Special high-molecular water-retaining viscosity reducer for UHPC (Ultra High Performance Concrete) and preparation method thereof

Through free radical polymerization, a polymer water-retaining and viscosity reducing agent is synthesized to form a three-dimensional network structure, which solves the viscosity problem of UHPC concrete at low water-adhesion ratio, improves construction performance and durability, and achieves the excellent rheological performance and economy of UHPC Production.

CN118908623APending Publication Date: 2024-11-08江苏博思通新材料有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411150324.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the viscosity of UHPC concrete under low water bonding ratio, resulting in increased construction difficulty, reduced density, and poor strength and durability.

Method used

The polymer water-retaining and viscosity-reducing agent is synthesized by free radical polymerization. By constructing appropriate molecular weight and molecular structures, a three-dimensional network structure is formed to affect the arrangement of powder and aggregates, reduce viscosity, and at the same time, cellulose ether is introduced to improve water solubility and thickening.

Benefits of technology

It significantly reduces the viscosity of UHPC mixture, improves construction performance and rheology performance, ensures strength and durability, and has low product dosage and high cost-effectiveness, which is suitable for industrial development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908623A_ABST
    Figure CN118908623A_ABST
Patent Text Reader

Abstract

The invention discloses a special high-molecular water-retention viscosity reducer for UHPC (Ultra High Performance Concrete) and a preparation method of the special high-molecular water-retention viscosity reducer. The special high-molecular water-retention viscosity reducer is mainly prepared by copolymerizing acrylamide small monomers, acrylic acid small monomers, polyether large monomers and alkenyl sulfonate and then adding cellulose ether into a product. The high-molecular water-retention type viscosity reducer is synthesized in a free radical polymerization mode, a proper balance point is achieved mainly by constructing molecular weight and molecular structure, and a three-dimensional network structure water body is formed by hydrophilic groups and free water in a system, so that the arrangement mode of powder and aggregate in slurry is influenced, and the viscosity is influenced; the viscosity reducer is a breakthrough in the development direction, preparation and application technology of the traditional viscosity reducer, enriches and improves the defects of the prior art, and solves the limitation of the application of the existing viscosity reducer in UHPC (Ultra High Performance Concrete).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a high molecular water-retaining UHPC special viscosity reducer and a preparation method thereof. Background Art

[0002] Ordinary concrete materials have good characteristics such as good compression resistance, impermeability, plasticity and construction ability. They have been widely used in infrastructure construction since the mid-20th century. Today, concrete has become the most used building material in the world. However, ordinary concrete has defects such as low tensile strength, high brittleness, easy cracking and heavy weight, which cannot meet the development of building structures towards lightness, large span, durability and environmental protection. Therefore, it is necessary to further study and develop high-strength and durable concrete materials to meet the needs of modern infrastructure construction. In order to make up for the shortcomings of ordinary concrete, UHPC came into being and has been developed for more than 40 years. A large number of studies have shown that compared with ordinary concrete, UHPC has the advantages of super strong mechanical properties, high construction, light weight and ultra-high durability. However, due to the immaturity of technical research, especially the opening of the concrete state and the increase in viscosity under ultra-low water-cement ratio, the difficulty of concrete construction has increased. This has limited the application of UHPC concrete and has never been properly promoted and applied. The third generation of polycarboxylic acid-based water reducers has a high water reduction rate and can effectively reduce the water consumption of UHPC, but it cannot solve the problem of increased viscosity of UHPC caused by low water-binder ratio. Therefore, it is urgent to develop new admixtures with viscosity reduction effect to solve the problem of UHPC in actual engineering applications.

