Magnetic grinding material with core-shell structure and preparation method of magnetic grinding material
By preparing magnetic abrasives in the core structure, using ball milling and nitriding heat treatment technology, the problem of mismatch between the surface hardness of the magnetic abrasives and the workpiece is solved, significantly reducing the surface roughness of the workpiece and improving the grinding processing effect.
Patent Information
- Application Number
- CN202410957697.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The magnetic abrasive does not match the hardness of the workpiece surface during grinding and processing, resulting in the workpiece surface roughness that cannot be further reduced and the grinding effect is poor.
Using the preparation method of putaway structure magnetic abrasive, a ball mill is made by mixing single crystal silicon particles, magnetic iron-based powder and yttrium trioxide to form a precursor, and then undergoing nitriding heat treatment to form a ferromagnetic matrix and silicon nitride hardness. The putaway structure of the mass phase enhances the combination of the ferromagnetic matrix and the hard phase.
The workpiece surface roughness is reduced to 0.090±0.01μm, which improves the grinding effect.
Smart Images

Figure CN118909593A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic abrasives, and in particular to a core-shell structured magnetic abrasive and a preparation method thereof. Background Art
[0002] Magnetic grinding is a surface treatment method that uses a magnetic field to act on magnetic abrasives to cause abrasive impact with the workpiece. It is suitable for the processing and treatment of the surfaces of various metals, ceramics, plastics and other materials, and is widely used in manufacturing industries such as machinery, molds, automobiles, bearings, semiconductors and aviation.
[0003] Magnetic abrasives are the key to magnetic grinding. At present, the research on magnetic abrasives mainly focuses on the problems of low life of magnetic abrasives, poor metal cutting ability and low strength of the combination of ferromagnetic phase and abrasive particles. For example, patent CN105665725A discloses a method for preparing free-falling double-nozzle mixed powder gas atomization water-cooled rapid solidification metal-based CBN magnetic abrasives, which solves the problems of poor metal cutting ability and low strength of the combination of ferromagnetic phase and abrasive particles existing in magnetic abrasives.
[0004] In fact, when a workpiece is placed in the air for a long time, a hard oxide film will be formed on the surface. Compared with the hardness of the oxide film on the surface, the metal matrix inside the workpiece is soft. Therefore, when using magnetic abrasives to perform magnetic grinding on the workpiece, after the oxide film on the surface is ground away, the hardness of the magnetic abrasive and the workpiece surface does not match, resulting in the surface roughness of the workpiece being unable to be further reduced after reaching a certain level, and the grinding effect is poor. Summary of the invention
[0005] The object of the present invention is to provide a core-shell structure magnetic abrasive and a preparation method thereof. The core-shell structure magnetic abrasive provided by the present invention can make a workpiece have a lower surface roughness when used for grinding processing.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing a core-shell structure magnetic abrasive, comprising the following steps:
[0008] (1) mixing single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then ball milling to obtain a precursor;
[0009] (2) The precursor obtained in step (1) is subjected to nitridation heat treatment to obtain a core-shell structured magnetic abrasive.
[0010] Preferably, in step (1), the mass ratio of the single crystal silicon particles to the magnetic iron-based powder is 1:(4-6).
[0011] Preferably, the magnetic iron-based powder in step (1) comprises one of iron powder, carbonyl iron powder, iron-silicon alloy powder, iron-aluminum alloy powder and iron-nickel alloy powder.
[0012] Preferably, the particle size ratio of the magnetic iron-based powder to the single crystal silicon particles in the precursor of step (1) is (20-50):1.
[0013] Preferably, in step (1), the rotation speed of the ball mill is 150 to 300 rpm, and the ball milling time is 8 to 10 hours.
[0014] Preferably, the temperature of the nitriding heat treatment in step (2) is 1000-1300° C., and the time of the nitriding heat treatment is 2-4 hours.
[0015] The present invention also provides a core-shell structure magnetic abrasive prepared by the above preparation method, comprising a ferromagnetic matrix and an iron-silicon intermetallic compound and a silicon nitride hard phase sequentially coated on the surface of the ferromagnetic matrix from the inside to the outside.
