Preparation process of starch additive for glue preparation
By combining gelatinized starch with antioxidant, a starch-based adhesive with high viscosity and good antioxidant properties was prepared, which solved the problems of low viscosity and poor anti-mold properties of starch additives, and achieved more stable adhesive Performance and longer service life.
Patent Information
- Application Number
- CN202410948730.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
AI Technical Summary
The low viscosity, poor water resistance and poor mildew resistance of existing starch additives limit their application in the field of adhesives.
The starch-based adhesive is prepared by combining gelatinized starch with antioxidants, and an antioxidant is added to improve its viscosity, antioxidant properties and anti-mold properties.
It significantly improves the viscosity, antioxidant properties and anti-mold properties of starch additives, forms a more stable three-dimensional network structure, enhances its adhesion and wettability, and extends its service life.
Smart Images

Figure BDA0004946512670000041 
Figure BDA0004946512670000141 
Figure BDA0004946512670000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of starch additive preparation, and in particular relates to a preparation process of a starch additive for glue making. Background Art
[0002] With the rapid development of industrialization, adhesives, as an indispensable and important material in industry, have been applied in many fields including packaging, construction, automobiles, electronics, etc. However, petroleum-based raw materials are often used in the preparation process of traditional adhesives, which not only increases production costs but also causes serious pollution to the environment. Therefore, developing an environmentally friendly, efficient and low-cost adhesive preparation process has become a hot topic in current research.
[0003] As a natural polymer compound, starch has the advantages of wide sources, low price, renewable, and easy biodegradation, making it an ideal raw material for preparing environmentally friendly adhesives. However, due to the characteristics of its molecular structure, starch has defects such as poor fluidity, poor water resistance, and easy mildew when used directly as an adhesive, which limits its application in the adhesive field. In order to overcome these problems, researchers have modified starch and changed its molecular structure and properties through physical, chemical or biological methods to prepare starch-based adhesives with excellent performance.
[0004] Patent CN 110484168 B discloses a method for preparing a low-cost, high-viscosity acrylic adhesive, comprising the following steps: (1) preparing a modified starch additive, (2) weighing raw materials, and (3) preparing a finished product. The invention provides a method for preparing an acrylic adhesive, which has a simple process, reasonable combinations of steps, and is easy to promote and apply. The acrylic adhesive prepared has the advantages of high adhesion, good waterproofness, wide applicability to materials, and good thermal conductivity. However, the viscosity, water resistance, and mildew resistance of the adhesive prepared by this method still have room for improvement. Summary of the invention
[0005] The purpose of the present invention is to provide a preparation process of a starch additive for glue making, which is used to solve the technical problems of low viscosity, poor water resistance and poor mildew resistance of the starch additive in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a preparation process of a starch additive for glue making, comprising the following steps:
[0008] Step (1): adding distilled water to a container, adding starch while stirring, and after the starch is completely added, heating and stirring continuously to obtain gelatinized starch;
[0009] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0010] Step (3): Mixing the obtained starch-based adhesive with an antioxidant to obtain a starch-based mixture, then dissolving sodium hydroxide with distilled water and adding it to the starch-based mixture, continuing to stir to form a glue solution, adjusting the pH, and obtaining a starch additive for glue making.
[0011] Preferably, in step (1), the ratio of distilled water to starch is (1200-1500) mL: (150-200) g, the heating and stirring temperature is 60-70° C., and the time is 20-30 min.
[0012] Preferably, in step (2), the method for preparing the starch-based adhesive comprises the following steps:
[0013] Q1: The gelatinized starch and glacial acetic acid are mixed, stirred and heated, and then phthalic anhydride is added to react by stirring, and then methanesulfonic acid is added. After stirring and reacting, distilled water is added to terminate the reaction to obtain a crude product, which is filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0014] Q2: Add esterified starch, 1,3-butanediol and polyethylene glycol into a container and mix them. Add N,N-dimethylformamide to dissolve it. Heat the container while stirring until it is completely dissolved and in liquid form. Add isophorone diisocyanate and dibutyltin dilaurate and stir to react. After the reaction is completed, cool down and add distilled water for emulsification to obtain a starch-based adhesive.
[0015] In the above process, the hydroxyl groups in the gelatinized starch react with the carboxyl groups in the phthalic anhydride to obtain esterified starch, and then the esterified starch, 1,3-butanediol, polyethylene glycol and isophorone diisocyanate react to generate a starch-based adhesive.
[0016] Preferably, in Q1, the usage ratio of gelatinized starch, glacial acetic acid, phthalic anhydride and methanesulfonic acid is (5-10) g: (10-20) mL: (13.32-26.64) g: (0.2-0.4) mL, the stirring heating temperature is 70-80°C, and the stirring time after adding methanesulfonic acid is 2-3 h.