[0003] In the existing technology, patent CN109651566A discloses a viscosity-reducing polycarboxylic acid water-reducing agent and a preparation method thereof, which is prepared by copolymerizing block-modified unsaturated polyoxyethylene ether, unsaturated carboxylic acid, and functional monomer under the action of an initiator and a chain transfer agent and neutralizing with alkali. The main effect is that the block polyether side chain contains a hydrophobic group. The polyether reduces the HLB value by adding propylene oxide, reduces the free water and the molecule, and exhibits a low viscosity and high water-reducing effect to achieve the purpose of viscosity reduction. According to the embodiments of the patent, the invention is mainly used for concrete with a 28d compressive strength of about 70MPa. This product achieves the effect of reducing viscosity by air entrainment, which is not suitable for the application scenario of UHPC; Patent CN116283030A early strength viscosity reducing water reducer and its preparation method are prepared by a water reducing component including a linear monomer of acrylic monomer and a first polyether macromonomer block polymerization and an early strength collapse protection component, and the raw materials include: 25-35 parts of concentrated tetradecyl ester, 90-110 parts of a second polyether macromolecule, 2-6 parts of sodium xylene sulfonate, 1-10 parts of sodium calcium sulfate and 1-10 parts of sodium aluminate, so that the concrete has excellent early strength and viscosity reduction effects. This patent is more like a combination of water reduction, collapse protection and early strength to achieve the stated purpose. From the perspective of the raw materials used, calcium nitrate and sodium aluminate are designed as early strength agents, which have an adverse effect on the density of concrete structures, so this series of products cannot be used in UHPC systems; Patent CN110172128B A brush-type polycarboxylic acid high-efficiency viscosity-reducing water-reducing agent and its preparation method use ammonium persulfate as an initiator, maleic anhydride, vinyl triethoxysilane, and allyl alcohol polyoxyethylene ether as monomers, and mercaptopropionic acid as a chain transfer agent, and are obtained through addition polymerization. Maleic anhydride with high carboxyl density and silane coupling agents containing silanols are used to enhance the adsorption amount of polycarboxylic acid water-reducing agent on the surface of the gelling component, improve the surface activity of the polycarboxylic acid water-reducing agent, significantly reduce the surface tension of the liquid phase of the gelling material system, and achieve extremely strong adsorption and steric hindrance effects. Although the invention can be used in the UHPC system, it is still a way to increase the water reduction rate to achieve the purpose of viscosity reduction, which is quite different from reducing the viscosity between the components in the system by using a viscosity-reducing agent, and from the results of the embodiment, the product conversion rate is not high, all below 85%, and the material cost is wasted. The existing technology mainly adopts the following methods: 1. reducing the molecular weight of polymer; 2. reducing the length of PEG side chain in polyether monomer and the modification of PEG side chain; 3. introducing hydrophobic and rigid groups such as methyl, ester, phenyl, etc. into the molecular structure to increase the hydrophobicity of the product, so as to reduce the binding with water, release free water to the maximum extent and reduce the viscosity of concrete. Obviously, these methods are contrary to the characteristics of low water-binder ratio and high density of UHPC, and it is difficult to achieve the purpose of viscosity reduction in UHPC system. Summary of the invention

[0004] Purpose of the invention: In order to solve the problems existing in the prior art, the purpose of the present invention is to provide a high molecular weight water-retaining UHPC special viscosity reducer and its preparation method, which mainly solves the problems of low water-cement ratio and complex cementitious component system of UHPC concrete with high viscosity and poor workability, and also solves the problem that the introduction of existing hydrophobic viscosity reducers leads to reduced density of UHPC system and deterioration of strength and durability. The present invention adopts free radical polymerization to synthesize high molecular weight water-retaining viscosity reducer, which mainly affects the arrangement of powder and aggregate in slurry and thus affects viscosity by constructing a suitable balance point between molecular weight and molecular structure and then forming a three-dimensional network structure water body with free water in the system through various hydrophilic groups. It is a breakthrough in the development direction, preparation and application technology of traditional viscosity reducers, enriches and improves the deficiencies of existing technologies, and solves the limitations of existing viscosity reducers in UHPC applications.

