoelectrode containing oxygen vacancies (WO 3-x ): First, 0.4g Na2WO4·2H2O and 0.2g (NH4)2C2O4 were dissolved in 33mL deionized water. Then, 9mL HCl was added to the solution, and a yellow precipitate was formed in the solution. Then, 8mL H2O2 was added to the mixed solution, and the solution became colorless and clear. Finally, 30mL anhydrous ethanol was added to the solution and stirred for 30min. At the same time, the 2×4cm 2FTO conductive glass is placed in a beaker. The prepared solution is poured into the beaker containing FTO conductive glass and transferred to a constant temperature water bath at 85°C for 2 hours. After natural cooling, the electrode surface is repeatedly rinsed with deionized water. After WO3 is dried at room temperature, it is calcined at 500°C for 2 hours in a nitrogen atmosphere. The sample obtained is WO 3-x Photoanode;
[0033] (3) Preparation of tungsten trioxide composite photoelectrodes loaded with nitrogen and phosphorus doped carbon quantum dots containing oxygen vacancies (N,P-CQDs / WO 3-x ): will WO 3-x The photoanode was placed in a beaker, and 15 ml of 1.5 g / L N, P-CQDs aqueous solution was added. The mixture was sealed and reacted at 80 °C for 14 h. After the solution cooled to room temperature, it was taken out and placed in an oven and dried at 60 °C to obtain N, P-CQDs / WO. 3-x .
[0034] Example 2
[0035] The difference from Example 1 is that the dialysis time in step (1) is 18 h, and the other parameter conditions and operation steps are the same.
[0036] Example 3
[0037] The difference from Example 1 is that the amount of hydrochloric acid in step (2) is 3 ml, 6 ml, 12 ml and 15 ml, and the other parameter conditions and operating steps are the same.
[0038] Example 4
[0039] The difference from Example 1 is that the reaction temperatures in step (2) are 55°C, 65°C, 95°C and 105°C, and the other parameter conditions and operating steps are the same.
[0040] Example 5
[0041] The difference from Example 1 is that the reaction time in step (2) is 3 h, 4 h, 5 h and 6 h, and the other parameter conditions and operation steps are the same.
[0042] Example 6
[0043] The difference from Example 1 is that the concentration of the N,P-CQDs aqueous solution in step (3) is 0.5 g / L, 1 g / L, 2 g / L and 2.5 g / L, and the other parameter conditions and operating steps are the same.
[0044] Example 7
[0045] The difference from Example 1 is that the heating temperatures in step (3) are 60° C., 70° C., 90° C. and 100° C., and the other parameter conditions and operating steps are the same.
[0046] Example 8
[0047] The difference from Example 1 is that the heating time in step (3) is 6 h, 8 h, 10 h and 12 h, and the other parameter conditions and operating steps are the same.
[0048] The N,P-CQDs / WO prepared in Examples 1 to 8 above 3-x The composite photoelectrode was tested and analyzed. The reagents and instruments used in the experiment are as follows:
[0049] Bagasse powder: Bagasse from Nanning Sugar Factory in Guangxi was processed by our research group. Sodium tungstate: Shanghai Aladdin Biochemical Technology Co., Ltd.; ammonium oxalate: Sinopharm Chemical Reagent Co., Ltd.; diammonium hydrogen phosphate: Sinopharm Chemical Reagent Co., Ltd.; hydrochloric acid: Sinopharm Chemical Reagent Co., Ltd.; anhydrous ethanol: Sinopharm Chemical Reagent Co., Ltd.; hydrogen peroxide (30%): Sinopharm Chemical Reagent Co., Ltd. Freeze dryer: FD-1A-50+, Boyikang Instrument Co., Ltd.; X-ray diffractometer: Rigaku miniflex600, Japan; UV-Vis-DRS: RG5000J.