[0016] The present invention provides a method for preparing a core-shell structure magnetic abrasive, comprising the following steps: (1) mixing single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then ball milling to obtain a precursor; (2) subjecting the precursor obtained in the step (1) to nitridation heat treatment to obtain a core-shell structure magnetic abrasive. The present invention mixes single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then ball milling, so that mechanical alloying occurs between the magnetic iron-based powder and the single crystal silicon through ball milling, thereby strengthening the interface bonding between the two, and also making the single crystal silicon uniformly distributed on the surface of the magnetic iron-based powder to form a precursor; then the obtained precursor is subjected to nitridation heat treatment, and a silicon nitride hard phase is formed in situ on the surface of the single crystal silicon. At the same time, under high temperature conditions, the single crystal silicon is embedded in the surface of the magnetic iron-based powder, so that the mechanical alloying between the magnetic iron-based powder and the single crystal silicon is further converted into a silicon-iron metal compound, thereby further strengthening the interface bonding between the two, thereby obtaining a core-shell structure magnetic abrasive. The results of the examples show that the roughness of the zirconium alloy tube wall can be reduced to 0.090±0.01 μm by grinding the zirconium alloy tube wall with the core-shell structure magnetic abrasive prepared by the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 XRD diagram of the core-shell structure magnetic abrasive obtained in Examples 1 to 4;
[0018] Figure 2 This is the SEM image of the core-shell structure magnetic abrasive obtained in Example 1;
[0019] Figure 3 This is the SEM image of the core-shell structure magnetic abrasive obtained in Example 2;
[0020] Figure 4This is the SEM image of the core-shell structure magnetic abrasive obtained in Example 3;
[0021] Figure 5 This is the SEM image of the core-shell structure magnetic abrasive obtained in Example 4;
[0022] Figure 6 The cross-sectional SEM image and EDS image of the core-shell structure magnetic abrasive obtained in Example 1;
[0023] Figure 7 The SEM image of the magnetic abrasive obtained in Comparative Example 1;
[0024] Figure 8 This is the test diagram of the surface roughness of the unprocessed zirconium tube;
[0025] Fig. 9 This is a test diagram of the surface roughness of the zirconium alloy tube wall after the core-shell structure magnetic abrasive grinding process obtained in Example 1;
[0026] Fig.10 This is a test chart of the surface roughness of the zirconium tube after traditional sintered magnetic abrasive processing. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a core-shell structure magnetic abrasive, comprising the following steps:
[0028] (1) mixing single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then ball milling to obtain a precursor;
[0029] (2) The precursor obtained in step (1) is subjected to nitridation heat treatment to obtain a core-shell structured magnetic abrasive.
[0030] The invention mixes single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then performs ball milling to obtain a precursor.
[0031] In the present invention, the particle size of the single crystal silicon particles is preferably 1-5 μm, more preferably 2-3 μm. The present invention limits the particle size of the single crystal silicon particles so that the single crystal silicon particles in the obtained precursor are more evenly distributed on the surface of the magnetic iron-based powder, thereby improving the processing effect of the magnetic abrasive on the workpiece.
[0032] In the present invention, when the particle size of the single crystal silicon particles is not within the above range, the single crystal silicon particles are preferably screened. The present invention has no special limitation on the screening method, and any screening method known in the art can be used.
[0033] In the present invention, the magnetic iron-based powder preferably includes one of iron powder, carbonyl iron powder, iron-silicon alloy, iron-aluminum alloy and iron-nickel alloy. The present invention limits the type of magnetic iron-based powder to ensure that the magnetic properties of the prepared magnetic abrasive are better, thereby improving the processing effect of the magnetic abrasive on the workpiece.
[0034] In the present invention, the particle size of the magnetic iron-based powder is preferably 80-200 μm, more preferably 120 μm. The present invention limits the particle size of the magnetic iron-based powder to make the single crystal silicon particles more evenly distributed on its surface, thereby improving the processing effect of the magnetic abrasive on the workpiece.