[0017] Preferably, in Q2, the dosage ratio of esterified starch, 1,3-butanediol, polyethylene glycol and isophorone diisocyanate is (12-15) g: (1.25-1.52) mL: (40-50) g: (6.66-6.98) g, the average molecular mass of polyethylene glycol is 1000 Da, the heating temperature is 80-90°C, the stirring reaction time is 2-4h, the rotation speed is 150-200rpm, the temperature is reduced to 40-50°C, the rotation speed is 400-420rpm, and the emulsification reaction time is 2-3h.
[0018] Preferably, in step (3), the method for preparing the antioxidant comprises the following steps:
[0019] S1: β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid is placed in a container, chloroform is added to dissolve it, and dichlorothionyl is added dropwise under nitrogen protection. After the addition is completed, the temperature is raised and kept constant for reaction, and then, the intermediate product 1 is obtained by distillation under reduced pressure;
[0020] S2: Dissolve 4,4'-diaminodiphenylmethane in acetonitrile, slowly drop a mixed solution of acetonitrile and intermediate product 1 under ice bath conditions, drop a mixed solution of triethylamine and acetonitrile under nitrogen protection, control the pH of the reaction system, continue stirring after the addition is complete, then heat the system, react at a constant temperature, and after the reaction is completed, perform reduced pressure distillation to obtain intermediate product 2;
[0021] S3: The intermediate product 2 is dissolved in dichloromethane, washed, and distilled under reduced pressure to obtain the intermediate product 3. The intermediate product 3 is dissolved in ethanol, and a sodium hydroxide solution is added to precipitate a solid. The solid is washed and dried to obtain an antioxidant.
[0022] In the above process, the synthesis reaction formula of the antioxidant is as follows:
[0023]
[0024] The results of mass spectrometry analysis were: m / z: 718.47 (100.0%), 719.47 (51.6%), 720.48 (13.9%), 721.48 (2.6%).
[0025] Preferably, in S1, the dosage ratio of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, chloroform and thionyl chloride is (5.56-8.34) g: (50-75) mL: (8-12) mL, the dropping speed is 1 s / drop, and the temperature is raised to 50-60° C. and the reaction is carried out at a constant temperature for 5-7 hours.
[0026] Preferably, in S2, the dosage ratio of 4,4'-diaminodiphenylmethane and acetonitrile is (0.25-0.5) g: (10-20) mL, the ice bath temperature is 0-1°C, the dosage ratio of acetonitrile and intermediate product 1 is (50-100) mL: (2.23-4.46) g, the volume ratio of triethylamine and acetonitrile is (13.8-27.6): (100-200), the pH of the reaction system is controlled to be 9-10, stirring is continued for 2-4 h, the heating temperature is 50-60°C, the constant temperature reaction time is 24-28 h, the reduced pressure distillation temperature is 50-60°C, and the pressure is 130-135 Pa.
[0027] Preferably, in S3, the amount ratio of the intermediate product 2 and dichloromethane is (8-12) g: (30-35) mL, first washed 3-5 times with 5vt% sodium bicarbonate solution and 0.5mol / L hydrochloric acid solution, then washed 2-3 times with saturated sodium chloride solution, the reduced pressure distillation temperature is 60-70°C, the pressure is 130-135Pa, the amount ratio of the intermediate product 3, ethanol and sodium hydroxide solution is (5-8) g: (30-40) mL: (10-20) mL, the concentration of the sodium hydroxide solution is 1mol / L, washed with deionized water, the drying temperature is 60-70°C, and the time is 12-14h.
[0028] Preferably, in step (3), the ratio of the starch-based adhesive to the antioxidant is (30-50) mL: (4-6) g, the ratio of the sodium hydroxide, distilled water and the starch-based mixture is (10-20) g: (40-90) mL: (6-9) mL, the stirring time is continued for 30-60 min, and the pH is adjusted to 7-7.2.
[0029] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0030] 1. The present invention firstly uses gelatinized starch, phthalate, 1,3-butanediol, polyethylene glycol and isophorone diisocyanate as raw materials to synthesize a starch-based adhesive, then uses β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, dichlorothionyl and 4,4'-diaminodiphenylmethane as raw materials to prepare an antioxidant, and then uses the starch-based adhesive and the antioxidant as raw materials to synthesize a starch additive for glue making, which can effectively improve its viscosity, antioxidant performance and mildew resistance.