[0005] Technical solution: In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0006] A high molecular weight water-retaining UHPC special viscosity reducer is mainly obtained by copolymerizing acrylamide small monomers, acrylic acid small monomers, polyether macromonomers and olefin sulfonate, and then adding cellulose ether to the product.

[0007] As a specific implementation, the acrylamide small monomer is one or a combination of acrylamide, N-tert-butylacrylamide, N-alkylacrylamide, N-benzylacrylamide, N-dodecylacrylamide, N,N-dimethylacrylamide, and 2-acrylamido-2-methylpropanesulfonic acid.

[0008] As a specific implementation, the acrylic small monomer is a combination of two or more of acrylic acid, itaconic anhydride, 2-methylmaleic anhydride, methacrylic acid, fumaric acid, maleic acid and methyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl methacrylate, and ethylene glycol methacrylate phosphate, and the combination includes at least one acid and one ester.

[0009] As a specific implementation, the polyether macromonomer is one of methyl allyl polyoxyethylene ether, isopentenyl polyoxyethylene ether, and ethylene glycol monovinyl polyoxyethylene ether; the molecular weight of the polyether macromonomer is 750-5000.

[0010] As a specific embodiment, the olefin sulfonate is one of sodium methyl propylene sulfonate, sodium propylene sulfonate and styrene sulfonic acid.

[0011] As a specific embodiment, the cellulose ether is one of methyl hydroxyethyl cellulose ether, methyl hydroxypropyl cellulose ether and hydroxyethyl cellulose ether.

[0012] As a specific implementation scheme, the molecular weight of the copolymerization product is 250,000 to 400,000 (all molecular weight values ​​in the present invention are rounded to 10,000).

[0013] The present invention also provides a method for preparing the polymer water-retaining UHPC special viscosity reducer, comprising the following steps:

[0014] Under alkaline conditions, acrylamide small monomers, acrylic acid small monomers, polyether macromonomers and olefin sulfonates are subjected to free radical polymerization reaction under the joint action of an initiator, a reducing agent and a catalyst to obtain a copolymer product, which is diluted with water and then added with cellulose ether to obtain the polymer water-retaining UHPC special viscosity reducer.

[0015] As a specific implementation scheme, the alkaline conditions refer to a NaOH aqueous solution or a KOH aqueous solution with a mass concentration of 0.5% to 1.0%; the molar ratio of the acrylamide small monomer, acrylic acid small monomer, polyether macromonomer, olefin sulfonate, initiator and reducing agent is 1: (2.0 to 4.0): (0.05 to 0.20): (0.01 to 0.02): (0.01 to 0.03): (0.005 to 0.01).

[0016] As a specific implementation scheme, the initiator is one or a combination of hydrogen peroxide, ammonium persulfate, sodium persulfate and potassium persulfate; the reducing agent is one or a combination of sodium formaldehyde sulfoxylate, L-ascorbic acid and sodium bisulfite; the catalyst is FeSO4•7H2O, preferably dissolved into a solution with a mass fraction of 0.05%-0.2%.

[0017] As a specific implementation scheme, the temperature of the free radical polymerization reaction is 40°C to 60°C, and the reaction time is 30min to 60min; the dilution with water is to dilute to a solid content of 2.0% to 5.0%; and the amount of cellulose ether added is 0.1% to 0.5%.

[0018] In the above method, in order to make the polymer structure uniform and stable and prevent chain breakage during polymerization, the stirring rate needs to be reduced and should be controlled at 30 rpm / min to 50 rpm / min; in order to prevent the polymer from exploding, the base material concentration should be controlled at 10% to 20%. Preferably, the reducing agent sample is added by dropwise addition, and the dropwise addition time is 10 min to 30 min.

[0019] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0020] 1. The product of the present invention has a low dosage and can significantly reduce the viscosity of the UHPC mixture slurry at an extremely low dosage, effectively solving the problem of high viscosity and difficult construction of UHPC.