[0035] In the present invention, the particle size ratio of the magnetic iron-based powder to the single crystal silicon particles in the precursor is (20-50): 1, more preferably (30-40): 1. The present invention limits the particle size ratio of the magnetic iron-based powder to the single crystal silicon particles in the precursor so that the single crystal silicon particles completely cover the surface of the ferromagnetic matrix, thereby improving the relative magnetic permeability of the obtained magnetic abrasive, making the obtained magnetic abrasive have a relatively consistent cutting depth during processing, and improving the processing efficiency of the magnetic abrasive.
[0036] In the present invention, the mass ratio of the single crystal silicon particles to the magnetic iron-based powder is preferably 1: (4-6), and more preferably 1: 5. The present invention limits the mass ratio of the single crystal silicon particles to the magnetic iron-based powder so that the single crystal silicon particles are more evenly distributed on the surface of the magnetic iron-based powder, thereby improving the processing effect of the magnetic abrasive on the workpiece.
[0037] In the present invention, the particle size of the yttrium trioxide is preferably 1 to 5 μm, more preferably 2 to 4 μm. The present invention limits the particle size of the yttrium trioxide to ensure more complete mixing with the single crystal silicon particles, thereby achieving a better catalytic effect of in-situ formation of silicon nitride on the surface of the single crystal silicon in the subsequent nitridation heat treatment.
[0038] In the present invention, the mass of the yttrium trioxide is preferably 6-12% of the total mass of the single crystal silicon particles, the magnetic iron-based powder and the yttrium trioxide, and more preferably 8-10%. The present invention sufficiently reduces the temperature of the subsequent nitriding heat treatment by limiting the mass of the yttrium trioxide, so that the ferromagnetic matrix will not be completely melted, thereby maintaining its original morphology, and the catalytic effect of catalyzing the in-situ generation of silicon nitride on the surface of the single crystal silicon in the subsequent nitriding heat treatment is more sufficient.
[0039] In the present invention, the mixing of the monocrystalline silicon particles, the magnetic iron-based powder and the yttrium trioxide is preferably carried out under stirring. In the present invention, the stirring rate is preferably 120 to 150 r / min; in the present invention, the stirring time is preferably 20 to 60 min, more preferably 30 to 50 min. The present invention limits the stirring rate and time to ensure that the monocrystalline silicon particles, the magnetic iron-based powder and the yttrium trioxide are mixed more fully.
[0040] In the present invention, the rotation speed of the ball mill is preferably 150-300 rpm, more preferably 200-250 rpm. In the present invention, the time of the ball milling is preferably 8-10 hours, more preferably 9 hours. In the present invention, the grinding balls used in the ball milling are preferably steel balls. In the present invention, the ball-to-material ratio of the ball milling is preferably (8-12):1, more preferably 10:1. In the present invention, the packing coefficient during the ball milling is preferably 0.4-0.6, more preferably 0.5. In the present invention, the ball milling is preferably carried out under vacuum conditions. The present invention limits the parameters of the ball milling to ensure that mechanical alloying occurs sufficiently between the ferromagnetic matrix and the single crystal silicon, thereby strengthening the degree of interface bonding between the two.
[0041] After the precursor is obtained, the precursor obtained in the present invention is subjected to nitridation heat treatment to obtain a core-shell structured magnetic abrasive.
[0042] In the present invention, the mechanized alloy between the ferromagnetic matrix and the single crystal silicon in the nitriding heat treatment is transformed into a Fe3Si silicon-iron intermetallic compound at the temperature of the nitriding heat, and at the same time, a silicon nitride hard phase is generated in situ on the surface of the single crystal silicon under the catalysis of yttrium trioxide. In the present invention, the temperature of the nitriding heat treatment is preferably 1000-1300°C, and more preferably 1200°C. In the present invention, the heating rate of the nitriding heat treatment is preferably 5-8 / min when the temperature is less than 800°C; and preferably 3-5 / min when the temperature is greater than 800°C. In the present invention, the time of the nitriding heat treatment is preferably 2-4h, and more preferably 3h. In the present invention, the nitriding heat treatment is preferably carried out under nitrogen conditions. The present invention limits the parameters of the nitriding heat treatment to ensure that the mechanized alloy between the ferromagnetic matrix and the single crystal silicon is more fully transformed into a Fe3Si iron-silicon intermetallic compound, further improves the degree of bonding between the ferromagnetic matrix and the hard phase; and ensures that the reaction of the in-situ generation of the silicon nitride hard phase on the surface of the single crystal silicon is more sufficient.