[0031] 2. The present invention uses gelatinized starch, phthalate and isophorone diisocyanate as raw materials to prepare a starch-based adhesive, which is used in the preparation process of a starch additive to effectively improve its bonding performance, water resistance and stability. The ester bonds contained in the esterified starch have higher hydrophobic properties than hydroxyl groups, and the three-dimensional network structure formed by the starch-based adhesive can further improve its water resistance, and can also resist changes in the external environment, keeping its physical and chemical properties stable. The presence of the three-dimensional network structure can increase the viscosity of the starch-based adhesive, making it have better adhesion and wettability, and improving its performance.
[0032] 3. The present invention uses β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid, dichlorothionyl and 4,4'-diaminodiphenylmethane as raw materials to prepare antioxidants, and adding the antioxidants to starch additives can effectively improve their antioxidant properties and mildew resistance, thereby increasing their service life. Antioxidants can capture free radicals, inhibit the oxidation chain reaction, prevent further oxidation and degradation of starch additives, and improve their antioxidant properties; the presence of antioxidants can improve the microenvironment of starch additives, which is not conducive to the growth and reproduction of molds, inhibit the metabolic activities of molds, protect starch additives from damage by mycotoxins, and enhance their mildew resistance. DETAILED DESCRIPTION
[0033] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] This embodiment discloses a method for preparing a starch-based adhesive, comprising the following steps:
[0036] Q1: 7.5 g of gelatinized starch and 15 mL of glacial acetic acid were mixed, heated with stirring at 80°C, and then 19.98 g of phthalic anhydride was added for stirring reaction, followed by 0.3 mL of methanesulfonic acid. After stirring for 3 h, distilled water was added to terminate the reaction to obtain a crude product, which was filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0037] Q2: 14 g of esterified starch, 1.38 mL of 1,3-butanediol and 45 g of polyethylene glycol with an average molecular weight of 1000 Da were added into a container for mixing, N,N-dimethylformamide was added for dissolution, and the temperature of the container was raised to 90°C while stirring until all dissolved in a liquid state. Then, 6.83 g of isophorone diisocyanate and dibutyltin dilaurate were added, and the reaction was stirred at 200 rpm for 4 h. After the reaction was completed, the speed was adjusted to 400 rpm, the temperature was lowered to 40°C, and distilled water was added for emulsification reaction for 3 h to obtain a starch-based adhesive.
[0038] This embodiment discloses a method for preparing an antioxidant, comprising the following steps:
[0039] S1: 6.95 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was placed in a container, 62.5 mL of chloroform was added to dissolve, and 10 mL of thionyl chloride was added dropwise under nitrogen protection at a rate of 1 s / drop. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out at a constant temperature for 7 hours. Subsequently, the intermediate product 1 was obtained by distillation under reduced pressure.
[0040] S2: 0.375 g of 4,4'-diaminodiphenylmethane was dissolved in 15 mL of acetonitrile. Under a 0°C ice bath condition, a mixed solution of 75 mL of acetonitrile and 3.34 g of intermediate product 1 was slowly added dropwise. Under nitrogen protection, a mixed solution of 20.4 mL of triethylamine and 150 mL of acetonitrile was added dropwise. The pH of the reaction system was controlled to be 9. After the addition was completed, stirring was continued for 4 h. Then the system was heated to 60°C and reacted at this temperature for 24 h. After the reaction was completed, vacuum distillation was performed at 60°C and 135 Pa to obtain intermediate product 2.
[0041] S3: Dissolve 10g of intermediate product 2 in 32.5mL of dichloromethane, wash it three times with 5vt% sodium bicarbonate solution and 0.5mol / L hydrochloric acid solution, then wash it three times with saturated sodium chloride solution, and distill it under reduced pressure at 70℃ and 135Pa to obtain intermediate product 3. Dissolve 6.5g of intermediate product 3 in 35mL of ethanol, and add 15mL of 1mol / L sodium hydroxide solution. Solid precipitates, wash the solid with deionized water, and dry it at 60℃ for 12h to obtain an antioxidant.
[0042] This embodiment discloses a preparation process of a starch additive for glue making, comprising the following steps:
[0043] Step (1): add 1300 mL of distilled water into a container, add 175 g of starch while stirring, and after the starch is completely added, heat to 70° C. and continue stirring for 30 min to obtain gelatinized starch;
[0044] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0045] Step (3): 40 mL of the obtained starch-based adhesive is mixed with 5 g of an antioxidant to obtain a starch-based mixture. Subsequently, 15 g of sodium hydroxide is dissolved in 65 mL of distilled water and then added to 7.5 mL of the starch-based mixture. Stirring is continued for 60 min to form a glue solution. The pH is adjusted to 7 to obtain a starch additive for glue making.