[0050] N,P-CQDs / WO 3-x Composite photoelectrode effect analysis and structure analysis:
[0051] 1. Effect of N, P-CQDs concentration on N, P-CQDs / WO 3-x Effect of photoanode on the degradation of 4-chlorophenol
[0052] Prepare N,P-CQDs / WO according to the method described in Example 1 3-x , put the WO3 photoanode in a beaker, add 10ml of 0.5, 1, 1.5, 2, 2.5g / L N, P-CQDs aqueous solution, seal, react at 85℃ for 14h, take out the solution after it cools to room temperature and put it in an oven, dry it at 60℃ and finally get N, P-CQDs / WO3. The removal rate of 4-chlorophenol under 60min condition is taken as the examination index to investigate the removal rate of 4-chlorophenol by photoanode loaded with different N, P-CQDs concentrations. The electrolysis conditions are: 100mL of 4-chlorophenol with an initial concentration of 10mg / L, 2g / L of Na2SO4 concentration, and a bias voltage of 1.2V. The photoelectrocatalytic experiment is carried out in a photoelectrochemical reactor, using a 300w xenon lamp light source, and using a filter to filter out part of the light with a wavelength less than 420nm, and the electrolysis time is 60min. After the test, the degradation rate of 4-CP by the photoanode was calculated according to the following formula: (initial 4-CP concentration - 4-CP concentration at 60 minutes) / initial 4-CP concentration. Figure 1It can be seen that when the electrolysis time is 60 min, the degradation effect is best when the N, P-CQDs concentration is 1.5 g / L, and the degradation effect is 25.7%.
[0053] 2. WO3, WO 3-x and N,P-CQDs / WO 3-x Determination of photoelectrode photocatalytic degradation effect
[0054] Depend on Figure 2 It can be seen that the degradation effect of WO3 after loading N, P-CQDs has been improved. After 150 minutes of reaction, the degradation rate of 4-CP increased from 43.45% to 65.33%, an increase of 21.88%. This is because the doping of N, P-CQDs promotes the charge conduction on the catalyst surface, provides more reactive sites, and improves the catalytic efficiency of 4-CP. 3-x The N,P-CQDs loaded photoanode has a 4-CP degradation rate of 72.71%, which is 7.38% higher than the 65.33% 4-CP removal efficiency of WO3 / N,P-CQDs photoanode. 3-x Oxygen vacancies in the photoanode can improve the catalytic performance in the photoelectrocatalytic system and increase the degradation efficiency of the photoanode for pollutants.
[0055] 3. X-ray diffractometer (XRD) analysis of WO3, WO 3-x and N,P-CQDs / WO 3-x Crystal structure of the photoelectrode
[0056] Figure 3 The XRD patterns of WO3 and N,P-CQDs / WO3 are shown in Figure 2. The diffraction peaks of WO3 samples at 23.1°, 23.5°, 24.3°, 42.6°, 50.2° and 56.2° correspond to the (002), (020), (200), (222), (232) and (241) crystal planes of monoclinic WO3, respectively. This result shows that the laboratory has successfully synthesized WO3 thin films by in-situ hydrothermal method, and the diffraction peaks all show strong and sharp characteristics, indicating that the obtained WO3 thin films have good crystallinity. 3-x The successful preparation of WO3 has changed some of its crystal forms but still retained the characteristic peaks of WO3. In addition, XRD characterization of N,P-CQDs / WO3 composite samples was also performed. Figure 3It can be seen that after the modification of N, P-CQDs by surface adsorption method, the N, P-CQDs / WO3 sample still conforms to the characteristic peak type of typical WO3, indicating that the crystal structure of WO3 itself is well maintained during the surface modification process. At the same time, due to the low content and large dispersion of N, P-CQDs in the sample, the characteristic diffraction peaks corresponding to N, P-CQDs cannot be observed in the XRD spectrum. Based on the above results, the experiment successfully prepared WO3 with good crystallinity. After the surface compounding of N, P-CQDs, the lattice structure of WO3 was not affected (N, P-CQDs did not enter the WO3 lattice but only compounded on the surface), and no other impurities appeared in the sample, and the prepared catalyst had a high purity.
[0057] 4. WO3, WO 3-x and N,P-CQDs / WO 3-x UV-Vis diffuse reflectance spectrum
[0058] Figure 4 It shows that after the oxygen vacancies are formed, the oxygen atoms in the WO3 structure escape, which increases the specific surface area of WO3 and improves the absorbance in the visible light region. 3-x The absorbance intensity of the photoanode in the visible light region is significantly enhanced, which may be due to the promotion of electron transfer and upconversion effect by N,P-CQDs.
[0059] 5. WO3, WO 3-x and N,P-CQDs / WO 3-x Tauc Curve
[0060] Depend on Figure 5 It can be seen that WO3, WO 3-x and N, P-CQDs / WO 3-x The band gap values of WO3 are 2.33, 2.25, and 1.57, respectively. The formation of oxygen vacancies and the loading of N and P-CQDs reduce the band gap of WO3, making WO 3-x and N,P-CQDs / WO 3-x The energy required to transfer electrons is reduced, the efficiency of electron transfer is increased, and the photoelectrocatalytic ability of WO3 is greatly improved, which can reasonably explain Figure 2 N,P-CQDs / WO 3-x The principle of best degradation effect.