[0043] The present invention mixes single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then performs ball milling. The ball milling causes mechanical alloying between the magnetic iron-based powder and the single crystal silicon, thereby strengthening the interface bonding between the two and also making the single crystal silicon evenly distributed on the surface of the magnetic iron-based powder to form a precursor. The obtained precursor is then subjected to nitridation heat treatment to in-situ form a silicon nitride hard phase on the surface of the single crystal silicon. At the same time, under high temperature conditions, the single crystal silicon is embedded in the surface of the magnetic iron-based powder, thereby further converting the mechanical alloying between the magnetic iron-based powder and the single crystal silicon into a silicon-iron intermetallic compound, thereby further strengthening the interface bonding between the two and thus obtaining a core-shell structured magnetic abrasive.
[0044] The present invention also provides a core-shell structure magnetic abrasive prepared by the above preparation method, comprising a ferromagnetic matrix and an iron-silicon intermetallic compound and a silicon nitride hard phase sequentially coated on the surface of the ferromagnetic matrix from the inside to the outside.
[0045] During grinding processing of the core-shell structure magnetic abrasive provided by the present invention, after the outermost silicon nitride hard phase of the core-shell structure magnetic abrasive is ground off from the outermost oxide layer of the workpiece, the silicon-iron intermetallic compound with relatively low hardness continues to grind the softer metal surface below the oxide layer of the workpiece, thereby making the workpiece have a lower surface roughness; and the silicon-iron intermetallic compound in the core-shell structure magnetic abrasive can improve the bonding degree between the ferromagnetic matrix and the hard phase.
[0046] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] Example 1
[0048] A method for preparing a core-shell structure magnetic abrasive comprises the following steps:
[0049] (1) Putting single crystal silicon particles with a particle size of 4 μm, spherical iron powder with a particle size of 120 μm and yttrium trioxide with a particle size of 1 μm into a blender, stirring and mixing at 100 rpm for 30 min, and then ball milling to obtain a precursor; the mass ratio of the single crystal silicon particles to the spherical iron powder is 1:4; the mass of the yttrium trioxide is 8% of the total mass of the single crystal silicon particles, the spherical iron powder and the yttrium trioxide; the rotation speed of the ball mill is 150 rpm; the ball milling time is 8 h; the grinding balls are steel balls; the ball-to-material ratio is 1:10; the packing coefficient is 0.4; the particle size ratio of the spherical iron powder to the single crystal silicon particles in the precursor is 30:1;
[0050] (2) placing the precursor obtained in step (1) into a vacuum tube furnace, and subjecting it to a nitriding heat treatment at 1100° C. for 8 h under nitrogen conditions to obtain a core-shell structured magnetic abrasive; the heating rate of the nitriding heat treatment is 5 / min when the temperature is less than 800° C.; and 3 / min when the temperature is greater than 800° C.
[0051] Example 2
[0052] A method for preparing a core-shell structure magnetic abrasive comprises the following steps:
[0053] (1) Putting single crystal silicon particles with a particle size of 5 μm, spherical iron powder with a particle size of 150 μm and yttrium trioxide with a particle size of 1.2 μm into a blender, stirring and mixing at 100 rpm for 30 min, and then ball milling to obtain a precursor; the mass ratio of the single crystal silicon particles to the spherical iron powder is 1:6; the mass of the yttrium trioxide is 8% of the total mass of the single crystal silicon particles, the spherical iron powder and the yttrium trioxide; the rotation speed of the ball mill is 250 rpm; the ball milling time is 10 h; the grinding balls are steel balls; the ball-to-material ratio is 1:10; the packing coefficient is 0.4; the particle size ratio of the spherical iron powder to the single crystal silicon particles in the precursor is 30:1;
[0054] (2) placing the precursor obtained in step (1) into a vacuum tube furnace, and subjecting it to a nitriding heat treatment at 1100° C. for 5 h under nitrogen conditions to obtain a core-shell structured magnetic abrasive; the heating rate of the nitriding heat treatment is 5 / min when the temperature is less than 800° C.; and 3 / min when the temperature is greater than 800° C.