[0046] Example 2
[0047] This embodiment discloses a method for preparing a starch-based adhesive, comprising the following steps:
[0048] Q1: 5 g of gelatinized starch and 10 mL of glacial acetic acid were mixed, heated with stirring at 80°C, and then 13.32 g of phthalic anhydride was added for stirring reaction, followed by 0.2 mL of methanesulfonic acid. After stirring for 3 h, distilled water was added to terminate the reaction to obtain a crude product, which was filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0049] Q2: 12 g of esterified starch, 1.25 mL of 1,3-butanediol and 40 g of polyethylene glycol with an average molecular weight of 1000 Da were added into a container and mixed, N,N-dimethylformamide was added to dissolve, and the temperature of the container was raised to 90°C while stirring until all dissolved in a liquid state, 6.66 g of isophorone diisocyanate and dibutyltin dilaurate were added, and the reaction was stirred at 200 rpm for 4 h. After the reaction was completed, the speed was adjusted to 400 rpm, the temperature was lowered to 40°C, and distilled water was added for emulsification reaction for 3 h to obtain a starch-based adhesive.
[0050] This embodiment discloses a method for preparing an antioxidant, comprising the following steps:
[0051] S1: 5.56 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was placed in a container, 50 mL of chloroform was added to dissolve, and 8 mL of thionyl chloride was added dropwise under nitrogen protection at a rate of 1 s / drop. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out at a constant temperature for 7 hours. Subsequently, the intermediate product 1 was obtained by distillation under reduced pressure.
[0052] S2: 0.25 g of 4,4'-diaminodiphenylmethane was dissolved in 10 mL of acetonitrile. Under a 0°C ice bath condition, a mixed solution of 50 mL of acetonitrile and 2.23 g of intermediate 1 was slowly added dropwise. Under nitrogen protection, a mixed solution of 13.8 mL of triethylamine and 100 mL of acetonitrile was added dropwise. The pH of the reaction system was controlled to be 9. After the addition was completed, stirring was continued for 4 h. Then the system was heated to 60°C and reacted at a constant temperature for 24 h. After the reaction was completed, vacuum distillation was performed at 60°C and 135 Pa to obtain intermediate 2.
[0053] S3: Dissolve 8 g of intermediate product 2 in 30 mL of dichloromethane, wash three times with 5vt% sodium bicarbonate solution and 0.5 mol / L hydrochloric acid solution, then wash three times with saturated sodium chloride solution, and distill under reduced pressure at 70°C and 135 Pa to obtain intermediate product 3. Dissolve 5 g of intermediate product 3 in 30 mL of ethanol, and add 10 mL of 1 mol / L sodium hydroxide solution. Solid precipitates, wash the solid with deionized water, and dry at 60°C for 12 h to obtain an antioxidant.
[0054] This embodiment discloses a preparation process of a starch additive for glue making, comprising the following steps:
[0055] Step (1): Add 1200 mL of distilled water to a container, add 150 g of starch while stirring, and after the starch is completely added, heat to 70° C. and continue stirring for 30 minutes to obtain gelatinized starch;
[0056] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0057] Step (3): 30 mL of the obtained starch-based adhesive is mixed with 4 g of an antioxidant to obtain a starch-based mixture. Subsequently, 10 g of sodium hydroxide is dissolved in 40 mL of distilled water and then added to 6 mL of the starch-based mixture. Stirring is continued for 60 min to form a glue solution. The pH is adjusted to 7 to obtain a starch additive for glue making.
[0058] Example 3
[0059] This embodiment discloses a method for preparing a starch-based adhesive, comprising the following steps:
[0060] Q1: 10 g of gelatinized starch and 20 mL of glacial acetic acid were mixed, heated with stirring at 80°C, and then 26.64 g of phthalic anhydride was added for stirring reaction, followed by 0.4 mL of methanesulfonic acid. After stirring for 3 h, distilled water was added to terminate the reaction to obtain a crude product, which was filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0061] Q2: 15 g of esterified starch, 1.52 mL of 1,3-butanediol and 50 g of polyethylene glycol with an average molecular weight of 1000 Da were added into a container for mixing, N,N-dimethylformamide was added for dissolution, and the temperature of the container was raised to 90°C while stirring until all dissolved in a liquid state. Then, 6.98 g of isophorone diisocyanate and dibutyltin dilaurate were added, and the reaction was stirred at 200 rpm for 4 h. After the reaction was completed, the speed was adjusted to 400 rpm, the temperature was lowered to 40°C, and distilled water was added for emulsification reaction for 3 h to obtain a starch-based adhesive.
[0062] This embodiment discloses a method for preparing an antioxidant, comprising the following steps:
[0063] S1: 8.34 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was placed in a container, 75 mL of chloroform was added to dissolve, and 12 mL of thionyl chloride was added dropwise under nitrogen protection at a rate of 1 s / drop. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out at a constant temperature for 7 hours. Subsequently, the intermediate product 1 was obtained by distillation under reduced pressure.