[0021] 2. It has good compatibility with polycarboxylic acid water reducer. When mixed with water reducer, it will not affect the homogeneity, water reduction rate and other characteristics of the water reducer.

[0022] 3. The present invention is a new type of high molecular polymer, which enables the viscosity of UHPC to reach a better balance between fluidity, permeability and cohesion of concrete, thereby obtaining excellent rheological properties. Such excellent rheological properties cannot be achieved by increasing the amount of water reducer or adding water.

[0023] 4. The product of the present invention is a water-soluble high molecular polymer that can form a three-dimensional network structure, produce thixotropic flow properties to prevent sedimentation and improve anti-sagging properties, thereby obtaining optimal construction performance.

[0024] 5. The cellulose ether introduced into the product of the present invention has good water solubility and thickening properties, and can form a stable colloid in concrete, thereby increasing viscosity and improving fluidity.

[0025] 6. The preparation process of the present invention is simple, short in time, low in energy consumption, low in requirements for production equipment, and various raw materials are readily available, which is suitable for industrial development. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is the peak time of different polymer water-retaining viscosity reducers. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] At 40°C and with FeSO4•7H2O as the catalyst, add 0.7mol N,N-dimethylacrylamide and 0.3mol N-dodecylacrylamide, 2mol 2-methylmaleic anhydride and 1mol hydroxyethyl acrylate, 0.1mol isopentyl polyoxyethylene ether with a molecular weight of 2400, 0.01mol sodium methyl propylene sulfonate and 0.015mol potassium persulfate to the KOH aqueous solution with a mass concentration of 1.0%, and at the same time, add 0.005mol L-ascorbic acid to the above solution at a uniform speed of 10min. The stirring rate of the system should be controlled at 30 rpm / min, and the copolymer product is obtained by stirring for 30min. After diluting with water to a solid content of 2.0%, 0.3% methyl hydroxypropyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 380000, which is recorded as U1.

[0030] Example 2

[0031] At 40°C and with FeSO4•7H2O as the catalyst, add 1 mol N,N-dimethylacrylamide, 1 mol acrylic acid and 1 mol methyl acrylate, 0.05 mol 750 molecular weight methyl allyl polyoxyethylene ether, 0.02 mol styrene sulfonic acid and 0.01 mol sodium persulfate to a 0.5% mass concentration NaOH aqueous solution, and at the same time, add 0.01 mol sodium formaldehyde sulfoxylate to the above solution at a uniform rate of 30 minutes. The stirring rate of the system should be controlled at 40 rpm / min, and the copolymer product is obtained by stirring for 60 minutes. After diluting with water to a solid content of 5.0%, 0.1% hydroxyethyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 300,000, which is recorded as U2.

[0032] Example 3

[0033] At 40°C and with FeSO4•7H2O as the catalyst, add 0.1mol N-benzyl acrylamide and 0.9mol acrylamide, 2mol maleic acid and 2mol ethylene glycol methacrylate phosphate, 0.2mol 1000 molecular weight ethylene glycol monovinyl polyoxyethylene ether, 0.015mol sodium propylene sulfonate and 0.03mol hydrogen peroxide to a 0.6% mass concentration NaOH aqueous solution, and at the same time, add 0.01mol L-ascorbic acid to the above solution at a uniform speed for 20min. The stirring rate of the system should be controlled at 50 rpm / min, and the copolymer product is obtained by stirring for 50min. After diluting with water to a solid content of 4.0%, 0.15% methyl hydroxyethyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 400000, which is recorded as U3.