[0055] Example 3
[0056] A method for preparing a core-shell structure magnetic abrasive comprises the following steps:
[0057] (1) Putting single crystal silicon particles with a particle size of 5.7 μm, spherical iron powder with a particle size of 170 μm and yttrium trioxide with a particle size of 1.3 μm into a blender, stirring and mixing at 100 rpm for 30 min, and then ball milling to obtain a precursor; the mass ratio of the single crystal silicon particles to the spherical iron powder is 1:6; the mass of the yttrium trioxide is 8% of the total mass of the single crystal silicon particles, the spherical iron powder and the yttrium trioxide; the rotation speed of the ball mill is 250 rpm; the ball milling time is 10 h; the grinding balls are steel balls; the ball-to-material ratio is 1:10; the packing coefficient is 0.4; the particle size ratio of the spherical iron powder to the single crystal silicon particles in the precursor is 30:1;
[0058] (2) placing the precursor obtained in step (1) into a vacuum tube furnace, and subjecting it to a nitriding heat treatment at 1100° C. for 5 h under nitrogen conditions to obtain a core-shell structured magnetic abrasive; the heating rate of the nitriding heat treatment is 5 / min when the temperature is less than 800° C.; and 3 / min when the temperature is greater than 800° C.
[0059] Example 4
[0060] A method for preparing a core-shell structure magnetic abrasive comprises the following steps:
[0061] (1) Putting single crystal silicon particles with a particle size of 3.0 μm, spherical iron powder with a particle size of 90 μm and yttrium trioxide with a particle size of 1.0 μm into a blender, stirring and mixing at 100 rpm for 30 min, and then ball milling to obtain a precursor; the mass ratio of the single crystal silicon particles to the spherical iron powder is 1:6; the mass of the yttrium trioxide is 8% of the total mass of the single crystal silicon particles, the spherical iron powder and the yttrium trioxide; the rotation speed of the ball mill is 250 rpm; the ball milling time is 10 h; the grinding balls are steel balls; the ball-to-material ratio is 1:10; the packing coefficient is 0.4; the particle size ratio of the spherical iron powder to the single crystal silicon particles in the precursor is 30:1;
[0062] (2) placing the precursor obtained in step (1) into a vacuum tube furnace, and subjecting it to a nitriding heat treatment at 1100° C. for 5 h under nitrogen conditions to obtain a core-shell structured magnetic abrasive; the heating rate of the nitriding heat treatment is 5 / min when the temperature is less than 800° C.; and 3 / min when the temperature is greater than 800° C.
[0063] Comparative Example 1
[0064] A method for preparing a magnetic abrasive, comprising the following steps:
[0065] (1) Putting iron powder with a particle size of 150 μm and silicon carbide with a particle size of 38 μm into a mixer, stirring and mixing at 100 rpm for 30 min, and then ball milling to obtain a precursor; the mass ratio of silicon carbide to iron powder is 1:4; the rotation speed of the ball mill is 250 rpm; the ball milling time is 8 hours; the grinding balls are steel balls; the ball-to-material ratio is 1:10; the packing coefficient is 0.4; the particle size ratio of iron powder to silicon carbide in the precursor is 4:1;
[0066] (2) The precursor obtained in step (1) is mixed with a binder at 120 rpm for 30 min, pressed into blocks, placed in a vacuum drying oven at 100° C. for 10 h, placed in a vacuum tube furnace, sintered at 1200° C. for 2-3 h, cooled in the furnace, and then mechanically crushed to obtain a magnetic abrasive.
[0067] The structures of the core-shell magnetic abrasives prepared in Examples 1 to 4 were characterized by X-ray diffraction (XRD, PANAnalytical X'Pert PRO). Figure 1 As shown in the figure, it can be seen that diffraction peaks corresponding to the Fe3Si phase and the Si3N4 phase appear in the XRD spectrum of the magnetic abrasive. The morphology of the core-shell structure magnetic abrasives prepared in Examples 1 to 4 was characterized by SEM electron microscopy. The results are shown in FIG. Figures 2 to 5 As shown in the figure, it can be seen that the silicon nitride hard phase of the core-shell structure magnetic abrasive prepared in Examples 1 to 4 is well and evenly distributed on the surface of the spherical iron powder.