[0064] S2: 0.5 g of 4,4'-diaminodiphenylmethane was dissolved in 20 mL of acetonitrile. Under ice bath condition at 0°C, a mixed solution of 100 mL of acetonitrile and 4.46 g of intermediate 1 was slowly added dropwise. Under nitrogen protection, a mixed solution of 27.6 mL of triethylamine and 200 mL of acetonitrile was added dropwise. The pH of the reaction system was controlled to be 9. After the addition was completed, stirring was continued for 4 h. Then the system was heated to 60°C and reacted at constant temperature for 24 h. After the reaction was completed, vacuum distillation was performed at 60°C and 135 Pa to obtain intermediate 2.
[0065] S3: Dissolve 12g of intermediate product 2 in 35mL of dichloromethane, wash three times with 5vt% sodium bicarbonate solution and 0.5mol / L hydrochloric acid solution, then wash three times with saturated sodium chloride solution, and distill under reduced pressure at 70°C and 135Pa to obtain intermediate product 3. Dissolve 8g of intermediate product 3 in 40mL of ethanol, and add 20mL of 1mol / L sodium hydroxide solution. Solid precipitates, wash the solid with deionized water, and dry at 60°C for 12h to obtain an antioxidant.
[0066] This embodiment discloses a preparation process of a starch additive for glue making, comprising the following steps:
[0067] Step (1): add 1500 mL of distilled water into a container, add 200 g of starch while stirring, and after the starch is completely added, heat to 70° C. and continue stirring for 30 min to obtain gelatinized starch;
[0068] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0069] Step (3): 50 mL of the obtained starch-based adhesive is mixed with 6 g of an antioxidant to obtain a starch-based mixture. Subsequently, 20 g of sodium hydroxide is dissolved in 90 mL of distilled water and then added to 9 mL of the starch-based mixture. Stirring is continued for 60 min to form a glue solution. The pH is adjusted to 7 to obtain a starch additive for glue making.
[0070] Example 4
[0071] This embodiment discloses a method for preparing a starch-based adhesive, comprising the following steps:
[0072] Q1: 8 g of gelatinized starch and 18 mL of glacial acetic acid were mixed, heated with stirring at 80°C, and then 15.47 g of phthalic anhydride was added for stirring reaction, followed by 0.28 mL of methanesulfonic acid. After stirring for 3 h, distilled water was added to terminate the reaction to obtain a crude product, which was filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0073] Q2: 13 g of esterified starch, 1.41 mL of 1,3-butanediol and 42 g of polyethylene glycol with an average molecular weight of 1000 Da were added into a container and mixed, N,N-dimethylformamide was added to dissolve, and the temperature of the container was raised to 90°C while stirring until all dissolved in a liquid state, 6.71 g of isophorone diisocyanate and dibutyltin dilaurate were added, and the reaction was stirred at 200 rpm for 4 h. After the reaction was completed, the speed was adjusted to 400 rpm, the temperature was lowered to 40°C, and distilled water was added for emulsification reaction for 3 h to obtain a starch-based adhesive.
[0074] This embodiment discloses a method for preparing an antioxidant, comprising the following steps:
[0075] S1: 7.21 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was placed in a container, 73 mL of chloroform was added to dissolve, and 11 mL of thionyl chloride was added dropwise under nitrogen protection at a rate of 1 s / drop. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out at a constant temperature for 7 hours. Subsequently, the intermediate product 1 was obtained by distillation under reduced pressure.
[0076] S2: 0.43 g of 4,4'-diaminodiphenylmethane was dissolved in 12 mL of acetonitrile. Under a 0°C ice bath condition, a mixed solution of 80 mL of acetonitrile and 2.83 g of intermediate product 1 was slowly added dropwise. Under nitrogen protection, a mixed solution of 22.1 mL of triethylamine and 170 mL of acetonitrile was added dropwise. The pH of the reaction system was controlled to be 9. After the addition was completed, stirring was continued for 4 h. Then the system was heated to 60°C and reacted at a constant temperature for 24 h. After the reaction was completed, vacuum distillation was performed at 60°C and 135 Pa to obtain intermediate product 2.
[0077] S3: Dissolve 11g of intermediate product 2 in 31mL of dichloromethane, wash it three times with 5vt% sodium bicarbonate solution and 0.5mol / L hydrochloric acid solution, then wash it three times with saturated sodium chloride solution, and distill it under reduced pressure at 70℃ and 135Pa to obtain intermediate product 3. Dissolve 7g of intermediate product 3 in 32mL of ethanol, and add 12mL of 1mol / L sodium hydroxide solution. Solid precipitates. Wash the solid with deionized water, and dry it at 60℃ for 12h to obtain an antioxidant.