[0034] Example 4

[0035] At 40℃ and with FeSO4•7H2O as catalyst, add 0.4mol N-tert-butyl acrylamide and 0.6mol N-alkyl acrylamide, 1mol fumaric acid and 2mol methyl methacrylate, 0.05mol ethylene glycol monovinyl polyoxyethylene ether with a molecular weight of 5000, 0.018mol sodium methyl propylene sulfonate and 0.01mol hydrogen peroxide and 0.01mol ammonium persulfate, and at the same time, add 0.008mol sodium bisulfite to the above solution at a uniform speed for 25min. The stirring rate of the system should be controlled at 35 rpm / min, and the copolymer product is obtained by stirring for 50min. After diluting with water to a solid content of 3.0%, 0.20% methyl hydroxyethyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 350000, which is recorded as U4.

[0036] Example 5

[0037] At 40°C and with FeSO4•7H2O as the catalyst, add 0.2mol N2-acrylamido-2-methylpropanesulfonic acid and 0.8mol acrylamide, 1mol itaconic anhydride and 1mol hydroxypropyl acrylate, 0.08mol ethylene glycol monovinyl polyoxyethylene ether with a molecular weight of 3000, 0.015mol sodium methyl propylene sulfonate and 0.025mol ammonium persulfate to the KOH aqueous solution with a mass concentration of 0.8%, and at the same time, add 0.005mol sodium bisulfite and 0.005mol L-ascorbic acid to the above solution at a uniform speed for 30min. The stirring rate of the system should be controlled at 45 rpm / min, and the copolymer product is obtained by stirring for 50min. After diluting with water to a solid content of 2.0%, 0.5% methyl hydroxyethyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 280000, which is recorded as U5.

[0038] Example 6

[0039] At 40°C and with FeSO4•7H2O as the catalyst, add 0.4mol N-tert-butylacrylamide and 0.6mol N-alkylacrylamide, 1.5mol acrylic acid and 1.5mol methyl acrylate, 0.15mol methyl allyl polyoxyethylene ether with a molecular weight of 2900, 0.01mol styrene sulfonic acid and 0.03mol potassium persulfate to the NaOH aqueous solution with a mass concentration of 0.5%, and at the same time, add 0.009mol sodium formaldehyde sulfoxylate to the above solution at a uniform speed for 30min. The stirring rate of the system should be controlled at 40 rpm / min, and the copolymer product is obtained by stirring for 60min. After diluting with water to a solid content of 5.0%, 0.1% methyl hydroxypropyl cellulose ether is added to obtain a high molecular weight water-retaining viscosity reducer with a molecular weight of 250,000, which is recorded as U6.

[0040] Test on the effect of high molecular water-retaining UHPC special viscosity reducer: Referring to GB8076-2008 "Concrete Admixtures", GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures", GB / T50082-2019 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete" and GB / T31387 "Reactive Powder Concrete", the viscosity comparison test of Examples 1 to 6 and the blank group was carried out. The specific UHPC mix ratio and test results are shown in Tables 1, 2 and 3. The water reducer used in the experiment is the BST-309 highly adaptable polycarboxylic acid water reducer of Jiangsu Bositong New Materials Co., Ltd., with a solid content of 30%; the GPC spectrum of the molecular weight peak comparison of the high molecular water-retaining viscosity reducers U1 to U6 of the present invention is shown in Figure 1 .

[0041] Table 1 UHPC mix ratio Unit: kg / m 3

[0042]

[0043] Table 2 Viscosity test results of different samples of UHPC

[0044]

[0045] The shorter the stirring and T500 time is, the lower the slurry viscosity is and the better the viscosity reducing effect of the viscosity reducer is.

[0046] Table 3 Strength and durability test results of UHPC of different samples

[0047]

[0048] It can be found from the test results of Table 2 and Table 3 that when the U1-U6 polymer water-retaining viscosity reducer prepared by the present invention is used in UHPC, it has a faster slurry discharge time, a faster T500 flow rate, and a lower viscosity, so that the slurry has better working performance. The introduction of the product of the present invention enables the UHPC adhesive system to fully exert its characteristics, so it has significant performance in mechanical properties and later durability.