[0061] Although the above describes the specific implementation mode of the present invention in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art on the basis of the technical solution of the present invention without creative work are still within the scope of protection of the present invention.
Claims
1. A N,P-CQDs / WO with good photoelectrocatalytic effect 3-x The method for preparing a composite photoanode is characterized by: The following steps are involved: (1) Preparation of nitrogen and phosphorus-doped carbon quantum dots (N, P-CQDs): Take 1.2 g of fine powdered bagasse in a beaker, add 0.96 g (NH4)2HPO4 and 30 ml of deionized water and stir evenly, then transfer the obtained mixture into the PPL lining, and then put it into the reactor. Finally, place the reactor in a muffle furnace and react at 260°C for 12 hours. After the reactor is cooled down, take out the product in the PPL lining, filter it with a vacuum pump, and take the supernatant. Use a dialysis bag (500Da) for 12 hours to obtain a yellow-brown clear liquid. Replace the deionized water every 6 hours to obtain an N, P-CQDs solution. Freeze-dry the N, P-CQDs solution to obtain solid N, P-CQDs; (2) Preparation of tungsten trioxide photoanode containing oxygen vacancies (WO 3-x ): First, 0.4g Na2WO4·2H2O and 0.2g (NH4)2C2O4 were dissolved in 33mL deionized water. Then, 9mL HCl was added to the solution, and a yellow precipitate was formed in the solution. Then, 8mL H2O2 was added to the mixed solution, and the solution became colorless and clear. Finally, 30mL anhydrous ethanol was added to the solution and stirred for 30min. At the same time, the 2×4cm 2 FTO conductive glass is placed on the wall of a 15mL beaker. The prepared solution is poured into the 15mL beaker containing FTO conductive glass and transferred to a constant temperature water bath at 85℃ for 2h. After natural cooling, the anode surface is repeatedly rinsed with deionized water. After WO3 is dried at room temperature, it is calcined at 400℃ for 2h in a nitrogen atmosphere. The sample obtained is WO 3-x Photoanode; (3) Preparation of tungsten trioxide composite photoanode loaded with nitrogen and phosphorus doped carbon quantum dots containing oxygen vacancies (N, P-CQDs / WO 3-x ): will WO 3-x The photoanode was placed in a beaker, and 15 ml of 1.5 g / L N, P-CQDs aqueous solution was added. The beaker was sealed and reacted at 80 °C for 14 h. After the solution cooled to room temperature, it was taken out and placed in an oven and dried at 60 °C to obtain N, P-CQDs / WO. 3-x .
2. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The mass ratio of bagasse, diammonium hydrogen phosphate and water in step (1) is 5:4:
125.
3. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction temperature of the nitrogen and phosphorus doped carbon quantum dots in step (1) is 260°C.
4. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction time of the nitrogen and phosphorus doped carbon quantum dots in step (1) is 12 hours.
5. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction temperature in step (2) is 85°C.
6. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction time of step (2) is 2 hours.
7. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The concentration of the nitrogen and phosphorus doped carbon quantum dot solution in step (3) is 1.5 g / L.
8. The method for preparing the tungsten trioxide composite photoanode containing oxygen vacancies loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction temperature in step (3) is 80°C.
9. The method for preparing a tungsten trioxide composite photoanode containing oxygen vacancies and loaded with nitrogen and phosphorus doped carbon quantum dots according to claim 1, characterized in that: The heating reaction time of step (3) is 14 hours.
10. The method for preparing a tungsten trioxide composite photoanode containing oxygen vacancies and loaded with nitrogen and phosphorus doped carbon quantum dots according to any one of claims 1 to 10, characterized in that: The prepared tungsten trioxide composite photoanode loaded with nitrogen and phosphorus doped carbon quantum dots and containing oxygen vacancies is used for photoelectric degradation of wastewater.
Citation Information
Patent Citations
Preparation of biochar quantum dot metal doped AgVO4 composite photocatalyst
CN111437817A
Preparation method of defective WO3 photo-anode
CN114134515A
Treatment process for organic wastewater of liquid crystal panel factory
CN117125769A