[0078] This embodiment discloses a preparation process of a starch additive for glue making, comprising the following steps:
[0079] Step (1): add 1400 mL of distilled water into a container, add 180 g of starch while stirring, and after the starch is completely added, heat to 70° C. and continue stirring for 30 min to obtain gelatinized starch;
[0080] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0081] Step (3): 35 mL of the obtained starch-based adhesive is mixed with 4.7 g of an antioxidant to obtain a starch-based mixture. Subsequently, 12 g of sodium hydroxide is dissolved in 70 mL of distilled water and then added to 8 mL of the starch-based mixture. Stirring is continued for 60 min to form a glue solution. The pH is adjusted to 7 to obtain a starch additive for glue making.
[0082] Example 5
[0083] This embodiment discloses a method for preparing a starch-based adhesive, comprising the following steps:
[0084] Q1: 6.5 g of gelatinized starch and 13 mL of glacial acetic acid were mixed, heated with stirring at 80°C, and then 22.38 g of phthalic anhydride was added for stirring reaction, followed by 0.33 mL of methanesulfonic acid. After stirring for 3 h, distilled water was added to terminate the reaction to obtain a crude product, which was filtered under reduced pressure, washed, and dried to obtain esterified starch;
[0085] Q2: 14.5 g of esterified starch, 1.49 mL of 1,3-butanediol and 47 g of polyethylene glycol with an average molecular weight of 1000 Da were added into a container for mixing, N,N-dimethylformamide was added for dissolution, and the temperature of the container was raised to 90°C while stirring until all dissolved in a liquid state. Then, 6.95 g of isophorone diisocyanate and dibutyltin dilaurate were added, and the reaction was stirred at 200 rpm for 4 h. After the reaction was completed, the speed was adjusted to 400 rpm, the temperature was lowered to 40°C, and distilled water was added for emulsification reaction for 3 h to obtain a starch-based adhesive.
[0086] This embodiment discloses a method for preparing an antioxidant, comprising the following steps:
[0087] S1: 8.05 g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was placed in a container, 54.5 mL of chloroform was added to dissolve, and 9 mL of thionyl chloride was added dropwise under nitrogen protection at a rate of 1 s / drop. After the addition was completed, the temperature was raised to 50°C and the reaction was carried out at a constant temperature for 7 hours. Subsequently, the intermediate product 1 was obtained by distillation under reduced pressure.
[0088] S2: 0.33 g of 4,4'-diaminodiphenylmethane was dissolved in 17 mL of acetonitrile. Under an ice bath at 0°C, a mixed solution of 63 mL of acetonitrile and 2.98 g of intermediate product 1 was slowly added dropwise. Under nitrogen protection, a mixed solution of 22.5 mL of triethylamine and 130 mL of acetonitrile was added dropwise. The pH of the reaction system was controlled to be 9. After the addition was completed, stirring was continued for 4 h. Then the system was heated to 60°C and reacted at this temperature for 24 h. After the reaction was completed, vacuum distillation was performed at 60°C and 135 Pa to obtain intermediate product 2.
[0089] S3: Dissolve 9 g of intermediate product 2 in 34 mL of dichloromethane, wash three times with 5 vt% sodium bicarbonate solution and 0.5 mol / L hydrochloric acid solution, then wash three times with saturated sodium chloride solution, and distill under reduced pressure at 70°C and 135 Pa to obtain intermediate product 3. Dissolve 6 g of intermediate product 3 in 37 mL of ethanol, and add 17 mL of 1 mol / L sodium hydroxide solution. Solid precipitates, wash the solid with deionized water, and dry at 60°C for 12 h to obtain an antioxidant.
[0090] This embodiment discloses a preparation process of a starch additive for glue making, comprising the following steps:
[0091] Step (1): add 1350 mL of distilled water into a container, add 190 g of starch while stirring, and after the starch is completely added, heat to 70° C. and continue stirring for 30 min to obtain gelatinized starch;
[0092] Step (2): preparing a starch-based adhesive using gelatinized starch;
[0093] Step (3): 45 mL of the obtained starch-based adhesive is mixed with 4.2 g of an antioxidant to obtain a starch-based mixture. Subsequently, 17 g of sodium hydroxide is dissolved in 80 mL of distilled water and then added to 7 mL of the starch-based mixture. Stirring is continued for 60 min to form a glue solution, and the pH is adjusted to 7 to obtain a starch additive for glue making.