[0068] The cross-sectional morphology of the core-shell structure magnetic abrasive prepared in Example 1 was characterized by scanning electron microscope (SEM) images and EDS spectrum analysis. Figure 6 As shown in the figure, it can be seen that the core-shell structured magnetic abrasive prepared by this method presents a good core-shell structure distribution, the outer layer is mainly composed of the hard phase Si3N4, and the interface connection with the spherical iron powder is the intermetallic compound of Fe3Si.
[0069] The morphology of the magnetic abrasive prepared in Comparative Example 1 was characterized by SEM electron microscopy. Figure 7 As shown in the figure, it can be seen that the hard phase of the magnetic abrasive prepared in Comparative Example 1 is unevenly distributed on the surface of the spherical iron powder.
[0070] The core-shell structure magnetic abrasive prepared in Example 1 and the magnetic abrasive prepared in Comparative Example 1 were used to grind the zirconium alloy tube wall, respectively. The surface roughness of the original zirconium alloy tube wall, the zirconium alloy tube wall after grinding by the core-shell structure magnetic abrasive prepared in Example 1, and the zirconium alloy tube wall after grinding by the magnetic abrasive prepared in Comparative Example 1 were tested using a TR200 roughness measuring instrument. Figures 8 to 10 As shown in the figure, it can be seen that the surface roughness of the original zirconium alloy tube wall is Ra=0.508±0.01μm; the surface roughness of the zirconium alloy tube wall after grinding the zirconium alloy tube wall with the magnetic abrasive prepared in Example 1 is Ra=0.090±0.01μm; the surface roughness of the zirconium alloy tube wall after grinding the zirconium alloy tube wall with the magnetic abrasive prepared in Comparative Example 1 is Ra=0.236±0.01μm.
[0071] In summary, it can be seen that the core-shell structure magnetic abrasive provided by the present invention can make the workpiece have a lower surface roughness when used for grinding processing.
[0072] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a core-shell structure magnetic abrasive, comprising the following steps: (1) mixing single crystal silicon particles, magnetic iron-based powder and yttrium trioxide and then ball milling to obtain a precursor; (2) The precursor obtained in step (1) is subjected to nitridation heat treatment to obtain a core-shell structured magnetic abrasive.
2. The preparation method according to claim 1, characterized in that: In the step (1), the mass ratio of the single crystal silicon particles to the magnetic iron-based powder is 1:(4-6).
3. The preparation method according to claim 1 or 2, characterized in that: The magnetic iron-based powder in step (1) includes one of iron powder, carbonyl iron powder, iron-silicon alloy powder, iron-aluminum alloy powder and iron-nickel alloy powder.
4. The preparation method according to claim 2 or 3, characterized in that: In the step (1), the particle size ratio of the magnetic iron-based powder to the single crystal silicon particles in the precursor is (20-50):
1.
5. The preparation method according to claim 1, characterized in that: In the step (1), the rotation speed of the ball mill is 150 to 300 rpm, and the ball milling time is 8 to 10 hours.
6. The preparation method according to claim 1, characterized in that: The temperature of the nitriding heat treatment in the step (2) is 1000-1300° C., and the time of the nitriding heat treatment is 2-4 hours.
7. The core-shell structure magnetic abrasive prepared by the preparation method according to any one of claims 1 to 6 comprises a ferromagnetic matrix and an iron-silicon intermetallic compound and a silicon nitride hard phase sequentially coated on the surface of the ferromagnetic matrix from the inside to the outside.
Citation Information
Patent Citations
Rare earth-iron-nitrogen system magnetic powder and method for producing same
CN109982791A
Preparation method of high-temperature heat treatment iron-silicon material
CN110931235A
Spherical magnetic abrasive and preparation method thereof
CN112280535A
Insulating material coated soft magnetic powder, powder magnetic core, magnetic element, electronic device
CN113363043A
Production method of soft magnetic metal powder
US10607757B1
Cited By
Integrated preparation device of ball-milling magnetic material
CN120155269A