[0049] The implementation modes of the present invention have been described in detail above in conjunction with specific embodiments, but the present invention is not limited to the above-mentioned implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A polymer water-retaining UHPC special viscosity reducer, characterized in that: The viscosity reducer is mainly obtained by copolymerizing acrylamide small monomers, acrylic acid small monomers, polyether macromonomers and olefin sulfonate, and then adding cellulose ether into the product.

2. The polymer water-retaining UHPC special viscosity reducer according to claim 1, characterized in that: The acrylamide small monomer is one or a combination of acrylamide, N-tert-butyl acrylamide, N-alkyl acrylamide, N-benzyl acrylamide, N-dodecyl acrylamide, N,N-dimethyl acrylamide, and 2-acrylamido-2-methylpropanesulfonic acid.

3. The polymer water-retaining UHPC special viscosity reducer according to claim 1, characterized in that: The acrylic small monomer is a combination of two or more of acrylic acid, itaconic anhydride, 2-methylmaleic anhydride, methacrylic acid, fumaric acid, maleic acid and methyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl methacrylate, and ethylene glycol methacrylate phosphate, and the combination includes at least one acid and one ester.

4. The polymer water-retaining UHPC special viscosity reducer according to claim 1, characterized in that: The polyether macromonomer is one or a combination of methyl allyl polyoxyethylene ether, isopentenyl polyoxyethylene ether, ethylene glycol monovinyl polyoxyethylene ether; the molecular weight of the polyether macromonomer is 750-5000.

5. The polymer water-retaining UHPC special viscosity reducer according to claim 1, characterized in that: The olefin sulfonate is one of sodium methyl propylene sulfonate, sodium propylene sulfonate and styrene sulfonic acid; the cellulose ether is one of methyl hydroxyethyl cellulose ether, methyl hydroxypropyl cellulose ether and hydroxyethyl cellulose ether.

6. The polymer water-retaining UHPC special viscosity reducer according to claim 1, characterized in that: The molecular weight of the copolymerized product is 250,000 to 400,000.

7. The method for preparing the polymer water-retaining UHPC special viscosity reducer according to any one of claims 1 to 6, characterized in that: The following steps are involved: Under alkaline conditions, acrylamide small monomers, acrylic acid small monomers, polyether macromonomers and olefin sulfonates are subjected to free radical polymerization reaction under the joint action of an initiator, a reducing agent and a catalyst to obtain a copolymer product, which is diluted with water and then added with cellulose ether to obtain the polymer water-retaining UHPC special viscosity reducer.

8. The method for preparing the polymer water-retaining UHPC special viscosity reducer according to claim 7, characterized in that: The alkaline conditions mentioned above refer to a NaOH aqueous solution or a KOH aqueous solution with a mass concentration of 0.5% to 1.0%; the molar ratio of the acrylamide small monomer, acrylic acid small monomer, polyether macromonomer, olefin sulfonate, initiator and reducing agent is 1: (2.0 to 4.0): (0.05 to 0.20): (0.01 to 0.02): (0.01 to 0.03): (0.005 to 0.01).

9. The method for preparing the polymer water-retaining UHPC special viscosity reducer according to claim 7, characterized in that: The initiator is one or a combination of hydrogen peroxide, ammonium persulfate, sodium persulfate and potassium persulfate; the reducing agent is one or a combination of sodium formaldehyde sulfoxylate, L-ascorbic acid and sodium bisulfite; the catalyst is FeSO4•7H2O, preferably dissolved into a solution with a mass fraction of 0.05%-0.2%.

10. The method for preparing the polymer water-retaining UHPC special viscosity reducer according to claim 7, characterized in that: The temperature of the free radical polymerization reaction is 40°C to 60°C, and the reaction time is 30min to 60min; the dilution with water is to dilute to a solid content of 2.0% to 5.0%; and the amount of cellulose ether added is 0.1% to 0.5%.