[0094] Comparative Example 1
[0095] Comparative Example 1 Compared with Example 1, in the process of preparing the starch-based adhesive in Comparative Example 1, phthalic anhydride was not added, and other conditions remained unchanged.
[0096] Comparative Example 2
[0097] Comparative Example 2 Compared with Example 1, in the process of preparing the starch-based adhesive in Comparative Example 2, no polyethylene glycol was added, and other conditions remained unchanged.
[0098] Comparative Example 3
[0099] Comparative Example 3 Compared with Example 1, in the process of preparing the starch-based adhesive in Comparative Example 3, isophorone diisocyanate is not added, and other conditions remain unchanged.
[0100] Comparative Example 4
[0101] Comparative Example 4 Compared with Example 1, in the process of preparing the antioxidant in Comparative Example 4, no β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid was added, and other conditions remained unchanged.
[0102] Comparative Example 5
[0103] Comparative Example 5 Compared with Example 1, in the process of preparing the antioxidant in Comparative Example 5, 4,4'-diaminodiphenylmethane was not added, and other conditions remained unchanged.
[0104] Comparative Example 6
[0105] Comparative Example 6 Compared with Example 1, in the process of preparing the antioxidant in Comparative Example 6, no triethylamine was added, and other conditions remained unchanged.
[0106] Comparative Example 7
[0107] Compared with Example 1, in Comparative Example 7, during the preparation of the starch additive, no starch-based adhesive was added, and other conditions remained unchanged.
[0108] Comparative Example 8
[0109] Compared with Example 1, in Comparative Example 8, during the preparation of the starch additive, no antioxidant was added, and other conditions remained unchanged.
[0110] The performance of the starch additives for glue preparation prepared in Examples 1-5 and Comparative Examples 1-8 was tested. The viscosity of the samples was tested according to GB / T 2794-2022, the water resistance of the samples was tested according to ASTM D5570, and the mildew resistance of the samples was tested according to GB / T 1741-2020. The test results are shown in Table 1:
[0111] Table 1
[0112]
[0113]
[0114] It can be seen from the test results in Table 1 that the starch additives prepared in Examples 1-5 of the present invention have excellent viscosity, water resistance and mildew resistance. Comparison between Comparative Example 1 and Examples 1-5 shows that the addition of phthalic anhydride can effectively improve the viscosity and water resistance of the starch additive; comparison between Comparative Example 2 and Examples 1-5 shows that the addition of polyethylene glycol can effectively improve the viscosity and water resistance of the starch additive; comparison between Comparative Example 3 and Examples 1-5 shows that the addition of isophorone diisocyanate can effectively improve the viscosity and water resistance of the starch additive; comparison between Comparative Example 4 and Examples 1-5 shows that the addition of β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid can effectively improve the viscosity and water resistance of the starch additive. The anti-mildew performance of the additive; by comparing comparative example 5 with embodiments 1-5, it can be seen that the addition of 4,4'-diaminodiphenylmethane can effectively improve the anti-mildew performance of the starch additive; by comparing comparative example 6 with embodiments 1-5, it can be seen that the addition of triethylamine can effectively improve the anti-mildew performance of the starch additive; by comparing comparative example 7 with embodiments 1-5, it can be seen that the addition of a starch-based adhesive can effectively improve the viscosity and water resistance of the starch additive; by comparing comparative example 8 with embodiments 1-5, it can be seen that the addition of an antioxidant can effectively improve the anti-mildew performance of the starch additive.
[0115] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0116] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A process for preparing a starch additive for glue making, characterized in that: The following steps are involved: Step (1): adding distilled water to a container, adding starch while stirring, and after the starch is completely added, heating and stirring continuously to obtain gelatinized starch; Step (2): preparing a starch-based adhesive using gelatinized starch; Step (3): Mixing the obtained starch-based adhesive with an antioxidant to obtain a starch-based mixture, then dissolving sodium hydroxide with distilled water and adding it to the starch-based mixture, continuing to stir to form a glue solution, adjusting the pH, and obtaining a starch additive for glue making.
2. The preparation process of a starch additive for glue making according to claim 1, characterized in that: In the step (1), the usage ratio of distilled water to starch is (1200-1500) mL: (150-200) g, the heating and stirring temperature is 60-70° C., and the time is 20-30 min.
3. The preparation process of a starch additive for glue making according to claim 1, characterized in that: In the step (2), the method for preparing the starch-based adhesive comprises the following steps: Q1: The gelatinized starch and glacial acetic acid are mixed, stirred and heated, and then phthalic anhydride is added to react by stirring, and then methanesulfonic acid is added. After stirring and reacting, distilled water is added to terminate the reaction to obtain a crude product, which is filtered under reduced pressure, washed, and dried to obtain esterified starch; Q2: Add esterified starch, 1,3-butanediol and polyethylene glycol into a container and mix them. Add N,N-dimethylformamide to dissolve it. Heat the container while stirring until it is completely dissolved and in liquid form. Add isophorone diisocyanate and dibutyltin dilaurate and stir to react. After the reaction is completed, cool down and add distilled water for emulsification to obtain a starch-based adhesive.
4. The preparation process of a starch additive for glue making according to claim 3, characterized in that: In the Q1, the usage ratio of gelatinized starch, glacial acetic acid, phthalic anhydride and methanesulfonic acid is (5-10) g: (10-20) mL: (13.32-26.64) g: (0.2-0.4) mL, the stirring heating temperature is 70-80° C., and the stirring time after adding methanesulfonic acid is 2-3 h.
5. The preparation process of a starch additive for glue making according to claim 3, characterized in that: In Q2, the dosage ratio of esterified starch, 1,3-butanediol, polyethylene glycol and isophorone diisocyanate is (12-15) g: (1.25-1.52) mL: (40-50) g: (6.66-6.98) g, the average molecular weight of polyethylene glycol is 1000 Da, the heating temperature is 80-90° C., the stirring reaction time is 2-4 h, the rotation speed is 150-200 rpm, the temperature is reduced to 40-50° C., the rotation speed is 400-420 rpm, and the emulsification reaction time is 2-3 h.
6. The preparation process of a starch additive for glue making according to claim 1, characterized in that: In the step (3), the method for preparing the antioxidant comprises the following steps: S1: β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid is placed in a container, chloroform is added to dissolve it, and dichlorothionyl is added dropwise under nitrogen protection. After the addition is completed, the temperature is raised and kept constant for reaction, and then, the intermediate product 1 is obtained by distillation under reduced pressure; S2: Dissolve 4,4'-diaminodiphenylmethane in acetonitrile, slowly drop a mixed solution of acetonitrile and intermediate product 1 under ice bath conditions, drop a mixed solution of triethylamine and acetonitrile under nitrogen protection, control the pH of the reaction system, continue stirring after the addition is complete, then heat the system, react at a constant temperature, and after the reaction is completed, perform reduced pressure distillation to obtain intermediate product 2; S3: The intermediate product 2 is dissolved in dichloromethane, washed, and distilled under reduced pressure to obtain the intermediate product 3. The intermediate product 3 is dissolved in ethanol, and a sodium hydroxide solution is added to precipitate a solid. The solid is washed and dried to obtain an antioxidant.
7. The preparation process of a starch additive for glue making according to claim 6, characterized in that: In S1, the dosage ratio of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionic acid, chloroform and thionyl chloride is (5.56-8.34) g: (50-75) mL: (8-12) mL, the dropping speed is 1 s / drop, the temperature is raised to 50-60° C. and the reaction is carried out at a constant temperature for 5-7 hours.
8. The preparation process of a starch additive for glue making according to claim 6, characterized in that: In S2, the dosage ratio of 4,4'-diaminodiphenylmethane and acetonitrile is (0.25-0.5) g: (10-20) mL, the ice bath temperature is 0-1°C, the dosage ratio of acetonitrile and intermediate product 1 is (50-100) mL: (2.23-4.46) g, the volume ratio of triethylamine and acetonitrile is (13.8-27.6): (100-200), the pH of the reaction system is controlled to be 9-10, stirring is continued for 2-4 h, the heating temperature is 50-60°C, the constant temperature reaction time is 24-28 h, the reduced pressure distillation temperature is 50-60°C, and the pressure is 130-135 Pa.
9. The preparation process of a starch additive for glue making according to claim 6, characterized in that: In the S3, the amount ratio of the intermediate product 2 and dichloromethane is (8-12) g: (30-35) mL. It is first washed with 5vt% sodium bicarbonate solution and 0.5mol / L hydrochloric acid solution for 3-5 times, and then washed with saturated sodium chloride solution for 2-3 times. The reduced pressure distillation temperature is 60-70°C and the pressure is 130-135Pa. The amount ratio of the intermediate product 3, ethanol and sodium hydroxide solution is (5-8) g: (30-40) mL: (10-20) mL. The concentration of the sodium hydroxide solution is 1mol / L. It is washed with deionized water, and the drying temperature is 60-70°C for 12-14h.
10. The preparation process of a starch additive for glue making according to claim 1, characterized in that: In the step (3), the ratio of the starch-based adhesive to the antioxidant is (30-50) mL: (4-6) g, the ratio of the sodium hydroxide, distilled water and the starch-based mixture is (10-20) g: (40-90) mL: (6-9) mL, the stirring time is continued for 30-60 min, and the pH is adjusted to 7-7.2.